Industrial fan or blower comprising a flame retardant polyamide composition
By adding red phosphorus and magnesium hydroxide to the polyamide composition and combining other components, the problem that the polyamide composition in the prior art cannot meet the requirements of high refractory and mechanical properties is solved, and the polyamide composition is realized in industrial fans or efficient application in blowers.
Patent Information
- Application Number
- CN202080086909.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-22
- Filing Date
- 2020-12-07
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-12-07
AI Technical Summary
Existing polyamide-based flame retardant polymer compositions cannot meet the highest fire resistance requirements (5VA grade of UL94 standard) and have shortcomings in processing and mechanical properties (such as tensile strength, bending strength) and are difficult to use. High temperature applications such as industrial fans or blowers.
By adding 1.0 to 10.0 wt.% red phosphorus and 1.0 to 10.0 wt.% magnesium hydroxide to the polyamide composition, the weight ratio is controlled between 1:5 to 5:1 and combined with 20 wt.% to 20 wt.% to magnesium hydroxide 60 wt.% polyamide, 20 wt.% to 50 wt.% enhancer, 0.1 wt.% to 10.0 wt.% impact modifier, 0.01 wt.% to 5.0 wt.% stabilizer and 0.1 wt. % to 5.0 wt.% dispersant ensures that the composition has a viscosity of at least 114 ml/g, meeting the 5VA grade of UL94 standard.
The polyamide composition is achieved while maintaining good processability and mechanical properties while maintaining its highest refractory quality, making it suitable for the manufacture of formed products such as industrial fans or blowers.
Smart Images

Figure GDA0003851809560000051 
Figure GDA0003851809560000061 
Figure GDA0003851809560000181
Abstract
Description
Technical Field
[0001] The invention relates to a flame retardant polyamide composition, a preparation method thereof and use thereof in an industrial fan or blower. Background Art
[0002] The production of flame retardant polymer compositions for various applications is well known in the art. Requirements for various flame retardant properties of polymer compositions vary according to the intended end use of the polymer composition. For example, requirements related to heat release, smoke generation, vertical flame propagation, smoke density, smoke acidity and melt viscosity can vary according to the intended end use of the polymer composition. Requirements for other properties (e.g. mechanical properties, such as rigidity and tensile strength) can also vary according to the intended end use of the polymer composition. These properties may be affected by additives, which are included in the polymer composition to obtain the desired flame retardant properties.
[0003] Polymer compositions, such as polyamide-based compositions blended with suitable flame retardants, are known in the art. These compositions typically use polyamide 6 and / or polyamide 66 and have been used for molding applications. In addition, these compositions are known to have acceptable flame retardant properties that meet the fire resistance requirements according to the UL94 standard. In particular, existing compositions are known to meet the V-2 flame retardant requirements according to the UL94 standard.
[0004] WO 2018 / 187638 A1 discloses a flame retardant polymer composition comprising a polymer, a flame retardant, a high aspect ratio particulate material and an optional reinforcing material. When measured using the UL94 standard, the composition is disclosed as having a flame retardant rating equal to or greater than V-2.
[0005] US 6,146,557 B1 relates to a flame retardant composition having a fire resistance of up to V-0 or higher in a vertical flammability test according to UL94 standard. The composition comprises 100 parts by weight of a thermoplastic resin, 10 to 300 parts by weight of at least one flame retardant selected from the group consisting of a nitrogen-based flame retardant containing no halogen atoms, a phosphorus-based flame retardant containing no halogen atoms, and a nitrogen-phosphorus-based flame retardant containing no halogen atoms, and 1 to 100 parts by weight of a layered silicate hydrate.
[0006] EP 0,278,555 A1 discloses a polyamide composition comprising a thermoplastic polyamide accounting for at least 40% by weight of the composition, a flame retardant mainly composed of red phosphorus (the red phosphorus accounts for 4-15% by weight of the composition), 5-40% by weight of magnesium hydroxide accounting for 5-50% by weight of the composition, and a mineral reinforcing fiber accounting for 5-50% by weight of the composition, wherein the total amount of the flame retardant and the magnesium hydroxide does not exceed 50% by weight of the composition. According to the UL94 standard, the composition is disclosed to have a flame retardancy of V-0.
[0007] Existing polymer compositions, particularly compositions based on polyamides, have some limitations. One such limitation is that the flame retardancy of these compositions is not of the highest quality, i.e., these compositions meet the V-0, V-1 or V-2 requirements according to the UL94 standard. In addition, these compositions do not provide acceptable properties, such as, but not limited to, tensile strength, elongation, flexural strength and Charpy notch strength. In addition, the presence of other ingredients (such as, but not limited to, flame retardants, such as nitrogen-based flame retardants, and filling materials, such as talcum) makes it difficult to process. In addition, existing polyamide compositions are not yet disclosed for industrial fans or blowers.
[0008] It is therefore an object of the present invention to provide a flame retardant polyamide composition which can meet the highest fire resistance qualities, i.e. 5VA according to the UL94 standard, can be easily processed and still exhibits acceptable properties of tensile strength, elongation %, flexural strength and Charpy notched strength, making it useful for the manufacture of shaped articles, such as industrial fans or blowers. Summary of the invention
[0009] Surprisingly, it has been found that the above objects are met by providing a flame retardant polyamide composition, in particular comprising a flame retardant mixture having (i) 1.0 to 10.0 wt.% red phosphorus and (ii) 1.0 to 10.0 wt.% magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1, and wherein the flame retardant composition has a viscosity number determined according to ISO 307 of at least 114 ml / g.
[0010] Thus, in one aspect, the presently claimed invention is directed to a flame retardant polyamide composition comprising:
[0011] (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g,
[0012] (b) 20 wt.% to 50 wt.% of a reinforcing agent,
[0013] (c) a flame retardant mixture comprising (i) 1.0 to 10.0 wt.% of red phosphorus and (ii) 1.0 to 10.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1,
[0014] (d) 0.1 wt.% to 10.0 wt.% of an impact modifier,
[0015] (e) 0.01 to 5.0 wt.% of a stabilizer, and
[0016] (f) 0.1 to 5.0 wt.% of a dispersant,
[0017] The flame retardant polyamide composition has a viscosity number determined according to ISO 307 of at least 114 ml / g.
[0018] In another aspect, the present invention relates to a method for preparing the above flame retardant polyamide composition.
[0019] In yet another aspect, the presently claimed invention is directed to a shaped article comprising the flame retardant polyamide composition described above.
[0020] In yet another aspect, the present invention relates to an industrial fan or blower comprising the flame retardant polyamide composition described above. DETAILED DESCRIPTION
[0021] Before describing the present compositions and formulations of the present invention, it should be understood that the present invention is not limited to the specific compositions and formulations described, as such compositions and formulations may of course vary. It should also be understood that the terminology used herein is not intended to be limiting, as the scope of the present invention will be limited only by the appended claims.
[0022] As used herein, the terms "comprising, comprises, and "comprised of" are synonymous with "including, includes, or "containing, contains," and are inclusive or open-ended and do not exclude additional, unrecited members, elements, or method steps. It should be understood that, as used herein, the terms "comprising / comprises / comprised of" encompass the terms "consisting of, consists, and consists of."
[0023] In addition, the terms "first", "second", "third" or "(a)", "(b)", "(c)", "(d)", etc. in the specification and claims are used to distinguish similar elements, and are not necessarily used to describe a sequential or chronological order. It should be understood that the terms used in this way are interchangeable where appropriate, and that the embodiments of the invention described herein are capable of operating in other sequences than those described or illustrated herein. In the case where the terms "first", "second", "third" or "(A)", "(B)" and "(C)" or "(a)", "(b)", "(c)", "(d)", "i", "ii", etc. refer to steps of a method or use or determination, there is no continuity of time or time intervals between the steps, that is, the steps can be performed simultaneously, or there can be time intervals of seconds, minutes, hours, days, weeks, months or even years between such steps, unless otherwise indicated in the application set forth above or below.
[0024] In the following paragraphs, different aspects of the present invention are defined in more detail. Unless clearly indicated to the contrary, each aspect so defined can be combined with any one or more other aspects. Especially, any feature indicated as preferred or advantageous can be combined with any one or more other features indicated as preferred or advantageous.
[0025] References to "one embodiment" or "an embodiment" throughout this specification mean that a particular feature, structure, or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present invention. Therefore, the phrases "in one embodiment" or "in an embodiment" that appear in various places throughout this specification do not necessarily all refer to the same embodiment, but may refer to the same embodiment. In addition, in one or more embodiments, features, structures, or characteristics may be combined in any suitable manner, as will be apparent to those skilled in the art based on this disclosure. In addition, although some embodiments described herein include some features included in other embodiments but not others, as will be appreciated by those skilled in the art, the combination of features of different embodiments is intended to be within the scope of the present invention and to form different embodiments. For example, in the appended claims, any claimed embodiment may be used in any combination.
[0026] Furthermore, ranges defined throughout the specification also include the endpoints, ie, a range of 1 to 10 means that the range includes both 1 and 10. For the avoidance of doubt, the applicant is entitled to equivalents under applicable law.
[0027] Flame retardant polyamide composition
[0028] One aspect of the present invention is embodiment 1, which relates to a polyamide composition comprising:
[0029] (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g,
[0030] (b) 20 wt.% to 50 wt.% of a reinforcing agent,
[0031] (c) a flame retardant mixture comprising (i) 1.0 to 10.0 wt.% of red phosphorus and (ii) 1.0 to 10.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1,
[0032] (d) 0.1 wt.% to 10.0 wt.% of an impact modifier,
[0033] (e) 0.01 to 5.0 wt.% of a stabilizer, and
[0034] (f) 0.1 to 5.0 wt.% of a dispersant,
[0035] The flame retardant polyamide composition has a viscosity number determined according to ISO 307 of at least 114 ml / g.
[0036] In the context of the present invention, the phrases "composition" and "polyamide composition" are used interchangeably to refer to the flame retardant polyamide composition of Example 1.
[0037] In the context of the present invention, the phrase "ingredients" refers to (a), (b), (c), (d), (e) and (f) in the polyamide composition of Example 1 as described herein.
[0038] In the context of the present invention, the viscosity number is determined according to ISO 307 at 25° C. from a 0.5 wt. % solution of the polyamide composition in 96 wt. % sulfuric acid.
[0039] In one embodiment, the viscosity of the polyamide composition needs to be equal to or greater than 114 ml / g. This is because a viscosity less than 114 ml / g tends to drip during the flame retardancy test despite the addition of a flame retardant. This makes the composition unacceptable because dripping can cause flame extinguishment in the 5VA test.
[0040] In another embodiment, the flame retardant polyamide composition in Example 1 does not contain any talc or phyllosilicate, such as phyllosilicate hydrate.
[0041] Polyamide
[0042] Suitable polyamides in Example 1 have a viscosity number between 90 ml / g and 350 ml / g determined according to ISO 307. As described herein, the polyamide is selected such that the flame retardant polyamide composition has a viscosity number of at least 114 ml / g.
[0043] In one embodiment, the viscosity of the polyamide in Example 1 is between 90 ml / g and 340 ml / g, or between 100 ml / g and 340 ml / g, or between 100 ml / g and 330 ml / g, or between 100 ml / g and 320 ml / g, or between 100 ml / g and 310 ml / g, or between 100 ml / g and 300 ml / g. In other embodiments, the viscosity number is between 110 ml / g and 300 ml / g, or between 110 ml / g and 290 ml / g, or between 110 ml / g and 280 ml / g, or between 110 ml / g and 280 ml / g, or between 110 ml / g and 270 ml / g, or between 120 ml / g and 270 ml / g, or between 120 ml / g and 260 ml / g, or between 120 ml / g and 250 ml / g, or between 120 ml / g and 240 ml / g, or between 120 ml / g and 230 ml / g, or between 120 ml / g and 220 ml / g. In yet another embodiment, the viscosity number is between 130ml / g and 220ml / g, or between 130ml / g and 210ml / g, or between 140ml / g and 210ml / g, or between 150ml / g and 210ml / g, or between 150ml / g and 210ml / g, or between 160ml / g and 210ml / g. In another embodiment, the viscosity number is between 170ml / g and 210ml / g, or between 180ml / g and 210ml / g.
[0044] In one embodiment, the polyamide of Embodiment 1 can be selected from aromatic and aliphatic polyamides. In another embodiment, the polyamide of Embodiment 1 comprises an aliphatic polyamide.
[0045] In another embodiment, the polyamide in Example 1 is derived from a lactam having 7 to 13 ring members or obtained by the reaction of a dicarboxylic acid with a diamine. Examples of polyamides derived from lactams include polycaprolactam, polycaprolactam and / or polylaurolactam.
[0046] In yet another embodiment, the polyamides in Example 1 also include those obtainable from ω-aminoalkylnitriles, such as, but not limited to, aminocapronitrile to produce nylon-6. Additionally, dinitriles can be reacted with diamines. For example, adiponitrile can be reacted with hexamethyleneethylenediamine to obtain nylon-6,6. The polymerization of nitrile is achieved in the presence of water and is also referred to as direct polymerization.
[0047] When using polyamides obtainable from dicarboxylic acids and diamines, dicarboxylic alkanes (aliphatic dicarboxylic acids) having 6 to 36 carbon atoms, or 6 to 12 carbon atoms, or 6 to 10 carbon atoms may be employed. Aromatic dicarboxylic acids are also suitable. Examples of dicarboxylic acids include adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, and also terephthalic acid and / or isophthalic acid.
[0048] For example, suitable diamines include alkane diamines having 5 to 36 carbon atoms, or 6 to 12 carbon atoms, or 6 to 8 carbon atoms; and aromatic diamines such as m-xylylenediamine, bis(4-aminophenyl)methane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminocyclohexyl)propane, and 1,5-diamino-2-methylpentane.
[0049] In other embodiments, the polyamide in Embodiment 1 may also include polyhexamethylene diamide, polyhexamethylene sebacamide and polycaprolactam, and may also include nylon-6 / 6,6 in which the proportion of caprolactam units is between 5 wt.% and 95 wt.%.
[0050] The following non-exhaustive list includes the polyamides described above in Example 1.
[0051] AB polymer:
[0052]
[0053]
[0054] AA / BB polymer:
[0055] PA 4.6 Tetramethylethylenediamine, adipic acid PA 66 Hexamethylenediamine, adipic acid PA 6.9 Hexamethylenediamine, Azelaic acid PA 6.10 Hexamethylenediamine, Sebacic acid PA 6.12 Hexamethylenediamine, decanedicarboxylic acid PA 6.13 Hexamethylenediamine, undecanedicarboxylic acid PA 12.12 Dodecane-1,12-diamine, decanedicarboxylic acid PA 13.13 Tridecane-1,13-diamine, undecanedicarboxylic acid PA 6T Hexamethylenediamine, terephthalic acid PA 9T Nonanediamine, terephthalic acid PA MXD6 Meta-phenylenediamine, adipic acid PA 6I Hexamethylenediamine, Isophthalic acid PA 6-3-T Trimethylhexamethylenediamine, terephthalic acid PA 6.6T (See PA 6 and PA 6T) PA 6.66 (See PA 6 and PA 66) PA 6.12 (See PA 6 and PA 12) PA 66.6.610 (See PA 66, PA 6 and PA 6.10) PA 6I.6T (See PA 6I and PA 6T) PA PACM 12 Diaminocyclohexylmethane, laurolactam PA 6I.6T.PACM As PA 6I.6T and diaminodicyclohexylmethane PA 12.MACMI Laurolactam, dimethyldiaminodicyclohexylmethane, isophthalic acid PA 12.MACMT Lauryl lactam, dimethyl diamino dicyclohexyl methane, terephthalic acid PA PDA-T Phenylenediamine, terephthalic acid
[0056] In one embodiment, the polyamide in Example 1 is selected from PA 6, PA 11, PA 12, PA 66, PA 6.9, PA 6.10 and PA 6.12. In another embodiment, the polyamide is selected from PA 6, PA 11, PA 12, PA 66 and PA 6.9. In yet another embodiment, the polyamide is selected from PA 6, PA 12 and PA 66.
[0057] In another embodiment, the polyamide in Embodiment 1 is selected from PA 6, PA 66, or blends or copolymers thereof. In yet another embodiment, the polyamide in Embodiment 1 includes PA 6.
[0058] An appropriate amount of polyamide can be added to the composition to achieve a viscosity number as described herein. In one embodiment, the polyamide in Example 1 is present in an amount of 20 wt.% to 60 wt.% based on the total weight of the composition. In another embodiment, the polyamide is present in an amount of 20 wt.% to 60 wt.%, or 20 wt.% to 55 wt.%, or 25 wt.% to 55 wt.%. In yet another embodiment, the polyamide is present in an amount of 25 wt.% to 50 wt.%, or 30 wt.% to 50 wt.%, or 30 wt.% to 45 wt.%. In yet another embodiment, the polyamide is present in an amount between 30 wt.% and 40 wt.%.
[0059] Enhancer
[0060] The polyamide composition of Example 1 also includes a suitable amount of reinforcing agent. As known in the art, suitable reinforcing agents can be used to control the properties of the polyamide composition.
[0061] In one embodiment, the reinforcing agent in Example 1 is selected from metal fiber, metallized inorganic fiber, metallized synthetic fiber, glass fiber, carbon fiber, ceramic fiber, mineral fiber, basalt fiber, kenaf fiber, jute fiber, flax fiber, hemp fiber, cellulose fiber, sisal fiber and coconut fiber. In another embodiment, the reinforcing agent is selected from metallized synthetic fiber, glass fiber, carbon fiber, ceramic fiber, mineral fiber, basalt fiber, kenaf fiber and jute fiber. In yet another embodiment, the reinforcing agent is selected from glass fiber, carbon fiber, ceramic fiber and mineral fiber. In another embodiment, the reinforcing agent in Example 1 is glass fiber.
[0062] For the purposes of the present invention, the reinforcing agent can be obtained in any shape and size. Further, the reinforcing agent can be subjected to a suitable surface treatment agent or sizing agent. For example, the reinforcing agent can be surface treated with a coupling agent, such as but not limited to a silane coupling agent, a titanium coupling agent, an aluminate coupling agent, a carbamate coupling agent, and an epoxy coupling agent. For this purpose, any suitable surface treatment technique can be used. For example, any suitable coating method can be used, such as but not limited to dip coating and spray coating.
[0063] In one embodiment, the carbamate coupling agent includes at least one carbamate group. Suitable carbamate coupling agents for use with reinforcing agents are known to those skilled in the art, such as, for example, described in U.S. Publication No. 2018 / 0282496. In one embodiment, the carbamate coupling agent includes, for example, a reaction product of an isocyanate, such as, but not limited to, m-phenylenediisocyanate (XDI), 4,4'-methylenebis(cyclohexyl isocyanate) (HMDI) or isophorone diisocyanate (IPDI) and a polyester-based polyol or a polyether-based polyol.
[0064] In another embodiment, the epoxy coupling agent includes at least one epoxy group. Suitable epoxy coupling agents used with reinforcing agents are known to those skilled in the art, such as described in U.S. Publication No. 2015 / 0247025, which is incorporated herein by reference. In one embodiment, the epoxy coupling agent is selected from aliphatic epoxy coupling agents, aromatic epoxy coupling agents, or mixtures thereof. Non-limiting examples of aliphatic coupling agents include polyether polyepoxides having two or more epoxy groups in the molecule and / or polyol polyepoxides having two or more epoxy groups in the molecule. As aromatic coupling agents, bisphenol A epoxy or bisphenol F epoxy can be used.
[0065] As described herein, suitable amounts of these coupling agents are well known to those skilled in the art. However, in one embodiment, the coupling agent may be present in an amount of 0.1 to 10.0 parts by mass relative to 100 parts by mass of the reinforcing agent.
[0066] In one embodiment, the reinforcing agent in Example 1 is present in an amount between 20 wt.% and 50 wt.% based on the total weight of the composition. In another embodiment, the reinforcing agent is present in an amount between 25 wt.% and 50 wt.% or between 25 wt.% and 45 wt.%. In yet another embodiment, the reinforcing agent is present in an amount between 30 wt.% and 45 wt.% or between 35 wt.% and 45 wt.%.
[0067] Flame retardant mixture
[0068] The polyamide composition of Example 1 includes a flame retardant mixture, which comprises (i) 1.0 wt.% to 10.0 wt.% of red phosphorus and (ii) 1.0 wt.% to 10.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1,
[0069] In one embodiment, the red phosphorus in Example 1 is present between 1.0wt.% and 9.5wt.%, or between 1.5wt.% and 9.5wt.%, or between 1.5wt.% and 9.0wt.%. In another embodiment, the magnesium hydroxide is present between 2.0wt.% and 9.0wt.%, or between 2.0wt.% and 8.5wt.%, or between 2.5wt.% and 8.5wt.%. In yet another embodiment, the magnesium hydroxide is present between 2.5wt.% and 8.0wt.%, or between 3.0wt.% and 8.0wt.%, or between 3.0wt.% and 7.5wt.%. In yet another embodiment, the magnesium hydroxide is present between 3.5wt.% and 7.5wt.%, or between 3.5wt.% and 7.0wt.%, or between 4.0wt.% and 7.0wt.%.
[0070] In the context of the present invention, the magnesium hydroxide in Example 1 is used as a flame retardant synergist, and can be surface treated with a conventionally known surface treatment agent as required. The amount of the surface treatment agent per 100 parts by weight of magnesium hydroxide is between 0.1 and 10 parts by weight. The surface treatment agent may include higher fatty acids such as oleic acid and stearic acid; alkali metal salts of these higher fatty acids; silane coupling agents such as vinylethoxysilane, vinyl-tri(2-methoxy)silane, γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane and γ-mercaptopropyltrimethoxysilane; titanic acid-containing coupling agents such as isopropyl triisostearoyl titanate, triisopropyl tri(dioctyl pyrophosphate) titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate and isopropyl tridecylbenzenesulfonyl titanate; aluminum-containing coupling agents such as acetoalkoxyaluminum diisopropoxide; and partial esterification products of orthophosphoric acid, such as monoester or diester of orthophosphoric acid and stearyl alcohol; and partial esterification products of orthophosphoric acid or alkali metal salts.
[0071] In one embodiment, the magnesium hydroxide in Example 1 can be a powdered solid material, which can be coated or uncoated, as described above. Magnesium hydroxide is used in a synergistic amount so that the weight ratio of red phosphorus (i) and magnesium hydroxide (ii) in the flame retardant mixture is between 1:5 and 5:1. In another embodiment, the ratio is between 1:4 and 5:1, or between 1:4 and 4:1, or between 1:3 and 4:1. In yet another embodiment, the weight ratio is between 1:3 and 3:1, or between 1:2 and 3:1, or between 1:2 and 2:1.
[0072] In one embodiment, the magnesium hydroxide in Example 1 is present in an amount between 1.0wt.% and 9.5wt.%, or between 1.5wt.% and 9.5wt.%, or between 1.5wt.% and 9.0wt.%. In another embodiment, the red phosphorus is between 2.0wt.% and 9.0wt.%, or between 2.0wt.% and 8.5wt.%, or between 2.5wt.% and 8.5wt.%. In yet another embodiment, the red phosphorus is between 2.5wt.% and 8.0wt.%, or between 3.0wt.% and 8.0wt.%, or between 3.0wt.% and 7.5wt.%. In yet another embodiment, the red phosphorus is between 3.5wt.% and 7.5wt.%, or between 3.5wt.% and 7.0wt.%, or between 4.0wt.% and 7.0wt.%.
[0073] In one embodiment, the composition of Example 1 does not include other flame retardants, particularly halogenated or non-halogenated nitrogen-based flame retardants.
[0074] Impact modifier
[0075] Impact modifiers are also commonly referred to as rubber or elastomeric polymers, and are used in the present invention, for example, as described in US 2014 / 03203631A1 and US 2008 / 0070023A1. Suitable impact modifiers are selected from (i) ethylene polymers and copolymers grafted with carboxylic acids, their anhydrides, maleimides or epoxides; and (ii) olefin or acrylic acid or anhydride terpolymers and ionomers.
[0076] In the ethylene polymers and copolymers grafted with carboxylic acids, their anhydrides, maleimides or epoxy compounds, the carboxylic acids or their anhydrides are selected from maleic acid, fumaric acid, itaconic acid, acrylic acid, crotonic acid, C1 to C4 alkyl half esters of maleic acid and their anhydrides or derivatives, including maleic anhydride. In addition, olefin rubbers can also be used as suitable impact modifiers.
[0077] In one embodiment, the impact modifier in Example 1 is an ethylene copolymer grafted with a carboxylic acid or any anhydride thereof, such as an ethylene copolymer grafted with maleic anhydride. In other embodiments, the impact modifier comprises ethylene propylene diene terpolymer (EPDM) grafted with maleic anhydride (maleic anhydride is between 2 wt.% and 6 wt.%); ethylene propylene grafted with maleic anhydride (maleic anhydride is between 0.5 wt.% and 6 wt.%); low density polyethylene grafted with maleic anhydride (maleic anhydride is between 0.2 wt.% and 6 wt.%); and ethylene butyl acrylate grafted with maleic anhydride (maleic anhydride is between 0.2 wt.% and 6 wt.%).
[0078] Olefin or acrylic acid or anhydride terpolymers and ionomer impact modifiers have polymeric chain units derived from monomers, the polymeric chain units including: (a) ethylene, butene, propylene and combinations thereof; (b) between 2 wt.% and 25 wt.% of an acid selected from acrylic acid, methacrylic acid and mixtures thereof; and (c) 0.1 wt.% to 15 wt.% of a dicarboxylic acid monomer selected from maleic acid, fumaric acid, itaconic acid, maleic anhydride, itaconic anhydride, C1 to C4 alkyl half esters of maleic acid and mixtures of these dicarboxylic acid monomers. In one embodiment, the terpolymer is an ethylene / methacrylic acid / maleic anhydride ionomer (between 0.5 wt.% and 12 wt.% of maleic anhydride). The ionomer can be formed by neutralizing the carboxylic acid units in the terpolymer with a metal ion selected from zinc, magnesium, manganese and mixtures thereof, alone or in combination with sodium or lithium ions. The terpolymer can further contain up to 40 wt.% of C1 to C8 alkyl acrylate monomer units.
[0079] In one embodiment, the impact modifier of Example 1 is present between 0.1 wt.% and 10.0 wt.% based on the total weight of the polyamide composition. In another embodiment, the impact modifier is present between 0.1 wt.% and 9.0 wt.%, or between 0.2 wt.% and 9.0 wt.%, or between 0.2 wt.% and 8.0 wt.%. In yet another embodiment, the impact modifier is present between 0.3 wt.% and 8.0 wt.%, or between 0.3 wt.% and 7.0 wt.%, or between 0.4 wt.% and 7.0 wt.%. In yet another embodiment, the impact modifier is present between 0.4 wt.% and 6.0 wt.%, or between 0.5 wt.% and 6.0 wt.%, or between 0.5 wt.% and 5.0 wt.%, or between 0.5 wt.% and 4.0 wt.%. In another embodiment, the impact modifier is present at between 0.5 wt.% and 3.0 wt.% or between 0.5 wt.% and 2.0 wt.%.
[0080] Stabilizer
[0081] In the context of the present invention, the stabilizer in Example 1 includes an antioxidant and a heat stabilizer.
[0082] Stabilizers include, but are not limited to, organic stabilizers such as phosphorus stabilizers, hindered phenol stabilizers, hindered amine stabilizers, oxalic acid anilide stabilizers, organic sulfur stabilizers, and secondary aromatic amine stabilizers; and inorganic stabilizers such as copper compounds and halides.
[0083] The phosphite compounds include, for example, distearyl pentaerythritol diphosphite, dinonylphenyl pentaerythritol diphosphite, di(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, di(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, di(2,6-di-tert-butyl-4-ethylphenyl)pentaerythritol diphosphite, di(2,6-di-tert-butyl-4-isopropylphenyl)pentaerythritol diphosphite, di(2,4,6-tri-tert-butylphenyl)pentaerythritol diphosphite, di(2,6-di-tert-butyl-4-sec-butylphenyl)pentaerythritol diphosphite, di(2,6-di-tert-butyl-4-tert-octylphenyl)pentaerythritol diphosphite and di(2,4)-dicumylphenyl)pentaerythritol diphosphite.
[0084] Hindered phenol stabilizers include, for example, n-octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl)-4-hydroxyphenyl) propionate], pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 3,9-bis[1,1-dimethyl-2-{β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, triethylene glycol bis[ 3-(3-tert-butyl-5-methyl)-4-hydroxyphenyl)propionate], diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl)-4-hydroxybenzyl)benzene, 2,2-thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate and N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid). The hindered amine stabilizer includes, for example, the well-known hindered amine compound having a 2,2,6,6-tetramethylpiperidine skeleton.Specific examples of the hindered amine compounds include 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-phenylacetoxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-methoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6,6-tetramethylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine. piperidine, 4-ethylcarbamoyloxy-2,2,6,6-tetramethylpiperidine, 4-cyclohexylcarbamoyloxy-2,2,6,6-tetramethylpiperidine, 4-phenylcarbamoyloxy-2,2,6,6-tetramethylpiperidine, bis(2,2,6,6-tetramethyl)-4-piperidinyl) carbonate, bis(2,2,6,6-tetramethyl-4-piperidinyl) oxalate, bis(2,2,6,6-tetramethyl-4-piperidinyl) malonate, bis(2,2,6),6-tetramethyl-4-piperidinyl) sebacate, bis(2,2,6,6-tetramethyl-4-piperidinyl) adipate, bis(2,2,6,6-tetramethyl-4-piperidinyl) 1,2-bis(2,2,6,6-tetramethyl-4-piperidinyloxy) terephthalate, 1,2-bis(2,2,6,6-tetramethyl-4-piperidinyloxy) ethane, α,α'-bis(2,2,6,6-t-tetramethyl-4-piperidinyloxy)-p-xylene, bis(2,2,6,6-tetramethyl-4-piperidinyltoluene)-2,4-dicarbamate, bis(2,2,6,6-tetramethyl-4-piperidinyl)hexamethylene-1,6-dicarbamate, tris(2,2,6,6-tetramethyl-4-piperidinyl)benzo-1,3,5-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidinylbenzene-1,3,4-tricarboxylate, 1-[2-{3-(3,5-di-tert-butyl 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol and β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro(5,5)undecane]diethanol, polycondensation products of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine, and 1,3-benzenedicarboxylic acid-N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl).
[0085] Amine antioxidants refer to amine compounds other than the above-mentioned hindered amine stabilizers, and include, for example, the reaction product of N-phenylaniline and 2,4,4-trimethylpentene, N,N'-diphenyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, polymerized 1,2-dihydro-2,2,4-trimethylquinoline and 6-ethoxy-1,2-dihydro-2,2,4-trimethylquinoline.
[0086] The oxalylanilide stabilizer includes 4,4'-dioctyloxyoxalylanilide, 2,2'-diethoxyoxalylanilide, 2,2'-dioctyloxy-5,5'-di-tert-butylanilide, 2,2'-docosyloxy-5,5'-di-tert-butyranilide, 2-ethoxy-2'-ethyloxalylanilide, N,N'-bis(3-dimethylaminopropyl)oxalylanilide, 2-ethoxy-5-tert-butyl-2'-acetanilide and a mixture thereof with 2-ethoxy-2'-ethyl-5,4'-di-tert-butyranilide, a mixture of o-methoxy-disubstituted oxalylanilide and p-methoxy-disubstituted oxalylanilide, and a mixture of o-ethoxy-disubstituted oxalylanilide and p-ethoxy-disubstituted oxalylanilide.
[0087] Organic sulfur stabilizers include, for example, organic thioester compounds such as didodecylthiodipropionate, dido-tetradecylthiodipropionate, dido-octadecylthiodipropionate, pentaerythritol tetrakis(3-thiododecylpropionate) and thiobis(N-phenyl-β-naphthylamine); mercaptobenzimidazole compounds such as 2-mercaptobenzothiazole, 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole and metal salts of 2-mercaptobenzimidazole; dithiocarbamate compounds such as metal salts of diethyldithiocarbamic acid and metal salts of dibutyldithiocarbamic acid; and thiourea compounds such as 1,3-bis(dimethylaminopropyl)-2-thiourea and tributylthiourea; and tetramethylthiuram monosulfide, tetramethylthiuram disulfide, nickel dibutyldithiocarbamate, nickel isopropylxanthate and trilauryl trithiophosphite.
[0088] The secondary aromatic amine stabilizer preferably includes a compound having a diphenylamine skeleton, a compound having a phenylnaphthylamine skeleton, and a compound having a dinaphthylamine skeleton. Specifically, compounds having a diphenylamine skeleton include p,p'-dialkyldiphenylamine (wherein the alkyl group contains 8 to 14 carbon atoms), octylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonamide)diphenylamine, N,N'-diphenyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine and N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine; compounds having a phenylnaphthylamine skeleton include N-phenyl-1-naphthylamine and N,N'-di-2-naphthyl-p-phenylenediamine; and compounds having a dinaphthylamine skeleton include 2,2'-dinaphthylamine, 1,2'-dinaphthylamine and 1,1'-dinaphthylamine.
[0089] Inorganic stabilizers include copper compounds and halides. Copper compounds are copper salts of various inorganic or organic acids, excluding the following halides. Copper can be cuprous or cupric, and specific examples of copper salts include copper chloride, copper bromide, copper iodide, copper phosphate, copper stearate, and natural minerals such as hydrotalcite, pyroxene, and zeolite.
[0090] In one embodiment, the stabilizer in Example 1 is present at 0.01 wt.% to 5.0 wt.% based on the total weight of the composition. In another embodiment, the stabilizer is present at 0.01 wt.% to 4.0 wt.%, or 0.01 wt.% to 3.0 wt.%, or 0.01 wt.% to 2.0 wt.%.
[0091] Dispersants
[0092] The polyamide composition of Example 1 further comprises a dispersant added for the purpose of preventing coagulation in the flame retardant mixture, if any. In one embodiment, the dispersant in Example 1 is selected from carboxamide-based waxes, higher fatty acid metal salts, and higher fatty acid ester compounds.
[0093] Carboxylic acid amide wax can be exemplified by compounds obtained by dehydration reaction between higher aliphatic monocarboxylic acid and / or polyacid and diamine. Higher aliphatic monocarboxylic acid is preferably a saturated aliphatic monocarboxylic acid and hydroxycarboxylic acid having 16 or more carbon atoms, and is exemplified by palmitic acid, stearic acid, behenic acid, montanic acid and 12-hydroxystearic acid. Polyacid is a dibasic or higher carboxylic acid, and can be exemplified by aliphatic dicarboxylic acids such as succinic acid, succinic acid, adipic acid, sebacic acid, pimelic acid and azelaic acid; aromatic dicarboxylic acids such as phthalic acid, terephthalic acid; and alicyclic dicarboxylic acids such as cyclohexyl dicarboxylic acid, cyclohexyl succinic acid. Diamine can be exemplified by ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, hexamethylenediamine, m-phenylenediamine, toluenediamine, p-phenylenediamine, phenylenediamine and isophoronediamine.
[0094] The carboxylic acid amide-based wax is preferably a compound obtained by a polycondensation reaction of stearic acid, sebacic acid and ethylenediamine, for example, a compound obtained by a polycondensation reaction between 2 mol of stearic acid, 1 mol of sebacic acid and 2 mol of ethylenediamine.
[0095] The metal salt of the higher fatty acid can be exemplified by the metal salt of the higher aliphatic monocarboxylic acid described above. For example, calcium stearate, barium stearate, magnesium stearate, aluminum stearate, zinc stearate and lignite calcium can be used in Example 1. The higher fatty acid ester compound can be exemplified by the ester compound formed between the higher aliphatic monocarboxylic acid and the alcohol described above, and more specifically, can be exemplified by stearyl stearate, glyceryl stearate, pentaerythritol stearate.
[0096] In one embodiment, the dispersant is present at between 0.1 wt.% and 5.0 wt.% by total weight of the composition. In another embodiment, the dispersant is present at between 0.1 wt.% and 4.5 wt.%, or between 0.1 wt.% and 4.0 wt.%, or between 0.1 wt.% and 3.5 wt.%. In yet another embodiment, the dispersant is present at between 0.1 wt.% and 3.0 wt.%, or between 0.1 wt.% and 2.5 wt.%, or between 0.1 wt.% and 2.0 wt.%.
[0097] additive
[0098] In one embodiment, the polyamide composition of embodiment 1 further comprises additives. Suitable additives include, for example, but not limited to, dyes, pigments, UV absorbers, antistatic agents, fungistatic agents, bacteriostatic agents, and IR absorbing materials.
[0099] Other additives may also be added to the polyamide composition. These additives include anti-drip agents; copper-, phosphorus- or sulfur-containing heat stabilizers; weathering agents; foaming agents; lubricants; plasticizers; flow modifiers; organic fillers; and nucleating agents.
[0100] Suitable amounts of these additives may be used in the present invention. In one embodiment, the polyamide composition of Example 1 is present in an amount between 0.1 wt.% and 10 wt.% based on the total weight of the polyamide composition.
[0101] As described herein, the ingredients and additives are selected so that the viscosity of the composition is between 114 ml / g and 300 ml / g as determined according to ISO 307. In one embodiment, the viscosity of the composition of Example 1 is between 114 ml / g and 290 ml / g as determined according to ISO 307. In another embodiment, the viscosity is between 114 ml / g and 280 ml / g, or between 114 ml / g and 270 ml / g, or between 114 ml / g and 260 ml / g. In yet another embodiment, the viscosity is between 114 ml / g and 250 ml / g, or between 114 ml / g and 240 ml / g, or between 114 ml / g and 230 ml / g. In another embodiment, the viscosity is between 114 ml / g and 220 ml / g, or between 114 ml / g and 210 ml / g, or between 114 ml / g and 200 ml / g.
[0102] As described herein, the synergistic amounts of ingredients and additives result in a polyamide composition that meets the highest quality of fire resistance, i.e., the 5VA rating according to the UL94 standard. The flammability test method is determined using the Underwriters Laboratories test method UL94. The standard determines the tendency of a material to extinguish or spread a flame once a sample is ignited. Testing is typically performed on 5" x 1 / 2" samples of the minimum approved thickness. For the 5VA rating, rod and block samples are tested, and the intensity of the flame ignition source is approximately five times that of the flame ignition source used to test other materials. If burning stops within 60 seconds on a vertical specimen, and there is no dripping and no holes are formed in the block specimen, the composition meets the 5VA rating.
[0103] Furthermore, the compositions of the present invention can be readily processed and still exhibit acceptable properties of tensile strength, elongation, flexural strength and Charpy notched strength, making them useful in the manufacture of shaped articles such as industrial fans or blowers.
[0104] method
[0105] Another aspect of the present invention is embodiment 2, which relates to a method for preparing the flame retardant polyamide composition of embodiment 1. As described herein, the method of embodiment 2 includes at least the step of compounding the ingredients and optional additives. Compounding itself is a technique well known to those skilled in the art of polymer processing and manufacturing, and consists of the following: a plastic formulation is prepared by mixing and / or blending the ingredients of embodiment 1 in a molten state and optional additives. In one embodiment, the mixing is carried out at a speed ranging from 200rpm to 320rpm. It is understood in the art that compounding is different from a blending or mixing process carried out at a temperature below the melting temperature of the ingredients. For example, compounding can be used to form a masterbatch composition. For example, compounding can include adding a masterbatch composition to a polymer to form another polymer composition.
[0106] In one embodiment, the polyamide composition in Example 2 can be, for example, extruded. For example, compounding can be performed using a screw, such as a twin screw. For example, compounding can be performed using a multi-roll mill, such as a twin-roll mill. For example, compounding can be performed using a co-kneader or an internal mixer. For example, the method disclosed herein can include compression molding or injection molding. The ingredients and optional additives can be pre-mixed and fed from a single hopper. The resulting melt can be cooled, for example, in a water bath, and then granulated.
[0107] In addition, the polyamide composition in Example 1 or 2 can be formed into a desired shape or article, for example. For example, the molding of the polyamide composition can include heating the composition to soften it. The polyamide composition of Example 1 or 2 can be formed, for example, by molding (e.g., compression molding, injection molding, stretch blow molding, injection blow molding, overmolding), extrusion, casting or thermoforming.
[0108] In one embodiment, the compounding in Example 2 is conducted at a temperature ranging between 220°C to 350°C.
[0109] Molded products
[0110] Another aspect of the present invention is embodiment 3, which relates to a shaped article, said shaped article comprising the polyamide composition of embodiment 1 or the polyamide composition obtained according to embodiment 2. As the name implies, a shaped article is any article obtained using a polyamide composition and suitably shaped.
[0111] In one embodiment, the shaped article of Example 3 is an industrial fan or blower.
[0112] Industrial fans or blowers
[0113] Yet another aspect of the present invention is embodiment 4, which relates to an industrial fan or blower, comprising the polyamide composition of embodiment 1 or the polyamide composition obtained according to embodiment 2.
[0114] An industrial fan or blower is a machine whose primary function is to supply and contain large volumes of air or gas to various parts of a building or other structure, such as a manufacturing facility. This is accomplished by rotating multiple blades that are attached to a hub and shaft and driven by a motor or turbine. These mechanical fans have flow rates ranging from approximately 200 cubic feet per minute (5.7 m 3 ) to 2,000,000 cubic feet (57,000m 3 ). A blower is another name for a fan that operates with resistance to flow primarily on the downstream side of the fan. Industrial fans produce a continuous flow of air or gas for many purposes including, but not limited to, combustion, ventilation, aeration, particulate transport, exhaust, cooling, air cleaning and drying. Industries served include, for example, power generation, pollution control, metal fabrication and processing, cement production, mining, petrochemical, food processing, cryogenics, and clean rooms.
[0115] Due to the high temperature operation of these industrial fans or blowers, it is relevant to choose the construction materials appropriately and, more importantly, to have a very high flame. Thus, the inventive polyamide composition of example 1 or 2 can be used for this purpose.
[0116] Exemplary embodiments of the present invention are listed below, but the present invention is not limited thereto. In particular, the present invention also includes those embodiments resulting from the combinations specified below as a result of the dependent references. More specifically, in the case of naming the scope of the embodiments below, for example, the expression "a method according to any one of embodiments 1 to 4" should be understood so that any combination of the embodiments within the scope is explicitly disclosed to those skilled in the art, which means that the expression should be regarded as synonymous with "a method according to any one of embodiments 1, 2, 3 and 4":
[0117] 1. A flame retardant polyamide composition comprising:
[0118] (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g,
[0119] (b) 20 wt.% to 50 wt.% of a reinforcing agent,
[0120] (c) a flame retardant mixture comprising (i) 1.0 wt.% to 10.0 wt.% of red phosphorus and (ii) 1.0 wt.% to 10.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1,
[0121] (d) 0.1 wt.% to 10.0 wt.% of an impact modifier,
[0122] (e) 0.01 wt.% to 5.0 wt.% of a stabilizer, and
[0123] (f) 0.1 wt.% to 5.0 wt.% of a dispersant,
[0124] The flame retardant polyamide composition has a viscosity number determined according to ISO 307 of at least 114 ml / g.
[0125] II. The composition of embodiment I, wherein the polyamide has a viscosity number determined according to ISO 307 between 150 ml / g and 210 ml / g.
[0126] III. The composition of embodiment I or II, wherein the polyamide comprises an aliphatic polyamide.
[0127] IV. The method according to one or more of embodiments I to III, wherein the polyamide is selected from polyamide 6, polyamide 66, or blends or copolymers thereof.
[0128] V. The composition of one or more of embodiments I to IV, wherein the polyamide comprises polyamide 6.
[0129] VI. The composition of one or more of embodiments I to V, wherein the amount of polyamide is between 30 wt.% and 40 wt.%, based on the total weight of the flame retardant polyamide composition.
[0130] VII. The composition of one or more of Embodiments I to VI, wherein the reinforcing agent is selected from metal fibers, metallized inorganic fibers, metallized synthetic fibers, glass fibers, carbon fibers, ceramic fibers, mineral fibers, basalt fibers, kenaf fibers, jute fibers, flax fibers, hemp fibers, cellulose fibers, sisal fibers, and coconut husk fibers.
[0131] VIII. The composition of one or more of embodiments I to VII, wherein the reinforcing agent is glass fiber.
[0132] IX. The composition of one or more of embodiments I to VIII, wherein the reinforcing agent is subjected to a surface treatment agent.
[0133] X. The composition of embodiment IX, wherein the surface treatment agent is a coupling agent comprising one or more of the following: a silane coupling agent, a titanium coupling agent, an aluminate coupling agent, a urethane coupling agent, and an epoxy coupling agent.
[0134] XI. The composition according to one or more of embodiments I to X, wherein the amount of the reinforcing agent is between 35 wt.% and 45 wt.% based on the total weight of the flame retardant polyamide composition.
[0135] XII. The composition of one or more of embodiments I to XI, wherein the weight ratio between (i) and (ii) is between 1:2 and 2:1.
[0136] XIII. The composition of one or more of embodiments I to XII, wherein the amount of the impact modifier is between 0.1 wt.% and 5.0 wt.%, based on the total weight of the flame retardant polyamide composition.
[0137] XIV. The composition of one or more of embodiments I to XIII, wherein the amount of the stabilizer is between 0.01 wt.% and 2.0 wt.%, based on the total weight of the flame retardant polyamide composition.
[0138] XV. The composition of one or more of embodiments I to XIV, wherein the amount of the dispersant is between 0.1 wt.% and 2.0 wt.%, based on the total weight of the flame retardant polyamide composition.
[0139] XVI. The composition according to one or more of embodiments I to XV, wherein the flame retardant polyamide composition has a viscosity number determined according to ISO 307 between 114 ml / g and 300 ml / g.
[0140] XVII. The composition according to one or more of embodiments I to XVI, further comprising an additive.
[0141] XVIII. The composition of embodiment XVII, wherein the additive is selected from dyes, pigments, UV absorbers, antistatic agents, fungistats, bacteriostats, and IR absorbing materials.
[0142] XIX. The composition of embodiment XVII or XVIII, wherein the amount of the additive is between 0.1 wt.% and 10 wt.%, based on the total weight of the flame retardant polyamide composition.
[0143] XX. The composition according to one or more of embodiments I to XVIII, wherein the flame retardant polyamide composition meets the fire resistance requirements of 5VA according to the UL94 standard.
[0144] XXI. A method for preparing a flame retardant polyamide composition according to one or more of embodiments I to XX, the method comprising at least the step of compounding:
[0145] (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g,
[0146] (b) 20 wt.% to 50 wt.% of a reinforcing agent,
[0147] (c) a flame retardant mixture comprising (i) 1.0 to 10.0 wt.% of red phosphorus and (ii) 1.0 to 10.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1,
[0148] (d) 0.1 wt.% to 10.0 wt.% of an impact modifier,
[0149] (e) 0.01 to 5.0 wt.% of a stabilizer, and
[0150] (f) 0.1 to 5.0 wt.% of a dispersant,
[0151] Said flame retardant polyamide composition having a viscosity number determined according to ISO 307 of at least 114 ml / g is obtained.
[0152] XXII. The method of embodiment XXI, wherein the compounding is performed at a temperature between 220°C and 350°C.
[0153] XXIII. A shaped article comprising the flame retardant polyamide composition according to one or more of embodiments I to XX or obtained by the process according to embodiment XXI or XXII.
[0154] XXIV. The shaped article of embodiment XXIII, wherein the shaped article is an industrial fan or blower.
[0155] XXV. A shaped article comprising a flame retardant polyamide, the flame retardant polyamide comprising:
[0156] (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g,
[0157] (b) 20 wt.% to 50 wt.% of a reinforcing agent,
[0158] (c) a flame retardant mixture comprising (i) 1.0 wt.% to 10.0 wt.% of red phosphorus and (ii) 1.0 wt.% to 10.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1,
[0159] (d) 0.1 wt.% to 10.0 wt.% of an impact modifier,
[0160] (e) 0.01 wt.% to 5.0 wt.% of a stabilizer, and
[0161] (f) 0.1 wt.% to 5.0 wt.% of a dispersant,
[0162] wherein the flame retardant polyamide composition has a viscosity number determined according to ISO 307 of at least 114 ml / g, and the shaped article is an industrial fan or blower.
[0163] XXVI. An industrial fan or blower comprising the flame retardant polyamide composition according to one or more of embodiments I to XX or obtained by the method according to embodiment XXI or XXII.
[0164] XXVII. An industrial fan or blower comprising a flame retardant polyamide composition comprising:
[0165] (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g,
[0166] (b) 20 wt.% to 50 wt.% of a reinforcing agent,
[0167] (c) a flame retardant mixture comprising (i) 1.0 wt.% to 10.0 wt.% of red phosphorus and (ii) 1.0 wt.% to 10.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1,
[0168] (d) 0.1 wt.% to 10.0 wt.% of an impact modifier,
[0169] (e) 0.01 wt.% to 5.0 wt.% of a stabilizer, and
[0170] (f) 0.1 wt.% to 5.0 wt.% of a dispersant,
[0171] The flame retardant polyamide composition has a viscosity number determined according to ISO 307 of at least 114 ml / g.
[0172] Examples
[0173] The presently claimed invention is illustrated by the following non-limiting examples:
[0174] raw materials
[0175]
[0176] Standard Methods
[0177] Tensile Strength ISO 527 % Elongation ISO 527 Bending Strength ISO 178 Charpy impact resistance ISO 179 Charpy notch resistance ISO 179
[0178] General Synthesis of Flame Retardant Polyamide Compositions
[0179] Details concerning the inventive and comparative polyamide compositions are summarized in the following Table 1. All amounts are in wt. %.
[0180] Table 1: Inventive polyamide compositions and comparative polyamide compositions
[0181]
[0182] nd = not determined
[0183] The present invention and comparative polyamide compositions were extruded using a WP 25 mm laboratory twin screw extruder under the above process conditions. Another comparative example (Comparative Example 2) of B3G8BK (polyamide 6 with 40% glass fibers), but which does not contain the flame retardant mixture according to the invention.
[0184] Mechanical testing and UL94 flame retardancy
[0185] ISO A-type rod samples with a size of 10.0 mm × 4.0 mm were prepared and their mechanical properties were tested according to the corresponding standards. In addition, samples with a thickness of 2.0 mm were prepared and flame retardancy tests were performed according to the UL94 standard. The test results are summarized in Table 2 below.
[0186] Table 2: Test results of the samples of the present invention and the comparative samples
[0187]
[0188]
[0189] It can be observed that the polyamide composition of the present invention meets the flammability requirements of 5VA according to the UL94 standard, while the comparative formulation according to the present invention containing only red phosphorus (see Comparative Example 1) and the comparative formulation without any flame retardant (see Comparative Example 2) do not meet the above requirements. In addition, the polyamide composition of the present invention has similar properties to the comparative formulation, which makes them suitable for the desired applications, in particular industrial fans or blowers.
Claims
1. An industrial fan or blower comprising a flame retardant polyamide composition, the composition comprising: (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g, (b) 20 wt.% to 50 wt.% of a reinforcing agent, (c) a flame retardant mixture comprising (i) 1.0 wt.% to 10.0 wt.% of red phosphorus and (ii) 4.0 wt.% to 9.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1, (d) 0.1 wt.% to 10.0 wt.% of an impact modifier, (e) 0.01 wt.% to 5.0 wt.% of a stabilizer, and (f) 0.1 wt.% to 5.0 wt.% of a dispersant, The flame retardant polyamide composition has a viscosity number determined according to ISO 307 of at least 114 ml / g.
2. An industrial fan or blower according to claim 1, wherein the polyamide has a viscosity number determined according to ISO 307 between 150 ml / g and 210 ml / g.
3. An industrial fan or blower according to claim 1 or 2, wherein the polyamide is selected from polyamide 6, polyamide 66 or blends or copolymers thereof.
4. An industrial fan or blower according to claim 1 or 2, wherein the reinforcement is glass fiber.
5. An industrial fan or blower according to claim 1 or 2, wherein the weight ratio between (i) and (ii) is between 1:2 and 2:
1.
6. The industrial fan or blower of claim 1 or 2, further comprising an additive.
7. An industrial fan or blower according to claim 6, wherein the additive is selected from dyes, pigments, UV absorbers, antistatic agents, fungistats, bacteriostats and IR absorbing materials.
8. The industrial fan or blower according to claim 1 or 2, wherein the flame retardant polyamide composition meets the fire resistance requirements of 5VA according to UL94 standard.
9. A flame retardant polyamide composition comprising: (a) 20 wt.% to 60 wt.% of a polyamide having a viscosity number determined according to ISO 307 between 90 ml / g and 350 ml / g, (b) 20 wt.% to 50 wt.% of a reinforcing agent, (c) a flame retardant mixture comprising (i) 1.0 wt.% to 10.0 wt.% of red phosphorus and (ii) 4.0 wt.% to 9.0 wt.% of magnesium hydroxide, based on the total weight of the flame retardant polyamide composition, wherein the weight ratio between (i) and (ii) in the flame retardant mixture is between 1:5 and 5:1, (d) 0.1 wt.% to 10.0 wt.% of an impact modifier, (e) 0.01 wt.% to 5.0 wt.% of a stabilizer, and (f) 0.1 wt.% to 5.0 wt.% of a dispersant, The flame retardant polyamide composition has a viscosity number determined according to ISO 307 of at least 114 ml / g.
10. The composition according to claim 8, wherein the polyamide has a viscosity number determined according to ISO 307 between 150 ml / g and 210 ml / g.
11. The composition of claim 9, wherein the polyamide is selected from polyamide 6, polyamide 66, or blends or copolymers thereof.
12. The composition of claim 9, wherein the reinforcing agent is glass fiber.
13. The composition of claim 9, wherein the weight ratio between (i) and (ii) is between 1:2 and 2:
1.
14. The composition according to claim 8, further comprising an additive.
15. The composition of claim 14, wherein the additive is selected from dyes, pigments, UV absorbers, antistatic agents, fungistats, bacteriostats and IR absorbing materials.
16. The composition according to claim 9, wherein the flame retardant polyamide composition meets the fire resistance requirements of 5VA according to UL94 standard.
17. A method for preparing the flame retardant polyamide composition according to claim 9, the method comprising At least components (a) to (f) are compounded, and the flame retardant polyamide composition is obtained.
18. The method of claim 17, wherein the compounding is performed at a temperature between 220°C and 350°C.
19. A shaped article comprising The flame retardant polyamide composition according to claim 9.
20. The shaped article of claim 19, wherein the shaped article is an industrial fan or blower.
21. An industrial fan or blower comprising the flame retardant polyamide composition according to claim 9.