Continuous fiber reinforced resin composite material and method for producing the same, and continuous fiber reinforced resin molded body

By improving the interfacial viscoelastic characteristics and the combination of multiple thermoplastic resins, the problem of insufficient interface characteristics between matrix resin and reinforced fiber in the prior art is solved, and the strength, rigidity, high temperature characteristics and water absorption characteristics of the continuous fiber reinforced resin composite material are significantly improved. Improved appearance performance.

CN115279821BActive Publication Date: 2024-11-12ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180020167.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-27
Filing Date
2021-03-16
Publication Date
2024-11-12
Estimated Expiration
2041-03-16

AI Technical Summary

Technical Problem

Among the existing continuous fiber reinforced resin composite materials, the interface characteristics between the matrix resin and the reinforced fiber are insufficient, resulting in room for improvement in strength, rigidity, high temperature characteristics, water absorption characteristics, impact characteristics and appearance.

Method used

By improving the interfacial viscoelastic properties of continuous fiber-reinforced resin composites, the specific methods include adjusting the aromatic ring concentration and wettability in the resin, improving the interface strength and interface constant, and combining a variety of thermoplastic resins to ensure the tanδ peak at the interface The temperature reaches above 80°C and optimize the interaction between fiber and resin.

Benefits of technology

The strength, rigidity, high temperature characteristics, water absorption characteristics and impact characteristics of the material are significantly improved, while improving the appearance performance, forming a continuous fiber reinforced resin composite material with excellent interfacial characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003840088250000181
    Figure BDA0003840088250000181
  • Figure BDA0003840088250000401
    Figure BDA0003840088250000401
  • Figure BDA0003840088250000411
    Figure BDA0003840088250000411
Patent Text Reader

Abstract

The continuous fiber reinforced resin composite material of the present invention comprises continuous reinforcing fibers and a thermoplastic resin, and is characterized in that the peak temperature of tan δ at the interface between the continuous reinforcing fibers and the thermoplastic resin is 80° C. or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a continuous fiber reinforced resin composite material and a method for producing the same, and a continuous fiber reinforced resin molded body. Background Art

[0002] Composite molded bodies formed by adding reinforcing materials such as glass fibers to matrix resin materials are used in various structural parts of machinery or automobiles, pressure vessels, and tubular structures. In particular, from the perspective of strength, a continuous fiber reinforced resin composite material in which the reinforcing fibers are continuous fibers is desired. As such continuous fiber reinforced resin composite materials, the following schemes have been proposed: a scheme for studying a sizing agent added to reinforcing fibers (for example, see Patent Document 1 below); a scheme for studying the difference between the melting point and the crystallization temperature (for example, see Patent Document 2 below); a scheme for adding an organic salt to a resin material (for example, see Patent Document 3 below); a scheme for laminating a fabric of a molding precursor with a thermoplastic resin (for example, see Patent Document 4 below).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2003-238213

[0006] Patent Document 2: Japanese Patent No. 5987335

[0007] Patent Document 3: Japanese Patent Application Publication No. 2017-222859

[0008] Patent Document 4: Japanese Patent Application Publication No. 2009-19202 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, the inventors have conducted in-depth research and found that in the continuous fiber reinforced resin composite materials of the prior art, the interface properties between the matrix resin and the reinforcing fibers are insufficient, and there is still room for improvement in strength, rigidity, high temperature properties, water absorption properties, impact properties and appearance.

[0011] In view of the level of these prior arts, the problem to be solved by the present invention is to provide a continuous fiber reinforced resin composite material and a method for manufacturing the same, as well as a continuous fiber reinforced resin molded body, wherein the continuous fiber reinforced resin composite material can improve the interface properties between the matrix resin and the reinforcing fibers, and has excellent strength, rigidity, high temperature properties, water absorption properties, impact properties and appearance.

[0012] Means for solving problems

[0013] The inventors have repeatedly conducted in-depth research and experiments to solve this problem, and unexpectedly found that by improving the viscoelastic properties of the interface of continuous fiber reinforced resin composite materials, a continuous fiber reinforced resin composite material having high strength and rigidity, as well as excellent interface properties, high temperature properties, water absorption properties, impact properties and appearance can be obtained, thereby completing the present invention.

[0014] That is, the present invention is as follows. [1]

[0016] A continuous fiber reinforced resin composite material, comprising continuous reinforcing fibers and a thermoplastic resin, characterized in that:

[0017] The continuous fiber-reinforced resin composite material has a tan δ peak temperature of 80° C. or higher at an interface between the continuous reinforcing fibers and the thermoplastic resin. [2]

[0019] The continuous fiber reinforced resin composite material as described in [1], wherein the interface strength of the continuous fiber reinforced resin composite material based on a push-out test is 1.58 to 5.00 mN / μm. [3]

[0021] The continuous fiber reinforced resin composite material as described in [1] or [2], wherein the interface constant of the continuous fiber reinforced resin composite material represented by the following formula is 20 to 100.

[0022] (Interface constant) = (concentration of carboxyl terminal groups in continuous fiber-reinforced resin composite material [μmol / g]) × (grinding pressure at which interface peeling occurs [MPa]) × (reinforcement fiber diameter [μm]) / (reinforcement fiber density [g / cm 3 ]) 2 [4]

[0024] The continuous fiber reinforced resin composite material as described in any one of [1] to [3], wherein the continuous reinforcing fiber composite material has a thickness of 950 to 1050 cm -1 Has Raman peak. [5]

[0026] The continuous fiber-reinforced resin composite material according to any one of [1] to [4], wherein the thermoplastic resin is two or more types. [6]

[0028] The continuous fiber reinforced resin composite material according to any one of [1] to [5], wherein the peak intensity of the (1,0,0) plane of the continuous fiber reinforced resin composite material in X-ray diffraction is stronger than the peak intensity of the (0,1,0) plane. [7]

[0030] The continuous fiber-reinforced resin composite material according to any one of [1] to [6], wherein a peak of a (1,1,0) plane is detected in X-ray diffraction of the continuous fiber-reinforced resin composite material. [8]

[0032] The continuous fiber reinforced resin composite material according to any one of [1] to [7], wherein

[0033] The continuous reinforcing fibers are woven fabrics, unidirectional materials or non-crimped fabrics of glass fibers.

[0034] The thermoplastic resin comprises 50 to 99 parts by mass of (A) an aliphatic polyamide and 1 to 50 parts by mass of (B) a semi-aromatic polyamide, wherein the (B) semi-aromatic polyamide comprises a dicarboxylic acid unit comprising at least 75 mol % of an isophthalic acid unit and a diamine unit comprising at least 50 mol % of a diamine unit having 4 to 10 carbon atoms,

[0035] The weight average molecular weight (Mw) of the thermoplastic resin is 15,000 to 35,000. [9]

[0037] The continuous fiber-reinforced resin composite material as described in [8], wherein the amount of blocked terminals expressed as equivalents per gram of the (A) aliphatic polyamide and the (B) semi-aromatic polyamide is 5 to 180 micro equivalents / g.

[10]

[0039] A continuous fiber reinforced resin molded body, comprising continuous reinforcing fibers and a thermoplastic resin, characterized in that:

[0040] The continuous fiber reinforced resin composite molded body has a tanδ peak temperature of 80°C or higher at the interface between the continuous reinforcing fibers and the thermoplastic resin, an interface strength of 1.58 to 5.00 mN / μm based on an ejection test, and has a plate-like, frame-like, box-like, or a combination thereof shape.

[11]

[0042] A method for producing a continuous fiber reinforced resin composite material, which is a method for producing a continuous fiber reinforced resin composite material according to any one of [1] to [9], wherein continuous reinforcing fibers are composited with a thermoplastic resin, and the method is characterized in that the dynamic wettability of the continuous reinforcing fibers with the thermoplastic resin is less than 3.0 sec.

[12]

[0044] The method for producing a continuous fiber-reinforced resin composite material as described in

[11] , wherein the contact angle between the continuous reinforcing fiber and the thermoplastic resin based on a static wettability test is 38° or less.

[13]

[0046] The method for producing a continuous fiber reinforced resin composite material as described in

[11] or

[12] , wherein the thermoplastic resin comprises two or more types, and the maximum value of the difference in dynamic wettability between each of the two or more thermoplastic resins and the continuous reinforcing fiber is greater than 3 sec.

[14]

[0048] The method for producing a continuous fiber reinforced resin composite material according to any one of

[11] to

[13] , wherein:

[0049] The thermoplastic resin comprises 50 to 99 parts by mass of (A) an aliphatic polyamide and 1 to 50 parts by mass of (B) a semi-aromatic polyamide, wherein the (B) semi-aromatic polyamide comprises a dicarboxylic acid unit comprising at least 75 mol % of an isophthalic acid unit and a diamine unit comprising at least 50 mol % of a diamine unit having 4 to 10 carbon atoms,

[0050] The terminal group concentration of the aliphatic polyamide (A) is 1 / 2 or less of the terminal group concentration of the semi-aromatic polyamide (B).

[15]

[0052] The method for producing a continuous fiber-reinforced resin composite material as described in

[14] , wherein the difference in tan δ peak temperature between the aliphatic polyamide (A) and the semi-aromatic polyamide (B) is 45 to 100°C.

[16]

[0054] The method for producing a continuous fiber-reinforced resin composite material as described in

[14] or

[15] , wherein the weight average molecular weight MwA of the aliphatic polyamide (A) is 1.5 times or more the weight average molecular weight MwB of the semi-aromatic polyamide (B).

[0055] Effects of the Invention

[0056] The continuous fiber reinforced resin composite material and the continuous fiber reinforced resin molded body of the present invention can exhibit high strength and rigidity, as well as excellent interface characteristics, high temperature characteristics, water absorption characteristics, impact characteristics and appearance. DETAILED DESCRIPTION

[0057] A specific embodiment of the present invention (hereinafter referred to as "this embodiment") will be described in detail below. The following this embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following contents.

[0058] [Continuous fiber reinforced resin composite materials]

[0059] The continuous fiber reinforced resin composite material of the present embodiment is a continuous fiber reinforced resin composite material comprising continuous reinforcing fibers and a thermoplastic resin, and is characterized in that the peak temperature of tan δ at the interface between the continuous reinforcing fibers and the thermoplastic resin is 80° C. or higher.

[0060] In this specification, the continuous fiber-reinforced resin composite material according to the present embodiment may be simply referred to as a "composite material".

[0061] The peak temperature of the loss tangent tanδ of the continuous fiber reinforced resin composite material of the present embodiment refers to the temperature at which the value of tanδ reaches a maximum when tanδ of the interface between the continuous reinforcing fiber and the thermoplastic resin is measured at each temperature while changing the temperature. When there are two or more temperatures reaching a maximum, the temperature of the peak with the largest maximum value is taken as the peak temperature of tanδ. The peak temperature of tanδ can be obtained, for example, by using a nanoindenter to perform nanoindentation (nanoDMA) measurement on a single filament of a continuous reinforcing fiber in a cross section orthogonal to the length direction of the continuous reinforcing fiber contained in the continuous fiber reinforced resin composite material and applying vibration of a specific frequency. Specifically, it can be measured by the method described in the embodiments described later.

[0062] The peak temperature of tan δ of the continuous fiber-reinforced resin composite material is 80° C. or higher, preferably 85° C. or higher, more preferably 90° C. or higher, and even more preferably 100° C. or higher.

[0063] As a method for adjusting the peak temperature of tan δ of the continuous fiber reinforced resin composite material to the above range, for example, a method of adjusting the aromatic ring concentration in the resin and adjusting the static wettability can be cited. If the aromatic ring concentration in the resin is increased and the contact angle based on the static wettability test is reduced, the peak temperature of tan δ tends to increase.

[0064] The continuous fiber reinforced resin composite material of this embodiment is preferably 950 to 1050 cm -1 It has a Raman peak (Raman spectrum peak), preferably at 970 to 1030 cm -1 Has Raman peak.

[0065] The Raman peak of the continuous fiber reinforced resin composite material of the present embodiment can be obtained by measuring the Raman spectrum of the resin region in the cross section perpendicular to the length direction of the continuous reinforcing fiber contained in the continuous fiber reinforced resin composite material using a laser Raman microscope, and specifically, it can be measured by the method described in the examples described later. When the Raman peak is within the above range, there is a tendency to have good strength, rigidity, water absorption characteristics, high temperature characteristics, and appearance.

[0066] The continuous fiber reinforced resin composite material of the present embodiment preferably has a peak intensity I(1,0,0) of the (1,0,0) plane in X-ray diffraction that is stronger than the peak intensity I(0,1,0) of the (0,1,0) plane. Specifically, the ratio (I(0,1,0) / I(1,0,0)) of the peak intensity I(0,1,0) of the (0,1,0) plane to the peak intensity I(1,0,0) of the (1,0,0) plane is preferably 0.30 to 0.95, more preferably 0.40 to 0.90, and even more preferably 0.50 to 0.87. When the ratio (I(0,1,0) / I(1,0,0)) is within the above range, the strength, rigidity, water absorption properties, impact properties, high temperature properties, and appearance tend to be good.

[0067] The continuous fiber reinforced resin composite material of this embodiment preferably has a peak of (1,1,0) plane detected in X-ray diffraction. When the peak of (1,1,0) plane is detected, the strength, rigidity, water absorption properties, impact properties, high temperature properties, and appearance tend to be good.

[0068] The X-ray diffraction peak of the continuous fiber-reinforced resin composite material can be measured, for example, using an X-ray diffractometer, and specifically, can be measured by the method described in the Examples below.

[0069] The interface strength of the continuous fiber reinforced resin composite material of the present embodiment (interface strength between the matrix resin and the reinforcing fiber of the continuous fiber reinforced resin composite material) is preferably 1.58mN / μm or more, more preferably 1.65mN / μm or more, further preferably 1.75mN / μm or more, and further preferably 1.85mN / μm or more. In addition, the interface strength is preferably 5.00mN / μm or less, more preferably 4.50mN / μm or less, and further preferably 3.50mN / μm or less. When the interface strength is within the above range, there is a tendency to improve strength, rigidity, water absorption characteristics, impact characteristics, and high temperature characteristics.

[0070] The interfacial strength of the continuous fiber composite material can be determined, for example, by performing a push-out test using a nanoindenter on a single continuous reinforcing fiber in a cross section perpendicular to the longitudinal direction of the continuous reinforcing fiber contained in the continuous fiber reinforced resin composite material. Specifically, it can be measured by the method described in the examples below.

[0071] As a method for adjusting the interface strength of the continuous fiber reinforced resin composite material of the present embodiment based on the ejection test to the above-mentioned range, for example, a method of adjusting the dynamic wettability and static wettability of the thermoplastic resin and the continuous reinforcing fibers can be cited. If the dynamic wettability is reduced and the contact angle based on the static wettability test is reduced, the interface strength tends to increase.

[0072] In the continuous fiber reinforced resin composite material of the present embodiment, the interface constant represented by the following formula is preferably 20 or more, more preferably 30 or more, further preferably 50 or more, and further preferably 65 or more. In addition, the interface constant is preferably 100 or less, more preferably 90 or less, and further preferably 80 or less.

[0073] (Interface constant) = (concentration of carboxyl terminal groups in continuous fiber-reinforced resin composite material [μmol / g]) × (grinding pressure at which interface peeling occurs [MPa]) × (reinforcement fiber diameter [μm]) / (reinforcement fiber density [g / cm 3 ]) 2

[0074] When the interface constant is within the above range, the strength, rigidity, water absorption characteristics, and high-temperature characteristics tend to be good.

[0075] In the above formula, the "concentration of carboxyl terminal groups in the continuous fiber-reinforced resin composite material" can be expressed as 1 H-NMR can be measured, and specifically, it can be measured by the method described in the examples described later.

[0076] The “grinding pressure at which interface peeling occurs” refers to a pressure at which a void is generated at the extreme interface between one of the continuous reinforcing fibers and the thermoplastic resin in the cross section perpendicular to the longitudinal direction of the continuous reinforcing fibers when the cross section in the thickness direction of the continuous fiber-reinforced resin (the cross section perpendicular to the longitudinal direction of the continuous reinforcing fibers) is cut into a specific size, the cross section is ground at varying pressures, and the ground sample is subjected to SEM observation.

[0077] The "reinforcing fiber diameter" can be obtained by cutting a cross section in the thickness direction of the continuous fiber-reinforced resin (a cross section perpendicular to the longitudinal direction of the continuous reinforcing fibers) into a specific size, grinding, and observing the grinded sample under SEM. The diameters of 10 or more continuous reinforcing fibers are measured based on the substantially circular cross section of the continuous reinforcing fibers in the cross section perpendicular to the longitudinal direction of the continuous reinforcing fibers, and the average value is obtained as the reinforcing fiber diameter.

[0078] The “reinforcement fiber density” can be determined by burning off the thermoplastic resin of the continuous fiber-reinforced resin in, for example, an electric furnace and measuring the remaining continuous reinforcement fibers with a specific gravity meter.

[0079] The continuous fiber-reinforced resin composite material of the present embodiment has a tensile stress (23° C., 50% RH) of preferably 500 MPa or more, more preferably 540 MPa or more.

[0080] Furthermore, the tensile stress retention rate of the continuous fiber-reinforced resin composite material at 80° C. is preferably 80% or more, more preferably 90% or more.

[0081] Furthermore, the tensile stress retention rate of the continuous fiber-reinforced resin composite material when absorbing water is preferably 80% or more, more preferably 90% or more.

[0082] It should be noted that the tensile stress can be measured by the method described in the examples described below. Regarding the tensile stress during water absorption, the test piece can be immersed in a constant temperature water bath at 80°C for 18 hours, and then placed in a constant temperature and humidity bath at 80°C and 57% RH for more than 150 hours, and the sample adjusted until the mass reaches a constant value is used as the sample during water absorption.

[0083] The tensile stress retention rate (%) at 80° C. and the tensile stress retention rate (%) upon water absorption can be obtained by the following formulae, respectively.

[0084] Tensile stress retention at 80°C = (tensile stress at 80°C, 50% RH / tensile stress at 23°C, 50% RH) × 100

[0085] Tensile stress retention rate when absorbing water = (tensile stress when absorbing water / tensile stress at 23°C, 50% RH) × 100

[0086] The bending stress (23° C., 50% RH) of the continuous fiber-reinforced resin composite material of the present embodiment is preferably 700 MPa or more, more preferably 800 MPa or more.

[0087] Furthermore, the bending stress retention rate of the continuous fiber-reinforced resin composite material at 80° C. is preferably 60% or more, more preferably 65% ​​or more.

[0088] Furthermore, the bending stress retention rate of the continuous fiber-reinforced resin composite material when absorbing water is preferably 80% or more, more preferably 90% or more.

[0089] The bending stress can be measured by the method described in the examples below. The bending stress during water absorption can be measured similarly using the test piece for measuring the tensile stress during water absorption described above.

[0090] The bending stress retention rate (%) at 80° C. and the bending stress retention rate (%) when absorbing water can be respectively calculated by the following formulae.

[0091] Bending stress retention at 80°C = (bending stress at 80°C, 50% RH / bending stress at 23°C, 50% RH) × 100

[0092] Bending stress retention rate when absorbing water = (bending stress when absorbing water / bending stress at 23°C, 50% RH) × 100

[0093] The flexural modulus (23° C., 50% RH) of the continuous fiber-reinforced resin composite material of the present embodiment is preferably 26 GPa or more, more preferably 27 GPa or more.

[0094] The flexural modulus retention rate of the continuous fiber-reinforced resin composite material at 80° C. is preferably 80% or more, more preferably 90% or more.

[0095] Furthermore, the flexural modulus retention rate of the continuous fiber-reinforced resin composite material when absorbing water is preferably 80% or more, more preferably 90% or more.

[0096] The flexural modulus can be measured by the method described in the examples below. The flexural modulus when absorbing water can be measured similarly using the test piece for measuring the tensile stress when absorbing water.

[0097] The flexural modulus retention rate (%) at 80° C. and the flexural modulus retention rate (%) upon water absorption can be obtained by the following formulae, respectively.

[0098] Flexural modulus retention at 80°C = (flexural modulus at 80°C, 50% RH / flexural modulus at 23°C, 50% RH) × 100

[0099] Flexural modulus retention rate when absorbing water = (flexural modulus when absorbing water / flexural modulus at 23°C, 50% RH) × 100

[0100] The continuous fiber-reinforced resin composite material of the present embodiment has an impact strength of preferably 5.0 kN / m or more, more preferably 5.5 kN / m or more.

[0101] The impact strength is a value obtained by dividing the maximum impact strength (kN) determined by a high-speed impact test (in accordance with JIS K7211-2; 2006) by the thickness of the test piece, and can be specifically measured by the method described in the examples described below.

[0102] (Morphology of continuous fiber reinforced resin composite materials)

[0103] The form of the continuous fiber reinforced resin composite material is not particularly limited, and the following various forms can be cited. For example, the form can be cited: a form in which a woven or knitted fabric, a braid, or a tubular product of continuous reinforcing fibers is compounded with a thermoplastic resin; a form in which continuous reinforcing fibers pulled in one direction are compounded with a thermoplastic resin; a form in which filaments composed of continuous reinforcing fibers and a thermoplastic resin are pulled in one direction and formed; a form in which filaments composed of continuous reinforcing fibers and a thermoplastic resin are formed into a woven or knitted fabric, a braid, or a tubular product.

[0104] The continuous fiber reinforced resin composite material of this embodiment may be a flat plate, or a laminate comprising a layer of continuous reinforcing fibers and a layer of thermoplastic resin. For example, the length direction of the continuous reinforcing fibers may be arranged substantially parallel to the surface of the flat plate, in which case the cross section orthogonal to the length direction of the continuous reinforcing fibers in the continuous fiber reinforced resin composite material may be a cross section in the thickness direction of the continuous fiber reinforced resin composite material. In addition, the layer of continuous reinforcing fibers may be a layer comprising continuous reinforcing fibers (e.g., a continuous reinforcing fiber substrate), or a layer in which the interior of the continuous reinforcing fibers is impregnated with a thermoplastic resin.

[0105] Examples of the intermediate material form of the continuous fiber reinforced resin composite material before molding include: mixed yarn of continuous reinforcing fibers and resin fibers; coated yarn formed by wrapping the continuous reinforcing fiber bundle with resin; a form in which the continuous reinforcing fibers are pre-impregnated with resin to form a strip; a form in which the continuous reinforcing fibers are sandwiched between resin films; a form in which resin powder is attached to the continuous reinforcing fibers; a bundle of continuous reinforcing fibers is used as a core material and the bundle is braided with resin fibers around it; a form in which the reinforcing fibers are pre-impregnated with resin; and the like.

[0106] (Method for producing continuous fiber reinforced resin composite material)

[0107] The method for producing the continuous fiber-reinforced resin composite material is not particularly limited, and the following various methods may be mentioned.

[0108] For example, the substrate constituting the continuous fiber reinforced resin composite material (e.g., a substrate composed of continuous reinforcing fibers, a substrate composed of thermoplastic resin) is cut according to the desired composite material, the required number of layers are stacked considering the thickness of the target product, and the layers are set according to the mold shape.

[0109] The method for producing the continuous fiber reinforced resin composite material of the present embodiment is preferably a method of compounding a thermoplastic resin with continuous reinforcing fibers, wherein the dynamic wettability of the continuous reinforcing fibers with the thermoplastic resin is 3.0 sec or less, and the thermoplastic resin preferably includes two or more types.

[0110] The dynamic wettability of the continuous reinforcing fiber and the thermoplastic resin can be evaluated, for example, by immersing the single filament of the continuous reinforcing fiber in a molten thermoplastic resin using a solder wettability tester, bringing the continuous reinforcing fiber into contact with the thermoplastic resin, and measuring the time from the time when the load takes a negative maximum value to the time when the load returns to 0 (wetting time), thereby evaluating the dynamic wettability. Specifically, it can be measured by the method described in the Examples described later.

[0111] The dynamic wettability between the continuous reinforcing fibers and the thermoplastic resin is preferably 3.0 sec or less, more preferably 2.5 sec or less, and even more preferably 2.0 sec or less. When the dynamic wettability is within the above range, a good interface can be formed.

[0112] Furthermore, when the continuous fiber-reinforced resin composite material of the present embodiment includes two or more thermoplastic resins, the maximum value of the difference in dynamic wettability between the thermoplastic resins may be 3 sec or more.

[0113] The contact angle between the continuous reinforcing fiber and the thermoplastic resin based on the static wettability test is preferably 38° or less, more preferably 36° or less, further preferably 34° or less, further preferably 32° or less, and particularly preferably 30° or less. When the contact angle based on the static wettability test is within the above range, a good interface can be formed.

[0114] The contact angle based on the static wettability test can be measured, for example, by sandwiching a single fiber of the continuous reinforcing fiber and a film of the thermoplastic resin between a cover glass and observing the contact angle between the continuous reinforcing fiber and the resin when the temperature is increased using an optical microscope. Specifically, the contact angle can be measured by the method described in the examples described below.

[0115] The cutting of the substrate can be performed piece by piece, or after the desired number of sheets are overlapped. From the aspect of productivity, it is preferred to cut in an overlapping state. The cutting method can be any method, for example, a water jet, a blade press, a hot blade press, a laser machine, a cutting plotter, etc. are cited. Preferably, a hot blade press with excellent cross-sectional shape and good handling properties by fusing the end faces when cutting multiple sheets overlapped is used. The appropriate cutting shape can also be adjusted by repeated trial and error, but is preferably set by simulation based on CAE (computer-aided engineering) according to the shape of the mold.

[0116] After placing the substrate in the mold, the mold is closed for compression. Afterwards, the mold is adjusted to a temperature above the melting point of the thermoplastic resin constituting the continuous fiber reinforced resin composite material, so that the thermoplastic resin is melted for shaping. The mold clamping pressure is not particularly limited, and is preferably above 1 MPa, and more preferably above 3 MPa. In addition, in order to vent, etc., the mold can be temporarily closed, and the mold clamping pressure of the mold can be temporarily released after compression molding. From the aspect of showing strength, the time of compression molding is preferably a long time within the range where the thermoplastic resin used does not thermally deteriorate. From the aspect of productivity, it is preferably within 2 minutes, and more preferably within 1 minute.

[0117] The continuous fiber reinforced resin composite material can be further injection filled with a thermoplastic resin composition for mixing to form a hybrid molded body. In the manufacturing process of the hybrid molded body, the substrate is placed in a mold, the mold is closed and pressurized, and after a specific time, a specific thermoplastic resin composition for mixing is further injection filled for molding, so that the thermoplastic resin and the specific thermoplastic resin composition for mixing are bonded, thereby manufacturing a hybrid molded body.

[0118] The timing of injection filling of a specific thermoplastic resin composition for mixing has a great influence on the interfacial strength between the two thermoplastic resins. The timing of injection filling of a specific thermoplastic resin composition for mixing is preferably within 30 seconds after the substrate is placed in the mold, the mold is closed, and the mold temperature is raised to a temperature above the melting point or glass transition temperature of the thermoplastic resin.

[0119] The mold temperature when injecting and filling the specific thermoplastic resin composition for mixing is preferably higher than the melting point or the glass transition temperature of the thermoplastic resin constituting the continuous fiber reinforced resin composite material bonded to the thermoplastic resin composition for mixing. More preferably, it is higher than the melting point of the thermoplastic resin constituting the continuous fiber reinforced resin composite material bonded to the thermoplastic resin composition for mixing + 10°C or higher than the glass transition temperature + 10°C, further preferably higher than the melting point + 20°C or higher than the glass transition temperature + 20°C, and further more preferably higher than the melting point + 30°C or higher than the glass transition temperature + 30°C.

[0120] In the hybrid molded product, the bonded portion between the thermoplastic resin constituting the continuous fiber-reinforced resin composite material and the thermoplastic resin composition for hybrid formed by injection molding preferably forms a concavo-convex structure in which they are mixed with each other.

[0121] In order to improve the interface strength, it is effective to set the mold temperature to the melting point of the injected thermoplastic resin composition and to increase the resin holding pressure during injection molding (for example, to 1 MPa or more). In order to improve the interface strength, the holding pressure is preferably 5 MPa or more, more preferably 10 MPa or more.

[0122] From the viewpoint of improving the interface strength, the pressure holding time is preferably extended, for example, to 5 seconds or more, preferably 10 seconds or more, and more preferably the holding time is until the mold temperature reaches the melting point of the thermoplastic resin composition or less.

[0123] (Resin for injection molding)

[0124] The thermoplastic resin composition for injection molding used to produce the hybrid molded body is not particularly limited as long as it is a thermoplastic resin composition commonly used in injection molding.

[0125] Examples of the thermoplastic resin composition for mixing include, but are not limited to, polyethylene, polypropylene, polyvinyl chloride, acrylic resins, styrene resins, polyethylene terephthalate, polybutylene terephthalate, polyarylate, polyphenylene ether, modified polyphenylene ether resin, wholly aromatic polyester, polyacetal, polycarbonate, polyetherimide, polyethersulfone, polyamide resin, polysulfone, polyetheretherketone, polyetherketone, etc., or a resin composition obtained by mixing two or more thereof.

[0126] Various fillers may be compounded in the thermoplastic resin composition for mixing. The thermoplastic resin composition for mixing may be a black resin composition containing a colorant.

[0127] Examples of various fillers include short fibers and long fiber materials that are discontinuous reinforcement materials of the same kind as the above-mentioned continuous reinforcement fibers.

[0128] When glass short fibers or long fibers are used as the discontinuous reinforcing material, the same sizing agent as that applied to the above-mentioned continuous reinforcing fibers constituting the continuous fiber-reinforced resin composite material of the present embodiment can be used.

[0129] The sizing agent (sizing agent) preferably contains a silane coupling agent, a lubricant, and a sizing agent. The types of the silane coupling agent, the lubricant, and the sizing agent may be the same as those of the sizing agent for the continuous reinforcing fibers.

[0130] From the perspective of the interfacial strength with the thermoplastic resin to be bonded, the thermoplastic resin contained in the hybrid thermoplastic resin composition used for injection molding is preferably similar to the thermoplastic resin constituting the bonding surface of the continuous fiber reinforced resin composite material, and more preferably the same material. Specifically, when polyamide 66 is used as the thermoplastic resin of the bonding surface, the resin material of the hybrid thermoplastic resin composition for injection molding is preferably polyamide 66.

[0131] Other methods include: a molding method in which a substrate is placed in a mold and compressed using a double-belt press; a method in which a mold frame is placed so as to surround the substrate and pressurized using a double-belt press for molding; a molding method in which a heating compression molding machine set at one or more temperatures and a cooling compression molding machine set at one or more temperatures are prepared, and a mold provided with the substrate is sequentially placed into the compression molding machines for molding; and the like.

[0132] (Continuous reinforcement fiber)

[0133] As the continuous reinforcing fibers, materials used in ordinary continuous fiber-reinforced resin composite materials can be used.

[0134] Examples of the continuous reinforcing fibers include, but are not limited to, glass fibers, carbon fibers, plant fibers, aramid fibers, ultra-high-strength polyethylene fibers, polybenzopyrrole fibers, liquid crystal polyester fibers, polyketone fibers, metal fibers, and ceramic fibers.

[0135] From the viewpoints of mechanical properties, thermal properties, and versatility, glass fiber, carbon fiber, plant fiber, and aramid fiber are preferred, and from the viewpoint of productivity, glass fiber is preferred.

[0136] When glass fiber is selected as continuous reinforcing fiber, a sizing agent can be used. The sizing agent (sizing agent) preferably contains a silane coupling agent, a lubricant and a bunching agent. By forming a strong bond with the resin around the continuous reinforcing fiber, a continuous fiber reinforced resin composite material with less void ratio can be obtained. When a thermoplastic resin is used as a synthetic resin, the preferred sizing agent is a sizing agent for thermoplastic resin. Regarding the sizing agent for thermoplastic resin, for example, when polyamide resin is selected as a synthetic resin, as a silane coupling agent, it is necessary to select a coupling agent that is easy to bond the carboxyl group as the terminal group of the polyamide resin to the amino group. Specifically, for example, γ-aminopropyl trimethoxysilane and epoxy silane can be cited. As a bunching agent, it is necessary to use a resin with good wettability or surface tension close to the polyamide resin. Specifically, for example, an emulsion of a polyurethane resin, an emulsion of a polyamide resin, or a modified product thereof can be selected. As a lubricant, it is necessary to use a substance that does not interfere with the silane coupling agent and the bunching agent, for example, carnauba wax can be cited.

[0137] -Silane coupling agent-

[0138] Silane coupling agents are usually used as surface treatment agents for glass fibers to help improve interfacial bonding strength.

[0139] As silane coupling agents, there can be mentioned, but not limited to, aminosilanes such as γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, etc.; mercaptosilanes such as γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane; epoxysilanes; vinylsilanes, maleic acids, etc. When polyamide is used as the synthetic resin, aminosilanes and maleic acids are preferred, and when epoxy resin is used as the synthetic resin, epoxysilanes are preferred.

[0140] - Lubricant -

[0141] Lubricants help improve the fiber opening properties of glass fibers.

[0142] As a lubricant, any conventional liquid or solid lubricating material corresponding to the purpose can be used, including but not limited to animal, plant or mineral waxes such as carnauba wax and lanolin wax; surfactants such as fatty amides, fatty acid esters, fatty acid ethers, aromatic esters, aromatic ethers, etc.

[0143] -Bundling Agents-

[0144] Bunching agents help to improve the bundling of glass fibers and enhance interfacial bonding strength.

[0145] As the bundling agent, a polymer or thermoplastic resin can be used according to the purpose.

[0146] Examples of polymers used as the bundling agent include, but are not limited to, homopolymers of acrylic acid, copolymers of acrylic acid and other copolymerizable monomers, and salts of these with primary, secondary and tertiary amines, etc. In addition, polyurethane resins synthesized from isocyanates and polyester or polyether diols, such as m-xylene diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate) and isophorone diisocyanate, are also suitable.

[0147] As the homopolymer of acrylic acid, the weight average molecular weight is preferably 1,000 to 90,000, more preferably 1,000 to 25,000.

[0148] As copolymerizable monomers constituting the copolymer of acrylic acid and other copolymerizable monomers, for example, but not limited to, one or more monomers selected from the group consisting of acrylic acid, maleic acid, methacrylic acid, vinylacetic acid, crotonic acid, methacrylic acid, fumaric acid, itaconic acid, citraconic acid and mesaconic acid among monomers having hydroxyl and / or carboxyl groups (excluding the case of only acrylic acid). As copolymerizable monomers, it is preferred to have one or more ester monomers.

[0149] Examples of salts of homopolymers and copolymers of acrylic acid with primary, secondary and tertiary amines include, but are not limited to, triethylamine salts, triethanolamine salts, glycine salts, etc. From the perspective of improving the stability of a mixed solution with other co-used chemical reagents (silane coupling agents, etc.) and reducing amine odor, the degree of neutralization is preferably 20 to 90%, more preferably 40 to 60%.

[0150] The weight average molecular weight of the acrylic acid polymer forming the salt is not particularly limited, but is preferably in the range of 3,000 to 50,000. It is preferably 3,000 or more to improve the bundling properties of the glass fibers, and is preferably 50,000 or less to improve the properties when formed into a composite molded body.

[0151] Thermoplastic resins used as bundling agents include, but are not limited to, polyolefin resins, polyamide resins, polyacetal resins, polycarbonate resins, polyester resins, polyetherketones, polyetheretherketones, polyethersulfones, polyphenylene sulfides, thermoplastic polyetherimides, thermoplastic fluorine resins, and modified thermoplastic resins obtained by modifying these resins. When the thermoplastic resin used as a bundling agent is the same thermoplastic resin and / or modified thermoplastic resin as the resin surrounding the continuous reinforcing fibers, the adhesion between the glass fibers and the thermoplastic resin is improved after the composite material is prepared, which is preferred.

[0152] In addition, in order to further improve the adhesion between the continuous reinforcing fibers and the thermoplastic resin coating the continuous reinforcing fibers and to attach the sizing agent to the glass fibers in the form of an aqueous dispersion, the thermoplastic resin used as the sizing agent is preferably a modified thermoplastic resin from the perspective of reducing the proportion of the emulsifier component or eliminating the need for an emulsifier.

[0153] Here, the modified thermoplastic resin refers to a material in which the hydrophilicity, crystallinity, thermodynamic properties, etc. are modified by copolymerizing different monomer components in addition to the monomer components that can form the main chain of the thermoplastic resin for the purpose of changing the properties of the thermoplastic resin.

[0154] Examples of the modified thermoplastic resin used as the bundling agent include, but are not limited to, modified polyolefin resins, modified polyamide resins, and modified polyester resins.

[0155] The modified polyolefin resin used as the bundling agent is a copolymer of an olefin monomer such as ethylene or propylene and a monomer copolymerizable with the olefin monomer such as an unsaturated carboxylic acid, and can be produced by a known method. It can be a random copolymer formed by copolymerizing an olefin monomer with an unsaturated carboxylic acid, or a graft copolymer formed by grafting an unsaturated carboxylic acid onto an olefin.

[0156] As the olefin monomer, for example, ethylene, propylene, 1-butene, etc. can be cited, but not limited to. They can be used alone or in combination of two or more. As the monomer that can be copolymerized with the olefin monomer, for example, acrylic acid, maleic acid, maleic anhydride, methacrylic acid, vinyl acetic acid, butyric acid, isomethacrylic acid, fumaric acid, itaconic acid, citraconic acid, unsaturated carboxylic acids such as mesaconic acid, etc. can be cited, and they can be used alone or in combination of two or more.

[0157] As the copolymerization ratio of the olefin monomer and the monomer copolymerizable with the olefin monomer, assuming that the total mass of the copolymer is 100 mass%, preferably the olefin monomer is 60 to 95 mass%, the monomer copolymerizable with the olefin monomer is 5 to 40 mass%, and more preferably the olefin monomer is 70 to 85 mass%, the monomer copolymerizable with the olefin monomer is 15 to 30 mass%. When the olefin monomer is 60 mass% or more, the affinity with the matrix is ​​good; in addition, when the mass% of the olefin monomer is 95 mass% or less, the water dispersibility of the modified polyolefin resin is good, and it is easy to uniformly impart to the continuous reinforcing fiber.

[0158] In the modified polyolefin resin used as a bundling agent, the modified groups such as carboxyl groups introduced by copolymerization can be neutralized by a basic compound. Examples of the basic compound include, but are not limited to, bases such as sodium hydroxide and potassium hydroxide; ammonia; and amines such as monoethanolamine and diethanolamine. The weight average molecular weight of the modified polyolefin resin used as a bundling agent is not particularly limited, but is preferably 5,000 to 200,000, and more preferably 50,000 to 150,000. From the perspective of improving the bundling properties of the glass fiber, it is preferably 5,000 or more, and from the perspective of emulsification stability when made into an aqueous dispersion, it is preferably 200,000 or less.

[0159] The modified polyamide resin used as the bundling agent is a modified polyamide compound having a hydrophilic group such as a polyalkylene oxide chain or a tertiary amine component introduced into the molecular chain, and can be produced by a known method.

[0160] When a polyalkylene oxide chain is introduced into the molecular chain, for example, a part or all of polyethylene glycol or polypropylene glycol is modified into diamine or dicarboxylic acid and the resulting modified product is copolymerized to produce the product. When a tertiary amine component is introduced, for example, aminoethylpiperazine, bisaminopropylpiperazine, α-dimethylaminoε-caprolactam, etc. are copolymerized to produce the product.

[0161] The modified polyester resin used as the bundling agent is a copolymer of a polycarboxylic acid or its anhydride and a polyol and has a hydrophilic group in its molecular skeleton including a terminal. The resin can be produced by a known method.

[0162] Examples of the hydrophilic group include polyalkylene oxide, sulfonate, carboxyl, neutralized salts thereof, etc. Examples of the polycarboxylic acid or its anhydride include aromatic dicarboxylic acids, aromatic dicarboxylic acids containing sulfonate, aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, trifunctional or higher polycarboxylic acids, etc.

[0163] Examples of the aromatic dicarboxylic acid include, but are not limited to, phthalic acid, terephthalic acid, isophthalic acid, phthalic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, and phthalic anhydride.

[0164] Examples of the sulfonate-containing aromatic dicarboxylic acid include, but are not limited to, sulfoterephthalate, 5-sulfoisophthalate, and 5-sulfophthalate.

[0165] Examples of the aliphatic dicarboxylic acid or alicyclic dicarboxylic acid include, but are not limited to, fumaric acid, maleic acid, itaconic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, dimer acid, 1,4-cyclohexanedicarboxylic acid, succinic anhydride, and maleic anhydride.

[0166] Examples of the trifunctional or higher polycarboxylic acid include, but are not limited to, trimellitic acid, pyromellitic acid, trimellitic anhydride, and pyromellitic dianhydride.

[0167] Among these, from the aspect of improving the heat resistance of the modified polyester resin, it is preferred that 40 to 99 mol% of the total polycarboxylic acid components are aromatic dicarboxylic acids. In addition, from the aspect of emulsification stability when the modified polyester resin is made into an aqueous dispersion, it is preferred that 1 to 10 mol% of the total polycarboxylic acid components are aromatic dicarboxylic acids containing sulfonates.

[0168] Examples of the polyol constituting the modified polyester-based resin include diols and trifunctional or higher-functional polyols.

[0169] Examples of the diol include, but are not limited to, ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, polybutylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, polytetramethylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, bisphenol A or its alkylene oxide adducts, etc. Examples of the trifunctional or higher polyol include trimethylolpropane, glycerol, pentaerythritol, etc.

[0170] As for the copolymerization ratio of the polycarboxylic acid or its anhydride and the polyol constituting the modified polyester resin, assuming that the total mass of the copolymer components is 100 mass%, preferably the polycarboxylic acid or its anhydride is 40 to 60 mass% and the polyol is 40 to 60 mass%, and more preferably the polycarboxylic acid or its anhydride is 45 to 55 mass% and the polyol is 45 to 55 mass%.

[0171] The weight average molecular weight of the modified polyester resin is preferably 3,000 to 100,000, more preferably 10,000 to 30,000. It is preferably 3,000 or more from the viewpoint of improving the bundling property of the glass fibers, and is preferably 100,000 or less from the viewpoint of emulsification stability when formed into an aqueous dispersion.

[0172] The polymer or thermoplastic resin used as the sizing agent may be used alone or in combination of two or more.

[0173] Assuming the total amount of the slinging agent is 100 mass %, at least 50 mass % and at least 60 mass % of one or more polymers selected from homopolymers of acrylic acid, copolymers of acrylic acid and other copolymerizable monomers, and salts of these with primary, secondary and tertiary amines are preferably used.

[0174] - Composition of sizing agent for glass fiber -

[0175] When glass fibers are used as continuous reinforcing fibers, the sizing agent of the glass fibers preferably contains 0.1 to 2 mass % of a silane coupling agent, 0.01 to 1 mass % of a lubricant, and 1 to 25 mass % of a sizing agent, and these components are preferably diluted with water to adjust the total mass to 100 mass %.

[0176] The amount of the silane coupling agent in the sizing agent for glass fibers is preferably 0.1 to 2% by mass, more preferably 0.1 to 1% by mass, and even more preferably 0.2 to 0.5% by mass, from the viewpoint of improving the bundling properties of the glass fibers and the interfacial bonding strength, and improving the mechanical strength of the composite molded product.

[0177] From the perspective of imparting sufficient lubricity, the amount of lubricant blended into the sizing agent for glass fibers is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and from the perspective of increasing the interfacial bonding strength and the mechanical strength of the composite molded body, the amount is preferably 1% by mass or less, more preferably 0.5% by mass or less.

[0178] From the viewpoint of controlling the bundling property of the glass fibers and improving the interfacial bonding strength and improving the mechanical strength of the composite molded body, the blending amount of the sizing agent in the sizing agent for the glass fibers is preferably 1 to 25% by mass, more preferably 3 to 15% by mass, and even more preferably 3 to 10% by mass.

[0179] -How to use the sizing agent for glass fiber-

[0180] The sizing agent for glass fiber can be prepared in any form such as an aqueous solution, a colloidal dispersion, or an emulsion using an emulsifier depending on the usage mode. From the perspective of improving the dispersion stability and heat resistance of the sizing agent, it is preferably prepared in the form of an aqueous solution.

[0181] Regarding the glass fibers serving as continuous reinforcing fibers constituting the continuous fiber-reinforced resin composite material of the present embodiment, the above-mentioned sizing agent is applied to the glass fibers using a known method such as a roll coater in a known glass fiber production process, and the produced glass fibers are dried to thereby continuously obtain the glass fibers.

[0182] The sizing agent is preferably added in an amount of 0.1 to 3 mass %, more preferably 0.2 to 2 mass %, and further preferably 0.2 to 1 mass % based on the total mass of the silane coupling agent, lubricant, and sizing agent relative to 100 mass % of the glass fiber.

[0183] From the perspective of controlling the bundling properties of the glass fibers and improving the interfacial bonding strength, the amount of the sizing agent added is preferably 0.1% by mass or more based on the total mass of the silane coupling agent, lubricant and bundling agent relative to 100% by mass of the glass fibers, and is preferably 3% by mass or less from the perspective of yarn handling properties.

[0184] It should be noted that, when carbon fibers are selected as continuous reinforcing fibers, the sizing agent preferably contains a coupling agent, a lubricant, and a bundling agent. As the coupling agent, a substance having good compatibility with the hydroxyl groups on the surface of the carbon fibers can be selected, as the bundling agent, a substance having good wettability with the selected synthetic resin or a surface tension close to that of the selected synthetic resin can be selected, and as the lubricant, a substance that does not hinder the coupling agent and the bundling agent can be selected.

[0185] When other continuous reinforcing fibers are used, the type and amount of the sizing agent used for glass fibers and carbon fibers can be appropriately selected according to the properties of the continuous reinforcing fibers, and the type and amount of the sizing agent used for carbon fibers are preferably used as a reference.

[0186] -Shape of continuous reinforcing fibers-

[0187] The continuous reinforcing fiber is a multifilament composed of a plurality of filaments, and the number of filaments is preferably 30 to 15,000 from the perspective of handling. From the perspective of strength and handling, the single filament diameter of the continuous reinforcing fiber is preferably 2 to 30 μm, more preferably 4 to 25 μm, further preferably 6 to 20 μm, and most preferably 8 to 18 μm.

[0188] From the perspective of the handling of continuous reinforcing fibers and the strength of composite materials, the single fiber diameter R (μm) and density D (g / cm 3) is preferably 5 to 100 μm·g / cm 3 , more preferably 10 to 50 μm·g / cm 3 , more preferably 15 to 45 μm·g / cm 3 , and more preferably 20 to 45 μm·g / cm 3 .

[0189] The density D can be measured using a densimeter. On the other hand, the single fiber diameter (μm) can be measured based on the density (g / cm 3 ) and fineness (dtex) and number of single yarns (roots) are calculated by the following formula.

[0190] [Number 1]

[0191]

[0192] In order to make the product RD of the continuous reinforcing fiber within a predetermined range, the fineness (dtex) and the number of filaments (roots) of the commercially available continuous reinforcing fiber can be appropriately selected according to the density of the continuous reinforcing fiber. For example, when glass fiber is used as the continuous reinforcing fiber, since the density is about 2.5 g / cm 3 , so a fiber with a single fiber diameter of 2 to 40 μm can be selected. Specifically, when the single fiber diameter of the glass fiber is 9 μm, by selecting a glass fiber with a fineness of 660 dtex and a single fiber number of 400, the product RD is 23. In addition, when the single fiber diameter of the glass fiber is 17 μm, by selecting a glass fiber with a fineness of 11,500 dtex and a single fiber number of 2,000, the product RD is 43. When carbon fiber is used as a continuous reinforcing fiber, since the density is about 1.8 g / cm 3 , so the fiber with a single fiber diameter of 2.8 to 55 μm can be selected. Specifically, when the single fiber diameter of the carbon fiber is 7 μm, by selecting a carbon fiber with a fineness of 2,000 dtex and a single fiber number of 3,000, the product RD is 13. When aramid fiber is used as a continuous reinforcing fiber, the density is about 1.45 g / cm 3 , so the fiber with a single yarn diameter of 3.4 to 68 μm can be selected. Specifically, when the single yarn diameter of the aramid fiber is 12 μm, the product RD is 17 by selecting an aramid fiber with a fineness of 1,670 dtex and a single yarn number of 1,000.

[0193] Continuous reinforcing fibers (e.g., glass fibers) are manufactured by measuring and mixing raw glass materials, making molten glass using a melting furnace, spinning the molten glass into glass fibers, applying a sizing agent, and passing through a spinning machine to produce the fibers in the form of direct untwisted roving (DWR), yarn cakes, twisted yarns, etc. The continuous reinforcing fibers may be in any form, but if they are curled into yarns, yarn cakes, or DWRs, the productivity and production stability in the process of coating with resins are improved, and therefore, they are preferred. From the perspective of productivity, DWRs are most preferred.

[0194] The form of the continuous reinforcing fibers is not particularly limited, and various forms may be mentioned, such as woven fabrics or knitted fabrics, braids, tubular products, non-crimped fabrics, unidirectional materials, etc. Among them, the continuous reinforcing fibers are preferably used in the form of woven fabrics, non-crimped fabrics, and unidirectional materials.

[0195] (Thermoplastic resin)

[0196] The thermoplastic resins constituting the continuous fiber reinforced resin composite material of this embodiment are preferably two or more. By appropriately combining two or more thermoplastic resins, the physical properties (strength, rigidity, high temperature properties, water absorption properties, impact properties, appearance, etc.) of the continuous fiber reinforced resin composite material can be adjusted.

[0197] When the two or more thermoplastic resins contained in the continuous fiber reinforced resin composite material are compatible with each other, the physical properties (strength, rigidity, high temperature properties, water absorption properties, impact properties, appearance, etc.) tend to be improved.

[0198] The state in which the thermoplastic resin is compatible means that, in a cross section perpendicular to the length direction of the continuous reinforcing fiber contained in the continuous fiber reinforced resin composite material, when the thermoplastic resin is electron-stained and observed using a scanning electron microscope (SEM), a state in which microdomains based on a plurality of thermoplastic resins are not formed. Specifically, the observation can be performed by the method described in the examples described later.

[0199] The viscosity of the thermoplastic resin is preferably 50 g / 10 min or less, more preferably 40 g / 10 min or less, from the viewpoints of strength, rigidity, moldability, and appearance.

[0200] The viscosity of the thermoplastic resin can be determined by MFR measurement (in accordance with ISO 1133), and specifically, can be observed by the method described in the examples below.

[0201] Among the two or more thermoplastic resins, from the perspective of high temperature characteristics and water absorption characteristics, the mass ratio of the resin with the largest mass ratio is preferably 5 times or less, more preferably 4 times or less, and further preferably 3 times or less of the mass ratio of the resin with the second largest mass ratio. When the mass ratio of the thermoplastic resin is within the above range, there is a tendency to improve physical properties (strength, rigidity, high temperature characteristics, water absorption characteristics, impact characteristics, appearance, etc.).

[0202] Thermoplastic resins include, but are not limited to, polyolefin resins such as polyethylene and polypropylene; polyamide resins such as polyamide 6, polyamide 66, polyamide 46, polyamide 612, and polyamide 6I; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polypropylene terephthalate; polyacetal resins such as polyoxymethylene; polycarbonate resins; polyether resins such as polyether ketone, polyether ether ketone, polyether glycol, polypropylene glycol, and polytetramethylene ether glycol; polyether sulfone; polyphenylene sulfide; thermoplastic polyetherimide; thermoplastic fluorine resins such as tetrafluoroethylene-ethylene copolymer; polyurethane resins; acrylic resins and modified thermoplastic resins thereof.

[0203] Among these thermoplastic resins, polyolefin resins, polyamide resins, polyester resins, polyether resins, polyether sulfones, polyphenylene sulfide, thermoplastic polyether imide, and thermoplastic fluorine resins are preferred. From the perspective of mechanical properties and versatility, polyolefin resins, modified polyolefin resins, polyamide resins, polyester resins, polyurethane resins, and acrylic resins are more preferred. If the thermal properties are taken into account, polyamide resins and polyester resins are further preferred. In addition, from the perspective of durability against repeated loads, polyamide resins are further preferred.

[0204] -Polyester resin-

[0205] The polyester resin refers to a polymer compound having a -CO-O- (ester) bond in the main chain.

[0206] Examples of the polyester resin include, but are not limited to, polyethylene terephthalate, polybutylene terephthalate, polybutylene terephthalate, poly-1,4-cyclohexyl dimethylene terephthalate, and polyethylene 2,6-naphthalate.

[0207] The polyester-based resin may be a homopolyester or a copolyester.

[0208] In the case of copolymerized polyester, it is preferred to appropriately copolymerize the third component with the homopolyester. Examples of the third component include, but are not limited to, diol components such as diethylene glycol, neopentyl glycol, and polyalkylene glycol, and dicarboxylic acid components such as adipic acid, sebacic acid, phthalic acid, isophthalic acid, and 5-(sodiosulfo)isophthalic acid.

[0209] In addition, polyester resins using raw materials derived from biomass may also be used, and examples thereof include, but are not limited to, aliphatic polyester resins such as polylactic acid, polybutylene succinate, and polybutylene succinate adipate, and aromatic polyester resins such as polybutylene adipate terephthalate.

[0210] -Polyamide resin-

[0211] The polyamide resin refers to a polymer compound having a -CO-NH- (amide) bond in the main chain, and examples thereof include aliphatic polyamides, aromatic polyamides, and wholly aromatic polyamides.

[0212] Examples of the polyamide resin include, but are not limited to, polyamides obtained by ring-opening polymerization of lactams, polyamides obtained by self-condensation of ω-aminocarboxylic acids, polyamides obtained by condensation of diamines and dicarboxylic acids, and copolymers thereof.

[0213] The polyamide-based resins may be used alone or as a mixture of two or more.

[0214] Examples of lactams include, but are not limited to, pyrrolidone, caprolactam, undecanolactam, and laurolactam.

[0215] Examples of ω-aminocarboxylic acids include, but are not limited to, ω-amino fatty acids, which are ring-opening compounds of lactams based on water. Lactams or ω-aminocarboxylic acids can be prepared by combining two or more monomers and condensing them.

[0216] Examples of the diamine (monomer) include, but are not limited to, linear aliphatic diamines such as hexamethylenediamine and pentamethylenediamine; branched aliphatic diamines such as 2-methylpentanediamine and 2-ethylhexamethylenediamine; aromatic diamines such as p-phenylenediamine and m-phenylenediamine; and alicyclic diamines such as cyclohexanediamine, cyclopentanediamine and cyclooctanediamine.

[0217] Examples of dicarboxylic acids (monomers) include, but are not limited to, aliphatic dicarboxylic acids such as adipic acid, pimelic acid, and sebacic acid; aromatic dicarboxylic acids such as phthalic acid and isophthalic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. The diamine and dicarboxylic acid as monomers may be used alone or in combination of two or more to be condensed.

[0218] Examples of polyamide resins include, but are not limited to, aliphatic polyamides such as polyamide 4 (poly-α-pyrrolidone), polyamide 6 (polycaprolactam), polyamide 11 (polyundecanamide), polyamide 12 (polydodecaneamide), polyamide 46 (polybutylene adipamide), polyamide 66 (polyhexamethylene adipamide), polyamide 610, and polyamide 612, semi-aromatic polyamides such as polyamide 6T (polyhexamethylene terephthalamide), polyamide 9T (polynonane terephthalamide), and polyamide 6I (polyhexamethylene isophthalamide), and copolymer polyamides containing these as constituent components.

[0219] Examples of the copolymer polyamide include, but are not limited to, copolymers of hexamethylene adipamide and hexamethylene terephthalamide, copolymers of hexamethylene adipamide and hexamethylene isophthalamide, and copolymers of hexamethylene terephthalamide and 2-methylpentamethylene terephthalamide.

[0220] When a polyamide resin is used, the thermoplastic resin preferably contains 50 to 99 parts by mass of (A) an aliphatic polyamide and 1 to 50 parts by mass of (B) a semi-aromatic polyamide containing a dicarboxylic acid unit containing at least 75 mol % of an isophthalic acid unit and a diamine unit containing at least 50 mol % of a diamine unit having 4 to 10 carbon atoms.

[0221] When the thermoplastic resin contains (A) aliphatic polyamide and (B) semi-aromatic polyamide in the above range, the physical properties (strength, rigidity, high temperature properties, water absorption properties, impact properties, appearance, etc.) of the continuous fiber reinforced resin composite material tend to be improved compared to the case where only (A) aliphatic polyamide is contained as the polyamide.

[0222] The total content of (A) aliphatic polyamide and (B) semi-aromatic polyamide is preferably 70 to 100 mass %, more preferably 80 to 100 mass %, and even more preferably 90 to 100 mass % based on 100 mass % of the thermoplastic resin.

[0223] The weight average molecular weight (Mw) of the thermoplastic resin containing (A) aliphatic polyamide and (B) semi-aromatic polyamide is preferably 15000 to 35000, more preferably 17000 to 35000, further preferably 20000 to 35000, further preferably 22000 to 34000, particularly preferably 24000 to 33000, and most preferably 25000 to 32000. When the weight average molecular weight (Mw) of the thermoplastic resin is within the above range, the strength and rigidity tend to be improved.

[0224] In addition, among the above thermoplastic resins, the weight average molecular weight Mw of the aliphatic polyamide (A) is AThe weight average molecular weight Mw of the (B) semi-aromatic polyamide is preferably B 1.5 times or more, more preferably 2 times or more. A Mw B When the ratio is 1.5 times or more, the strength and rigidity tend to be improved.

[0225] The weight average molecular weight (Mw) of the thermoplastic resin, (A) the aliphatic polyamide, and (B) the semi-aromatic polyamide can be measured by gel permeation chromatography (GPC), and specifically, can be observed by the method described in the examples below.

[0226] Examples of the aliphatic polyamide (A) include, but are not limited to, polyamide 4, polyamide 6, polyamide 11, polyamide 12, polyamide 46, polyamide 66, polyamide 610, and polyamide 612.

[0227] The content of the (A) aliphatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is preferably 50 to 99% by mass, more preferably 60 to 90% by mass, and even more preferably 70 to 80% by mass.

[0228] Examples of the (B) semi-aromatic polyamide include, but are not limited to, polyamide 6I, polyamide 9I, polyamide 10I, and the like.

[0229] The total amount of the isophthalic acid units and the diamine units having 4 to 10 carbon atoms is preferably 80 to 100 mol %, more preferably 90 to 100 mol %, and even more preferably 95 to 100 mol %, based on 100 mol % of all structural units of the (B) semiaromatic polyamide.

[0230] The ratio of the monomer units constituting the (B) semi-aromatic polyamide can be measured, for example, by 13C nuclear magnetic resonance spectroscopy (NMR).

[0231] (B) In the semi-aromatic polyamide, the ratio of isophthalic acid units in the dicarboxylic acid units is at least 75 mol%, preferably 85 mol% or more, and more preferably 90 mol% or more. When the ratio of isophthalic acid units in the dicarboxylic acid units is within the above range, high temperature properties and water absorption properties tend to be improved.

[0232] (B) In the semi-aromatic polyamide, the ratio of the diamine unit having 4 to 10 carbon atoms in the diamine unit is at least 50 mol%, preferably 60 mol% or more, more preferably 70 mol% or more. When the ratio of the diamine unit having 4 to 10 carbon atoms in the diamine unit is within the above range, the high temperature characteristics and water absorption characteristics tend to be improved.

[0233] The content of the (B) semi-aromatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is preferably 1 to 50% by mass, more preferably 10 to 40% by mass, and even more preferably 20 to 30% by mass.

[0234] The above-mentioned (A) aliphatic polyamide and (B) semi-aromatic polyamide may be capped with a known capping agent, and the total amount of the capped terminals of (A) aliphatic polyamide and (B) semi-aromatic polyamide expressed as an equivalent relative to 1 g of the total polyamide of (A) aliphatic polyamide and (B) semi-aromatic polyamide is preferably 5 to 180 micro equivalents / g, more preferably 10 to 170 micro equivalents / g, further preferably 20 to 160 micro equivalents / g, particularly preferably 30 to 140 micro equivalents / g, and most preferably 40 to 140 micro equivalents / g. When the amount of the capped terminals is within the above range, there is a tendency for physical properties (strength, rigidity, high temperature properties, water absorption properties, impact properties, appearance, etc.) to be improved.

[0235] Here, the amount of blocked terminals refers to the total amount of amino terminals and carboxyl terminals blocked by the blocking agent. 1 H-NMR can be measured, and specifically, it can be measured by the method described in the examples described later.

[0236] The terminal group concentration of the aliphatic polyamide (A) is preferably 1 / 2 or less, and more preferably 2 / 5 or less of the terminal group concentration of the semi-aromatic polyamide (B). When the terminal group concentration of the aliphatic polyamide (A) is 1 / 2 or less of the terminal group concentration of the semi-aromatic polyamide (B), the physical properties (strength, rigidity, high temperature properties, water absorption properties, impact properties, appearance, etc.) tend to be improved.

[0237] The terminal group concentrations of (A) aliphatic polyamide and (B) semi-aromatic polyamide can be calculated using 1 H-NMR can be measured, and specifically, it can be measured by the method described in the examples described later.

[0238] The difference in tan δ peak temperature between the aliphatic polyamide (A) and the semi-aromatic polyamide (B) is preferably 45 to 100° C., more preferably 50 to 90° C., and even more preferably 60 to 90° C. When the difference in tan δ peak temperature between the aliphatic polyamide (A) and the semi-aromatic polyamide (B) is within the above range, high temperature properties and water absorption properties tend to be improved.

[0239] The tan δ peak temperature of (A) aliphatic polyamide and (B) semi-aromatic polyamide can be measured, for example, using a viscoelasticity analysis device, and specifically, can be measured by the method described in Examples below.

[0240] From the viewpoints of strength, rigidity, moldability and appearance, the difference in viscosity between the (A) aliphatic polyamide and the (B) semi-aromatic polyamide is preferably 3 times or more, more preferably 4 times or more.

[0241] The viscosity of the thermoplastic resin can be determined by MFR measurement (in accordance with ISO 1133), and specifically, can be observed by the method described in Examples below.

[0242] (Colorant)

[0243] The thermoplastic resin may contain a colorant.

[0244] Examples of the colorant include carbon black, nigrosine, aluminum pigment, titanium dioxide, ultramarine, cyanine blue, cyanine green, quinacridone, diatomaceous earth, monoazo salts, perylene, diazo, condensed azo, isoindoline, red iron oxide, nickel titanium yellow, diketopyrrolopyrrole, metal salts, perylene red, metal oxides, bismuth vanadate, cobalt green, cobalt blue, anthraquinone, phthalocyanine green, phthalocyanine blue, etc. Among them, black colorants are preferred, and carbon black and nigrosine are more preferred.

[0245] (Application of continuous fiber reinforced resin composite materials)

[0246] The continuous fiber-reinforced resin composite material of the present embodiment can be suitably used as a structural material for aircraft, vehicles, construction materials, robots, and the like.

[0247] In vehicle applications, it can be used for, but not limited to, chassis / frame, undercarriage, drive system components, interior components, exterior components, functional components, and other components.

[0248] Specifically, the present invention can be suitably used as the following parts: steering shaft, bracket, sunroof, pedal, roof trim, door trim, trunk, trunk lid, hood, seat frame, seat back, seat belt retractor, seat belt retractor support frame, clutch, gear, pulley, cam, AG shaft, elastic beam, buffer, lamp, reflector, glass window, front module, rear door inner panel, brake pedal, steering wheel, electrical equipment material, sound absorbing material, door exterior, interior panel, instrument panel, tailgate, top beam, seat, seat frame, wiper link, EPS (Electric Power Steering), small motor, radiator, ECU (Engine Control Unit) box, ECU cover, steering gear box cover, plastic cover, EV (Electric Vehicle, Electric Vehicle) motor frame, wiring group, on-board instrument, combination switch, small motor, spring, shock absorber, wheel, rim cover, frame, subframe, side frame, two-wheeled vehicle frame, fuel tank, oil pan, intake manifold, drive shaft, drive motor, single cabin, hydrogen tank, fuel cell electrode, panel, floor panel, outer panel, door, cabin, roof, hood, steam valve, EGR (exhaust gas recirculation,Exhaust Gas Recirculation) valve, variable valve timing unit, connecting rod, cylinder bore, beams (engine foot, front floor crossbeam, footrest crossbeam, seat crossbeam, inner side beam, rear crossbeam, suspension beam, pillar reinforcement beam, front side beam, front plate beam, upper plate beam, front panel crossbeam, steering column), tunnel, locking insert, gearbox, gearshift rail, bridge housing, roof rail, upper body, side rail, trim, door surround assembly, airbag parts, pillar, front panel to pillar support, suspension tower, bumper, body lower pillar, front pillar, reinforcement (instrument panel, rail, roof, front pillar, roof rail, roof side rail, storage box, door waistline, front floor lower layer, front body upper pillar, front body lower pillar, center pillar, center pillar hinge, door outer panel), side outer panel, front door window frame, MICS (Minimum Intrusion Cabin System components, torque box, radiator support, radiator fan, water pump, fuel pump, electronic control throttle body, engine control ECU, starter, alternator, manifold, gearbox, clutch, dash panel, dash panel insulation pad, door side impact beam, bumper beam, door beam, partition, outer pad, inner pad, rear seat bar, door panel, door trim subassembly, energy absorber (bumper, shock absorber), shock absorber, shock absorber trim, pillar trim, roof inner trim, resin rib, side rail front spacer, side rail rear spacer, seat belt pretensioner, airbag sensor , arms (suspension, lower arms, hood hinges), suspension links, shock absorber brackets, fender brackets, inverter brackets, inverter modules, hood inner panels, hood panels, cowl vents, cowl top outer front panels, cowl top outer panels, floor silencers, shock absorber seats, hood insulation, fender side panel protection, cowl insulation, cowl top vents, cylinder head cover, tire deflectors, fender support frames, engine room tie rods, center channels, floor channels, radiator center support frames, trunk trim, trunk floor, accelerator pedal, accelerator pedal base and other parts.

[0249] [Molding of composite materials]

[0250] The continuous fiber reinforced resin composite material of the present embodiment can be further molded. As the above method, for example, a method of cutting the continuous fiber reinforced resin composite material of the present embodiment into a predetermined size, heating it with an infrared heater, and heating and compressing it with a press molding machine can be cited.

[0251] [Continuous fiber reinforced resin molded body]

[0252] The continuous fiber reinforced resin molded body of the present embodiment is a continuous fiber reinforced resin molded body comprising continuous reinforcing fibers and a thermoplastic resin, and is characterized in that the peak temperature of tanδ at the interface between the continuous reinforcing fibers and the thermoplastic resin of the above-mentioned continuous fiber reinforced resin composite molded body is above 80°C, the interface strength of the above-mentioned continuous fiber reinforced resin molded body based on the ejection test is 1.58 to 5.00 mN / μm, and the continuous fiber reinforced resin molded body has a plate-like, frame-like, box-like or a combination thereof.

[0253] The continuous reinforcing fibers contained in the continuous fiber-reinforced resin molded product of the present embodiment may be the same as the continuous reinforcing fibers contained in the above-mentioned continuous fiber-reinforced resin composite material.

[0254] The thermoplastic resin contained in the continuous fiber-reinforced resin molded product of the present embodiment may be the same as the thermoplastic resin contained in the above-mentioned continuous fiber-reinforced resin composite material.

[0255] In the continuous fiber reinforced resin molded body of the present embodiment, the peak temperature of tan δ, which is defined in the same manner as the peak temperature of tan δ of the above-mentioned continuous fiber reinforced resin composite material, is 80° C. or more, preferably 85° C. or more, more preferably 90° C. or more, and further preferably 100° C. or more. When the peak temperature of tan δ is within the above range, there is a tendency for the strength, rigidity, water absorption characteristics, impact characteristics, and high temperature characteristics to be improved.

[0256] As a method for adjusting the peak temperature of tan δ of the continuous fiber reinforced resin molded body to the above range, for example, a method of adjusting the aromatic ring concentration in the resin and adjusting the static wettability can be cited. If the aromatic ring concentration in the resin is increased and the contact angle based on the static wettability test is reduced, there is a tendency for the peak temperature of tan δ to increase.

[0257] The peak temperature of tan δ of the continuous fiber reinforced resin molded body can be obtained, for example, by performing nanoindentation (nanoDMA) measurement on a single continuous reinforcing fiber in a cross section perpendicular to the longitudinal direction of the continuous reinforcing fibers contained in the continuous fiber reinforced resin molded body using a nanoindenter and applying vibration of a specific frequency. Specifically, it can be measured by the method described in the examples described later.

[0258] The interface strength of the continuous fiber reinforced resin molded body of the present embodiment (interface strength between the matrix resin of the continuous fiber reinforced resin molded body and the reinforcing fiber) is 1.58 mN / μm or more, preferably 1.65 mN / μm or more, more preferably 1.75 mN / μm or more, and further preferably 1.85 mN / μm or more. In addition, the interface strength is 5.00 mN / μm or less, preferably 4.50 mN / μm or less, and more preferably 3.50 mN / μm or less. When the interface strength is within the above range, there is a tendency to improve strength, rigidity, water absorption characteristics, impact characteristics, and high temperature characteristics.

[0259] The interfacial strength of the continuous fiber reinforced resin molded body can be determined, for example, by performing a push-out test using a nanoindenter on a single continuous reinforcing fiber in a cross section perpendicular to the longitudinal direction of the continuous reinforcing fibers contained in the continuous fiber reinforced resin molded body. Specifically, it can be measured by the method described in the examples described below.

[0260] As a method for adjusting the interface strength of the continuous fiber reinforced resin molded body based on the ejection test to the above range, for example, a method of adjusting the dynamic wettability and static wettability of the thermoplastic resin and the continuous reinforcing fibers can be cited. If the dynamic wettability is reduced and the contact angle based on the static wettability test is reduced, there is a tendency for the interface strength to increase.

[0261] The continuous fiber-reinforced resin molded product of the present embodiment has a plate-like, frame-like, box-like, or a combination thereof shape in appearance.

[0262] The plate shape is not particularly limited, and for example, the shape under plane observation can be a polygon such as a quadrilateral, pentagon, hexagon, a circle, a semicircle, an ellipse, etc. In addition, the plate shape can be a curved strip, such as an L-shape, a V-shape, a U-shape, etc. In the case of a curved strip, the shape of the cross section in the thickness direction is not particularly limited, and for example, it can be a polygon such as a quadrilateral, pentagon, hexagon, a circle, a semicircle, an ellipse, etc.

[0263] It should be noted that the corners and curved portions of the polygon may be rounded. In addition, the polygon may have a flat plate portion and / or a curved portion partially.

[0264] The frame shape is a shape that is formed in a manner that surrounds a space in the central portion when viewed from above. The shape formed in a manner that surrounds the space may be in a completely closed state or in a partially disconnected state. The outer peripheral shape and the inner peripheral shape based on the top view are not particularly limited, and examples thereof include polygons such as quadrilaterals, pentagons, and hexagons, circles, semicircles, ellipses, etc., and the outer peripheral shape and the inner peripheral shape may be the same shape (similar figures, etc.) or different.

[0265] It should be noted that the corners of the polygon may be rounded. In addition, the polygon may have a flat plate portion and / or a curved portion in part.

[0266] The box shape is not particularly limited, and for example, a polygonal shape such as a quadrilateral, a pentagon, a hexagon, a circle, a semicircle, an ellipse, etc., can be cited in the top view. In addition, one face can be open. Each face can be of the same shape or different shapes.

[0267] It should be noted that the corners of the polygon may be rounded. In addition, the polygon may have a flat plate portion and / or a curved portion in part.

[0268] It should be noted that the overall shape of the continuous fiber reinforced resin molded body of the present embodiment can be the above-mentioned plate-like, frame-like, box-like, or a combination thereof when observed from the outside. Therefore, any shape can have concave-convex shapes including ribs, protrusions, grooves, through holes, etc. on each surface, and the edge can be not only straight, but also curved, or in a state with a cut, etc.

[0269] [Manufacture of continuous fiber reinforced resin molded body]

[0270] The continuous fiber reinforced resin molded body of the present embodiment can be produced by, for example, cutting a continuous fiber reinforced resin composite material including continuous reinforcing fibers and a thermoplastic resin into a predetermined size, heating the composite material with an infrared heater, and heating and compressing the composite material with a press molding machine.

[0271] [Application of continuous fiber reinforced resin molded body]

[0272] The continuous fiber-reinforced resin molded product of the present embodiment can be suitably used for structural material applications such as aircraft, vehicles, construction materials, robots, railways, and generators.

[0273] In vehicle applications, the composite material can be used for, but not limited to, chassis / frame, underframe, drive system parts, interior parts, exterior parts, functional parts, and other parts. Specifically, the same applications as those of the continuous fiber reinforced resin composite material can be cited.

[0274] Example

[0275] The present invention will be described in more detail below with reference to Examples and Comparative Examples. However, the present invention is not limited to these Examples and can be implemented with various modifications within the scope of the gist of the present invention.

[0276] First, the measurement methods and the like used in Examples and Comparative Examples will be described.

[0277] [Weight average molecular weight]

[0278] The weight average molecular weight (Mw) of the thermoplastic resin contained in the continuous fiber reinforced resin composite material was measured by GPC (gel permeation chromatography, HLC-8020; Tosoh Corporation) using hexafluoroisopropanol solvent and polymethyl methacrylate molecular weight conversion standard sample (Polymer Laboratories). It should be noted that TSK-GEL, GMHHR-M and G1000HHR were used as GPC columns.

[0279] When the thermoplastic resin contains (A) aliphatic polyamide and (B) semi-aromatic polyamide, the weight average molecular weight Mw of (A) aliphatic polyamide is A and (B) the semi-aromatic polyamide, each having a weight average molecular weight Mw B The ratio (Mw A / Mw B ).

[0280] [Dynamic wettability]

[0281] Using a solder wettability tester (Rehsca), a single continuous reinforcing fiber was immersed in a thermoplastic resin heated to a temperature 20°C higher than the melting point at an immersion speed of 1.0 mm / sec and an immersion depth of 0.5 mm, and the time (wetting time) (sec) from the time when the load took a negative maximum value to the time when the load reached 0 was measured. The shorter this time, the better the dynamic wettability was evaluated to be.

[0282] In addition, when the continuous fiber-reinforced resin composite material includes two or more thermoplastic resins, the maximum value (sec) of the difference in dynamic wettability between the thermoplastic resins is also determined.

[0283] [Static wettability]

[0284] The thermoplastic resin film and one reinforcing fiber were sandwiched between a cover glass, heated to 280°C at 100°C / min on a hot plate, left for 5 minutes, and then cooled at 50°C / min. The angle (contact angle) (°) formed between the reinforcing fiber surface and the thermoplastic resin at room temperature was measured by observation using an optical microscope. The smaller the angle, the better the static wettability.

[0285] [Amount of closed ends]

[0286] The amount of blocked terminals of the polyamide contained in the continuous fiber-reinforced resin composite material (micro equivalent / g) was determined by 1H-NMR measurement using JEOL-ECZ500 (JEOL Ltd.).

[0287] [Peak temperature of tanδ]

[0288] The continuous fiber reinforced resin composite material and the continuous fiber reinforced resin molded body were ground in a manner to obtain a cross section orthogonal to the continuous reinforcing fiber, and test pieces with a length of 1 cm, a width of 0.2 cm, and a thickness of 60 μm were prepared. The cross section of the obtained test piece was used as the measurement surface, and for a single continuous reinforcing fiber in the cross section, a nanoindenter (TI980, Bruker) was used to perform a nanoDMA test at a frequency of 10 Hz and a 10°C interval in a temperature range of 30°C to 150°C to obtain the peak temperature (°C) of tanδ at the interface between the continuous reinforcing fiber and the thermoplastic resin.

[0289] [Raman Peak]

[0290] A cross section in the thickness direction (a cross section perpendicular to the length direction of the continuous reinforcing fibers) of the continuous fiber-reinforced resin composite material was cut out at any five locations, embedded in epoxy resin, and carefully ground so as not to damage the continuous reinforcing fibers.

[0291] A mapping image of the cross section is captured using a laser Raman microscope (inViaQontor confocal Raman microscope; Renishaw Co., Ltd.), and the type of resin contained in the continuous fiber-reinforced resin composite material is determined from the obtained image and spectrum.

[0292] In addition, the peak of the Raman spectrum of the resin region of the cross section (cm -1 ).

[0293] [Compatibility of thermoplastic resins]

[0294] The cross section of the continuous fiber reinforced resin composite material was mapped at a resolution of 1 μm using the method described in the above [Raman measurement]. In addition, the cross section of the continuous fiber reinforced resin composite material was ground and immersed in a 5wt% aqueous solution of 12-tungsten (VI) phosphoric acid n-hydrate for 18 hours. After the resin was electron-stained, it was observed using a scanning electron microscope (SEM). The situation where micro-regions based on multiple thermoplastic resins were not formed was judged as 0 (compatible), and the situation where micro-regions were formed was judged as × (incompatible).

[0295] [X-ray diffraction peak intensity ratio]

[0296] The measurement was performed in the atmosphere using an X-ray diffraction apparatus (SmartLab, Rigaku Co., Ltd.) under the following conditions: X-ray source: CuKα, optical system: focusing method, output: 45 kV×200 mA, detector: D / tex Ultra.

[0297] The ratio of the peak intensity I(0,1,0) of the (0,1,0) plane to the peak intensity I(1,0,0) of the (1,0,0) plane (I(0,1,0) / I(1,0,0)) and the presence or absence of the peak of the (1,1,0) plane were determined.

[0298] [Interface strength]

[0299] The continuous fiber reinforced resin composite material and the continuous fiber reinforced resin molded body were cut in a manner that the cross section in the thickness direction (cross section orthogonal to the length direction of the continuous reinforcing fiber) was exposed, and the continuous reinforcing fiber was carefully polished in a manner that the continuous reinforcing fiber would not be damaged to obtain a test piece with a thickness of 60 μm. The cross section of the test piece was used as the measurement surface, and a single continuous reinforcing fiber in the cross section was tested using a nanoindenter (TI Premier, Bruker) to measure the interfacial strength (mN / μm) of the continuous fiber composite material.

[0300] [Carboxyl terminal group concentration of continuous fiber reinforced resin composites]

[0301] Using JEOL-ECZ500 (JEOL Ltd.), 1 The amount of carboxyl terminal groups (μmol / g) of the thermoplastic resin contained in the continuous fiber-reinforced resin composite material was determined by H-NMR measurement.

[0302] [Polishing pressure and reinforcing fiber diameter at which interface peeling occurs]

[0303] The continuous fiber reinforced resin composite material was cut by a band saw to expose the cross section in the thickness direction of the continuous fiber reinforced resin (a cross section orthogonal to the length direction of the continuous reinforcing fiber), and the cut test piece was ground by a grinder (small precision sample making system IS-POLISHER ISPP-1000 (Ikegami Seiki Co., Ltd.)) with the grinding pressure changed to 0.078 MPa, 0.167 MPa, 0.245 MPa, and 0.382 MPa. The grinding was carried out in the following order: 10 minutes with #2000 water-resistant sandpaper, 5 minutes with a silicon carbide film with a particle size of 9 μm, 5 minutes with an aluminum oxide film with a particle size of 5 μm, 5 minutes with an aluminum oxide film with a particle size of 3 μm, 5 minutes with an aluminum oxide film with a particle size of 1 μm, and 5 minutes with colloidal silica (Baikalox 0.1CR) with a particle size of 0.1 μm using a foamed polyurethane using a polishing paper, and grinding was carried out while adding water at about 7 mL / min during each grinding. The polished sample was observed using SEM (S-4700, Hitachi High-Technologies Corporation), and the pressure at which a void was generated at the extreme interface between one continuous reinforcing fiber and the thermoplastic resin in a cross section perpendicular to the longitudinal direction of the continuous reinforcing fiber was taken as the polishing pressure (MPa) at which interface delamination occurred.

[0304] In the SEM observation, the diameters of 10 continuous reinforcing fibers were measured from the substantially circular cross section of the continuous reinforcing fibers in a cross section perpendicular to the longitudinal direction of the continuous reinforcing fibers, and the average value was defined as the reinforcing fiber diameter (μm).

[0305] [Reinforcement fiber density]

[0306] The thermoplastic resin of the continuous fiber reinforced resin composite material was burned out in an electric furnace, and the reinforcing fiber density (g / cm 3 ).

[0307] [Interface constant]

[0308] For the continuous fiber reinforced resin composite material, the interface constant was calculated by the following formula from the obtained carboxyl terminal group concentration, the grinding pressure at which interface peeling occurred, the reinforcing fiber diameter, and the reinforcing fiber density.

[0309] (Interface constant) = (concentration of carboxyl terminal groups in continuous fiber-reinforced resin composite material [μmol / g]) × (grinding pressure at which interface peeling occurs [MPa]) × (reinforcement fiber diameter [μm]) / (reinforcement fiber density [g / cm 3 ]) 2

[0310] [Tensile stress]

[0311] A strip test piece with a length of 70 mm, a width of 10 mm, and a thickness of 2 mm was cut from the continuous fiber reinforced resin composite material. The test piece was clamped at intervals of 30 mm along the length direction using an INSTRON universal testing machine, and the tensile stress (MPa) was measured at a speed of 5 mm / min under an environment of 23°C and 50% RH and an environment of 80°C and 50% RH.

[0312] The tensile stress retention rate (%) at 80°C was calculated by the following formula.

[0313] Tensile stress retention at 80°C = (tensile stress at 80°C, 50% RH / tensile stress at 23°C, 50% RH) × 100

[0314] [Bending stress, bending modulus]

[0315] A strip test piece with a length of 100 mm, a width of 10 mm, and a thickness of 2 mm was cut out from the continuous fiber reinforced resin composite material. The span was set to 32 mm using a three-point bending fixture using an INSTRON universal testing machine. The bending stress (MPa) and bending modulus (GPa) were measured at a speed of 1 mm / min in an environment of 23°C and 50% RH and in an environment of 80°C and 50% RH, respectively.

[0316] The flexural stress retention rate (%) and flexural modulus retention rate (%) at 80° C. were determined by the following formulae.

[0317] Bending stress retention at 80°C = (bending stress at 80°C, 50% RH / bending stress at 23°C, 50% RH) × 100

[0318] Flexural modulus retention at 80°C = (flexural modulus at 80°C, 50% RH / flexural modulus at 23°C, 50% RH) × 100

[0319] [Water absorption characteristics]

[0320] A strip test piece with a length of 100 mm, a width of 10 mm, and a thickness of 2 mm was cut out from the continuous fiber reinforced resin composite material, immersed in a constant temperature water bath at 80°C for 18 hours, and then placed in a constant temperature and humidity bath at 80°C and 57% RH for more than 150 hours to adjust the humidity until the mass becomes constant, and used as a sample when water is absorbed. The tensile stress (MPa), flexural stress (MPa), and flexural modulus (GPa) were measured under an environment of 80°C and 50% RH by the methods described in the above [Tensile stress] measurement and [Flexural stress, flexural modulus] measurement.

[0321] The tensile stress retention rate (%), the bending stress retention rate (%), and the bending modulus retention rate (%) during water absorption were determined by the following formulae.

[0322] Tensile stress retention rate during water absorption = (tensile stress during water absorption / tensile stress at 23°C, 50% RH) × 100 Bending stress retention rate during water absorption = (bending stress during water absorption / bending stress at 23°C, 50% RH) × 100

[0323] Flexural modulus retention rate when absorbing water = (flexural modulus when absorbing water / flexural modulus at 23°C, 50% RH) × 100

[0324] [Impact Strength]

[0325] A test piece of 60 mm in length, 60 mm in width and 2 mm in thickness was cut out from the continuous fiber reinforced resin composite material, and the test was conducted using a high-speed impact tester (Shimadzu HYDRO SHOT HITS-P10, Shimadzu Corporation) in accordance with JIS K7211-2; 2006 under the conditions of a striker diameter of 20 mmФ, a placement diameter of 40 mmФ, a test speed of 4.4 m / sec, a test temperature of 23°C, and a test number of n = 5. A graph of the test force versus displacement was plotted, and the maximum impact strength (kN) obtained from the graph was divided by the thickness of the test piece, and the impact strength was obtained as the average value (kN / mm) of 5 samples.

[0326] [Appearance of the material]

[0327] The surface appearance of the continuous fiber reinforced resin composite material was observed, and the case where the surface was not rough and the surface was glossy was evaluated as 0 (excellent), the case where the surface was not rough and the surface was matte was evaluated as △ (good), and the case where the surface was rough was evaluated as × (poor).

[0328] The materials used in Examples and Comparative Examples are as follows.

[0329] [Continuous reinforcing fiber]

[0330] (Fiberglass)

[0331] ER1200T-423 (Nippon Electric Glass Co., Ltd.)

[0332] (Carbon Fiber)

[0333] Torayca T300 (Toray Corporation)

[0334] [Fiber cloth]

[0335] The glass fiber or carbon fiber cloth was woven using a rapier loom (weaving width 1m) using the above glass fiber or carbon fiber as warp and weft to produce glass cloth or carbon fiber cloth. The woven form of the obtained glass cloth was plain weave, the weaving density was 6.5 strands / 25mm, and the basis weight was 600g / m 2In addition, the weaving form of the obtained carbon fiber cloth is plain weave, the weaving density is 6.5 strands / 25mm, and the basis weight is 425g / m 2 .

[0336] [Thermoplastic resin]

[0337] Resin 1: Polyamide 66 (Leona 1300S (Asahi Kasei Corporation)) (weight average molecular weight (Mw): 45,000, viscosity: 25 g / 10 min, terminal group concentration: 100 μmol / g, tanδ peak temperature: 50°C)

[0338] Resin 2: Polyamide 6I (weight average molecular weight (Mw): 20,000, viscosity: 35 g / 10 min, terminal group concentration: 260 μmol / g, tanδ peak temperature: 130°C)

[0339] Resin 3: Polyamide 6 (weight average molecular weight (Mw): 31000, viscosity: 97 g / 10 min, terminal group concentration: 90 μmol / g, tanδ peak temperature: 50°C)

[0340] Resin 4: Polypropylene (viscosity: 20g / 10min)

[0341] Resin 5: Polyamide 66 (Leona 1500 (Asahi Kasei Corporation)) (weight average molecular weight (Mw): 70,000, viscosity: 2 g / 10 min, terminal group concentration: 70 μmol / g, tan δ peak temperature: 50° C.)

[0342] Resin 6: Polyamide 66 (Leona 1300 (Asahi Kasei Corporation)) (weight average molecular weight (Mw): 45,000, viscosity: 25 g / 10 min, terminal group concentration: 100 μmol / g, tan δ peak temperature: 50° C.)

[0343] Resin 7: Polyamide 66 (Leona 1402S (Asahi Kasei Corporation)) (weight average molecular weight (Mw): 45,000, viscosity: 25 g / 10 min, terminal group concentration: 100 μmol / g, tanδ peak temperature: 50° C.)

[0344] Resin 8: Polyamide 6 / 12 (Grilon C CF6S (EMS Chemie Japan Co., Ltd.) (weight average molecular weight (Mw): 20,000, viscosity: 34 g / 10 min, terminal group concentration: 80 μmol / g, tan δ peak temperature: 50° C.)

[0345] In addition, the viscosity of the thermoplastic resin, the terminal group concentration of the polyamide, and the peak temperature of tan δ were respectively determined by the following methods.

[0346] Resin 9: Polyamide 6T (weight average molecular weight (Mw): 31000, viscosity: 30 g / 10 min, terminal group concentration: 120 μmol / g, tanδ peak temperature: 125°C)

[0347] Resin 10: polyamide MXD6 (weight average molecular weight (Mw): 29000, viscosity: 28 g / 10 min, terminal group concentration: 160 μmol / g, tanδ peak temperature: 75°C)

[0348] Resin 11: Polyamide 6T / 6I (weight average molecular weight (Mw): 27,000, viscosity: 27 g / 10 min, terminal group concentration: 160 μmol / g, tanδ peak temperature: 125°C)

[0349] Resin 12: 75 parts by mass of polyetheretherketone resin (Victrex, PEEK90G), 25 parts by mass of polyetherimide resin (Sabic, UTM1010), 20 parts by mass of cyclic polyarylene sulfide (produced according to International Publication No. 2020 / 017287), and 5 parts by mass of linear polyarylene sulfide (produced according to International Publication No. 2020 / 017287) were dry-blended and mixed using a mixing bowl. The TEX30a twin-screw extruder (screw diameter 30mm, L / D=45, kneading section 5 positions, fully meshing screws rotating in the same direction) manufactured by Nippon Steel Works, Ltd. with a vacuum exhaust port was used. The barrel temperature was set at a screw speed of 300rpm and a discharge rate of 20kg / hr, so that the resin temperature leaving the die was the melting point of the resin composition + 20°C, and melt kneading was performed, and pellets were formed using a strand pelletizer. Tg=154°C

[0350] Resin 13: A polyamide 9T (PA9T) resin composition was obtained as follows. 790 g of 1,9-nonanediamine, 790 g of 2-methyl-1,8-octanediamine, 1639 g of terephthalic acid (1,9-nonanediamine: 2-methyl-1,8-octanediamine: terephthalic acid = 50:50:98 (molar ratio)), 48.8 g of benzoic acid, 3.3 g of sodium hypophosphite, and 1100 g of water were charged into a reaction apparatus and replaced with nitrogen. The internal temperature was raised to 200°C over 2 hours. At this time, the pressure of the reaction apparatus was raised to 2 MPa. Thereafter, the water vapor was slowly discharged, and the reaction was carried out for 2 hours while the pressure was maintained at 2 MPa. Next, the pressure was reduced to 1.2 MPa over 30 minutes to obtain a prepolymer. The prepolymer was crushed and dried at 120°C under reduced pressure for 12 hours. This was subjected to solid phase polymerization at 230° C. and 13.3 Pa for 10 hours to obtain PA9T.

[0351] After the PA9T was dried at 120°C for 24 hours under reduced pressure, 0.3 parts by mass of SUMILIZERGA-80 (manufactured by Sumitomo Chemical Co., Ltd.) and 0.2 parts by mass of LicoWax-OP (manufactured by Clariant Chemicals Co., Ltd.) as a phenolic heat stabilizer were dry-blended with respect to 100 parts by mass of PA9T, and the obtained mixture was fed from the feed hopper of a twin-screw extruder (screw diameter: 30 mm, L / D=28, barrel temperature 300°C, rotation speed 150 rpm), melt-kneaded, extruded into strands, and cut by a pelletizer to obtain a pelletized PA9T resin composition. Tg=136°C

[0352] (Viscosity of thermoplastic resin)

[0353] The viscosity of the thermoplastic resin was measured using a tabletop melt flow index tester (L260, Tateyama Akagaku High-Technologies Co., Ltd.) in accordance with ISO1133 at 270°C and a load of 2.16 kg for polyamide and at 270°C and a load of 2.16 kg for polypropylene.

[0354] (Terminal group concentration of polyamide)

[0355] Regarding the terminal group concentration of the polyamide, the amino terminal group concentration and the carboxyl terminal group concentration were measured as follows, respectively, and the total concentration was determined.

[0356] Measurement of carboxyl terminal group concentration and amino terminal group concentration: 1H-NMR measurement was performed using JEOL-ECZ500, and the concentration was determined from the peak area, molecular weight, and proton number.

[0357] (Peak temperature of tanδ of polyamide)

[0358] The peak temperature of tan δ of the polyamide was determined using a nanoindenter (TI Premier, Bruker Corporation) at a frequency of 10 Hz and a heating rate of 10° C. / min using a test piece having a thickness of 0.1 mm.

[0359] [Method for producing thermoplastic resin film]

[0360] The thermoplastic resin film was obtained by molding using a T-die extruder (manufactured by Soken Co., Ltd.) The film thickness was 200 μm.

[0361] [Example 1]

[0362] Resin 1 and resin 2 were dry-mixed at a mass ratio of resin 1:resin 2=7:3, and a thermoplastic resin film 1 was obtained by the above method.

[0363] Five sheets of glass cloth and six sheets of thermoplastic resin film 1 were alternately stacked and molded so that the thermoplastic resin film 1 became the surface, thereby obtaining a continuous fiber-reinforced resin composite material.

[0364] A double belt press was used as the molding machine. The glass cloth and the thermoplastic resin film 1 were stacked as above and placed in the molding machine. The temperature inside the molding machine was heated to 330° C. and compression molding was performed under the conditions of a pressure of 3 MPa and a belt speed of 0.5 m / min.

[0365] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0366] The obtained continuous fiber reinforced resin composite material is further cut into a size of 300mm×300mm×2mm, heated to 300°C using an infrared heater, and then placed in a press molding machine for pressing, thereby obtaining a plate-shaped continuous fiber reinforced resin molded body (300mm×300mm×2mm).

[0367] [Example 2]

[0368] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that only Resin 2 was used as the thermoplastic resin.

[0369] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, a thermoplastic resin was confirmed by Raman measurement.

[0370] [Example 3]

[0371] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 3 and the resin 2 were dry-blended at a mass ratio of resin 3:resin 2=7:3.

[0372] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0373] [Example 4]

[0374] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that resin 4 and resin 2 were dry-blended at a mass ratio of resin 4:resin 2=7:3.

[0375] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0376] [Example 5]

[0377] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 1 and the resin 2 were dry-blended at a mass ratio of resin 1:resin 2=95:5.

[0378] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0379] [Example 6]

[0380] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 1 and the resin 2 were dry-blended at a mass ratio of resin 1:resin 2=88:12.

[0381] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0382] [Example 7]

[0383] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that glass fibers aligned in one direction (GFUD) were used instead of the glass cloth.

[0384] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0385] [Example 8]

[0386] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that a 2×2 twill woven glass cloth was used as the glass cloth.

[0387] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0388] [Example 9]

[0389] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that carbon fibers were used as the continuous reinforcing fibers.

[0390] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0391] [Example 10]

[0392] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 5 and the resin 2 were dry-blended at a ratio of resin 5:resin 2=7:3.

[0393] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0394] [Example 11]

[0395] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 6 and the resin 2 were dry-blended at a ratio of resin 6:resin 2=7:3.

[0396] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0397] [Example 12]

[0398] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that resin 7 and resin 2 were dry-blended at a ratio of resin 7:resin 2=7:3.

[0399] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0400] [Example 13]

[0401] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that only Resin 9 was used as the thermoplastic resin.

[0402] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, a thermoplastic resin was confirmed by Raman measurement.

[0403] [Example 14]

[0404] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that only the resin 10 was used as the thermoplastic resin.

[0405] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, a thermoplastic resin was confirmed by Raman measurement.

[0406] [Example 15]

[0407] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that only the resin 11 was used as the thermoplastic resin.

[0408] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, a thermoplastic resin was confirmed by Raman measurement.

[0409] [Comparative Example 1]

[0410] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that only the resin 1 was used as the thermoplastic resin.

[0411] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, a thermoplastic resin was confirmed by Raman measurement.

[0412] [Comparative Example 2]

[0413] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 1 and the resin 3 were dry-blended at a ratio of resin 1:resin 3=7:3.

[0414] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0415] [Comparative Example 3]

[0416] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 1 and the resin 4 were dry-blended at a ratio of resin 1:resin 4=7:3.

[0417] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0418] [Comparative Example 4]

[0419] The same test as in Example 1 was conducted using "Tepex dynalite 101" (thickness 2 mm) manufactured by Lanxess, in which polyamide 66 was impregnated into glass cloth. Also, a continuous fiber-reinforced resin molded body was obtained in the same manner as in Example 1.

[0420] [Comparative Example 5]

[0421] The same test as in Example 1 was conducted using "Tepex dynalite 102" (thickness 2 mm) manufactured by Lanxess, in which polyamide 6 was impregnated into glass cloth. Also, a continuous fiber-reinforced resin molded body was obtained in the same manner as in Example 1.

[0422] [Comparative Example 6]

[0423] The same test as in Example 1 was conducted using "Tepex dynalite 104" (thickness 2 mm) manufactured by Lanxess, in which polypropylene was impregnated in glass cloth. Also, a continuous fiber-reinforced resin molded body was obtained in the same manner as in Example 1.

[0424] [Comparative Example 7]

[0425] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that only the resin 3 was used as the thermoplastic resin.

[0426] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, a thermoplastic resin was confirmed by Raman measurement.

[0427] [Comparative Example 8]

[0428] A continuous fiber reinforced resin composite material and a continuous fiber reinforced resin molded product were obtained in the same manner as in Example 1 except that the resin 1 and the resin 8 were dry-blended at a ratio of resin 1:resin 8=7:3.

[0429] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, two types of thermoplastic resins were confirmed by Raman measurement.

[0430] [Comparative Example 9]

[0431] A continuous fiber-reinforced resin composite material and a continuous fiber-reinforced resin molded product were obtained in the same manner as in Example 1 except that only Resin 4 was used as the thermoplastic resin.

[0432] The thickness of the continuous fiber reinforced resin composite material was 2 mm. In addition, a thermoplastic resin was confirmed by Raman measurement.

[0433] [Comparative Example 10]

[0434] Prepare 16 bobbins wound with carbon fiber bundles (Toray Industries, Inc., T700S-12K), and continuously feed the carbon fiber bundles from each bobbin through a yarn guide. In the impregnation mold, the resin 12 quantitatively supplied by the filled feeder is impregnated into the continuously fed carbon fiber bundle (CFUD). The carbon fiber impregnated with the resin 12 in the impregnation mold is continuously pulled out from the nozzle of the impregnation mold at a pulling speed of 1m / min using a pulling roller. The temperature (processing temperature) when drawing the carbon fiber is 445°C. The pulled carbon fiber bundle is passed through a cooling roller to cool and solidify the resin 12, and is wound on a winder as a continuous fiber reinforced resin composite material.

[0435] The obtained continuous fiber reinforced resin composite material had a thickness of 0.08 mm and a width of 50 mm, and a continuous fiber reinforced resin composite material in which the reinforcing fibers were arranged in one direction and the volume content was 60%. In addition, a continuous fiber reinforced resin molded body (300 mm×50 mm×0.08 mm) was obtained in the same manner as in Example 1.

[0436] [Comparative Example 11]

[0437] The continuous fiber (carbon fiber TR50S15L (single fiber number 15000) manufactured by Mitsubishi Rayon Co., Ltd.) (CFUD) opened at 120°C and expanded to a width of 30 cm was pulled at 2 m / min, and the resin 13 melted at 295°C was uniformly dripped on the continuous fiber so that the mass ratio of the resin 13 to the continuous fiber was about 1:1. It was sandwiched between polyimide films, pressed with a roll press at 295°C and 2 MPa, and then cooled to obtain a fiber-reinforced polyamide sheet with a width of 30 cm and a thickness of 0.21 mm.

[0438] 12 sheets of the obtained fiber-reinforced polyamide sheets were stacked in a manner such that the fiber directions were 0°, 90°, 0°, 90°, 0°, 90°, 90°, 0°, 90°, 0°, 90°, 0°, 90°, 0°, and 0° relative to one side of a 12 cm square mold (length 12 cm), and placed in the above mold. The mold was placed in a vacuum press, and the mold temperature was raised from 30°C to 300°C in 40 minutes while evacuating the mold. After maintaining at 300°C for 30 minutes, the evacuation was stopped, and the mold was cooled to 30°C in 15 minutes while applying a pressure of 5 MPa, to obtain a continuous fiber-reinforced resin composite material with a thickness of about 2 mm. In addition, a continuous fiber-reinforced resin molded body (120 mm × 120 mm × 2 mm) was obtained in the same manner as in Example 1.

[0439]

[0440]

[0441] According to Table 1 above, in the continuous fiber reinforced resin composite materials of Examples 1 to 15, the peak temperature of tan δ at the interface between the continuous reinforcing fiber and the thermoplastic resin is 80°C or more, thereby showing very high tensile stress, bending stress, bending modulus, impact strength, and physical properties when water absorption-high temperature. In addition, in the continuous fiber reinforced resin composite materials of Examples 1 to 12 and 15, since they contain isophthalic acid units, they are excellent in practically important water absorption-high temperature characteristics. On the other hand, in Comparative Examples 1 to 11, since the aromatic concentration and the static wettability of the continuous reinforcing fiber and the thermoplastic resin are insufficient, the peak temperature of tan δ at the interface is lower than the peak temperature of tan δ of the resin itself, which is less than 80°C, thereby reducing the tensile stress, bending stress, bending modulus, impact strength, and physical properties when water absorption-high temperature.

[0442] Industrial Applicability

[0443] The continuous fiber-reinforced resin composite material of this embodiment has industrial applicability as a reinforcing material for materials requiring high levels of mechanical properties such as structural parts of various machines and automobiles, and as a composite molded product material with a thermoplastic resin composition.

Claims

1. A continuous fiber reinforced resin composite material, comprising continuous reinforcing fibers and a thermoplastic resin, characterized in that: The continuous fiber reinforced resin composite material has a tan δ peak temperature of 80° C. or higher at the interface between the continuous reinforcing fiber and the thermoplastic resin. The thermoplastic resin contains 50 to 99 parts by mass of (A) an aliphatic polyamide and 1 to 50 parts by mass of (B) a semi-aromatic polyamide, wherein the (B) semi-aromatic polyamide contains a dicarboxylic acid unit containing at least 75 mol % of an isophthalic acid unit and a diamine unit containing at least 50 mol % of a diamine unit having 4 to 10 carbon atoms. The content of the (B) semi-aromatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is 12% by mass to 50% by mass.

2. The continuous fiber reinforced resin composite material according to claim 1, wherein: The interface strength of the continuous fiber reinforced resin composite material based on a push-out test is 1.58 mN / μm to 5.00 mN / μm.

3. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The interface constant of the continuous fiber reinforced resin composite material represented by the following formula is 20 to 100, (Interface constant) = (concentration of carboxyl terminal groups in continuous fiber-reinforced resin composite material [μmol / g]) × (grinding pressure at which interface peeling occurs [MPa]) × (reinforcement fiber diameter [μm]) / (reinforcement fiber density [g / cm 3 ]) 2 .

4. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The continuous reinforced fiber composite material is 950cm -1 ~1050cm -1 Has Raman peak.

5. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The thermoplastic resins are two or more.

6. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The peak intensity of the (1,0,0) plane of the continuous fiber reinforced resin composite material in X-ray diffraction is stronger than the peak intensity of the (0,1,0) plane.

7. The continuous fiber reinforced resin composite material according to claim 6, wherein: The ratio I(0,1,0) / I(1,0,0) of the peak intensity I(0,1,0) of the (0,1,0) plane to the peak intensity I(1,0,0) of the (1,0,0) plane is 0.30 to 0.

95.

8. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: A peak of the (1,1,0) plane is detected in X-ray diffraction of the continuous fiber-reinforced resin composite material.

9. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The continuous reinforcing fibers are woven fabrics, unidirectional materials or non-crimped fabrics of glass fibers, The weight average molecular weight (Mw) of the thermoplastic resin is 15,000 to 35,000.

10. The continuous fiber reinforced resin composite material according to claim 9, wherein: The amount of the blocked terminals expressed as equivalents relative to 1 g of the (A) aliphatic polyamide and the (B) semi-aromatic polyamide is 5 micro equivalents / g to 180 micro equivalents / g.

11. The continuous fiber reinforced resin composite material according to claim 9, wherein: The content of the (B) semi-aromatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is 20% by mass to 50% by mass.

12. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The continuous fiber reinforced resin composite material has a tensile stress of 500 MPa or more under the conditions of 23° C. and 50% RH.

13. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The tensile stress retention rate of the continuous fiber reinforced resin composite material at 80° C. is above 80%.

14. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The tensile stress retention rate of the continuous fiber reinforced resin composite material when absorbing water is more than 80%.

15. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The continuous fiber reinforced resin composite material has a bending stress of 700 MPa or more under the conditions of 23° C. and 50% RH.

16. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The bending stress retention rate of the continuous fiber reinforced resin composite material at 80° C. is above 60%.

17. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The bending stress retention rate of the continuous fiber reinforced resin composite material when absorbing water is more than 80%.

18. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The continuous fiber reinforced resin composite material has a flexural modulus of 26 GPa or more under the conditions of 23° C. and 50% RH.

19. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The flexural modulus retention rate of the continuous fiber reinforced resin composite material at 80° C. is above 80%.

20. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The bending modulus retention rate of the continuous fiber reinforced resin composite material when absorbing water is more than 80%.

21. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The continuous fiber reinforced resin composite material has an impact strength of 5.0 kN / m or more.

22. The continuous fiber reinforced resin composite material according to claim 1 or 2, wherein: The viscosity of the thermoplastic resin is 40 g / 10 min or less.

23. The continuous fiber reinforced resin composite material according to claim 5, wherein: Among the two or more thermoplastic resins, the mass ratio of the resin having the largest mass ratio is 5 times or less than the mass ratio of the resin having the second largest mass ratio.

24. The continuous fiber reinforced resin composite material according to claim 9, wherein: The total content of the (A) aliphatic polyamide and the (B) semi-aromatic polyamide is 70% to 100% by mass based on 100% by mass of the thermoplastic resin.

25. A continuous fiber reinforced resin molded body comprising continuous reinforcing fibers and a thermoplastic resin, characterized in that: The continuous fiber reinforced resin composite molded body has a tan δ peak temperature of 80° C. or higher at the interface between the continuous reinforcing fibers and the thermoplastic resin, an interface strength of 1.58 mN / μm to 5.00 mN / μm based on an ejection test, and has a plate-like, frame-like, box-like, or a combination thereof shape. The thermoplastic resin contains 50 to 99 parts by mass of (A) an aliphatic polyamide and 1 to 50 parts by mass of (B) a semi-aromatic polyamide, wherein the (B) semi-aromatic polyamide contains a dicarboxylic acid unit containing at least 75 mol % of an isophthalic acid unit and a diamine unit containing at least 50 mol % of a diamine unit having 4 to 10 carbon atoms. The content of the (B) semi-aromatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is 12% by mass to 50% by mass.

26. The continuous fiber reinforced resin molded body according to claim 25, wherein: The thermoplastic resins are two or more.

27. The continuous fiber reinforced resin molded body according to claim 25 or 26, wherein: The continuous reinforcing fibers are woven fabrics, unidirectional materials or non-crimped fabrics of glass fibers, The weight average molecular weight (Mw) of the thermoplastic resin is 15,000 to 35,000.

28. The continuous fiber reinforced resin molded body according to claim 27, wherein: The content of the (B) semi-aromatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is 20% by mass to 50% by mass.

29. The continuous fiber reinforced resin molded body according to claim 25 or 26, wherein: The amount of the blocked terminals expressed as equivalents relative to 1 g of the (A) aliphatic polyamide and the (B) semi-aromatic polyamide is 5 micro equivalents / g to 180 micro equivalents / g.

30. The continuous fiber reinforced resin molded body according to claim 25 or 26, wherein: The viscosity of the thermoplastic resin is 40 g / 10 min or less.

31. The continuous fiber reinforced resin molded body according to claim 26, wherein: Among the two or more thermoplastic resins, the mass ratio of the resin having the largest mass ratio is 5 times or less than the mass ratio of the resin having the second largest mass ratio.

32. The continuous fiber reinforced resin molded body according to claim 27, wherein: The total content of the (A) aliphatic polyamide and the (B) semi-aromatic polyamide is 70% to 100% by mass based on 100% by mass of the thermoplastic resin.

33. A method for producing a continuous fiber reinforced resin composite material, comprising compounding continuous reinforcing fibers with a thermoplastic resin, the method for producing a continuous fiber reinforced resin composite material according to any one of claims 1 to 24, wherein the dynamic wettability of the continuous reinforcing fibers with the thermoplastic resin is 3.0 sec or less, The thermoplastic resin contains 50 to 99 parts by mass of (A) an aliphatic polyamide and 1 to 50 parts by mass of (B) a semi-aromatic polyamide, wherein the (B) semi-aromatic polyamide contains a dicarboxylic acid unit containing at least 75 mol % of an isophthalic acid unit and a diamine unit containing at least 50 mol % of a diamine unit having 4 to 10 carbon atoms. The content of the (B) semi-aromatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is 12% by mass to 50% by mass.

34. The method for producing a continuous fiber reinforced resin composite material according to claim 33, wherein: The contact angle between the continuous reinforcing fibers and the thermoplastic resin based on a static wettability test is 38° or less.

35. The method for producing a continuous fiber reinforced resin composite material according to claim 33 or 34, wherein: The thermoplastic resin includes two or more types, and the maximum value of the difference in dynamic wettability between each of the two or more thermoplastic resins and the continuous reinforcing fibers is 3 sec or more.

36. The method for producing a continuous fiber reinforced resin composite material according to claim 33 or 34, wherein: The terminal group concentration of the (A) aliphatic polyamide is 1 / 2 or less of the terminal group concentration of the (B) semi-aromatic polyamide.

37. The method for producing a continuous fiber reinforced resin composite material according to claim 36, wherein: The content of the (B) semi-aromatic polyamide in 100% by mass of the polyamide in the thermoplastic resin is 20% by mass to 50% by mass.

38. The method for producing a continuous fiber reinforced resin composite material according to claim 36, wherein: The difference in tan δ peak temperature between the (A) aliphatic polyamide and the (B) semi-aromatic polyamide is 45°C to 100°C.

39. The method for producing a continuous fiber reinforced resin composite material according to claim 36, wherein: The weight average molecular weight Mw of the (A) aliphatic polyamide A is the weight average molecular weight Mw of the (B) semi-aromatic polyamide B More than 1.5 times of.