A method for preventing bubbles from appearing in Q235B slabs
By adjusting the chemical composition of the Q235B slab raw material and performing in-pack baking, controlling the opening and closing of the plug rod and water outlet, and pretreating the start and cold material of the starter, the bubble problem of the Q235B slab head is solved, and the finished product is improved rate and product quality.
Patent Information
- Application Number
- CN202210932283.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-08-04
AI Technical Summary
Q235B slabs often have head bubble defects in continuous casting production, resulting in black lines or scraps on the steel belt, affecting the yield rate.
Adjust the chemical composition of Q235B slab raw materials, increase the Al content, carry out in-pack baking, control the opening and closing of the plug rod and water outlet, ensure that the weight of the molten steel is within the range of 30-40 tons, and pretreat the starter cold material To avoid bubble generation.
It effectively avoids casting bubbles, improves product quality and yield, ensures sufficient deoxygenation of the steel water, and reduces the amount of casting billets due to bubble defects.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel production, and in particular to a method for preventing bubbles from appearing in a Q235B slab. Background Art
[0002] Q235B is a grade that is widely used in industrial production, and Q235B plates account for a large proportion of steel plant production orders.
[0003] In the process of implementing the present invention, the inventors found that there are at least the following problems in the prior art:
[0004] In the continuous casting production of Q235B, the subcutaneous bubble defects at the head of the first slab are relatively dense. When the bubbles are light, black lines appear on the steel strip after rolling. When the bubbles are serious, dense black lines will produce scrap. Therefore, how to prevent bubbles from appearing at the head of the Q235B slab and thus improve the yield rate is a problem that needs to be solved. Summary of the invention
[0005] The embodiment of the present invention provides a method for preventing bubbles from appearing in Q235B slabs, so as to solve the problem of dense bubble defects in the first slab cast from the machine in the prior art, thereby improving the yield.
[0006] To achieve the above-mentioned purpose, an embodiment of the present invention provides a method for preventing bubbles from appearing in Q235B slabs, characterized in that it includes: adjusting the chemical composition weight percentage of the Q235B slab raw material to: C: 0.16~0.19Wt%, Si: 0.08~0.12Wt%, Mn: 0.25~0.35Wt%, P: ≤0.030Wt%, S: ≤0.020Wt%, Alt: 0.009~0.012Wt%; baking the middle package before it goes online; wherein, it includes a low-temperature baking process and a high-temperature baking process; in the low-temperature baking process, the baking temperature is <900°C, and the baking time is ≥60min; in the high-temperature baking process, the baking temperature is 900~1300°C, and the baking time is 120~180min.
[0007] Furthermore, the method also includes: performing stopper rod opening and closing control on the first furnace of the middling machine; and performing argon blowing opening and closing control on the upper water inlet of the first furnace of the middling machine.
[0008] Furthermore, the method also includes: controlling the weight of the molten steel when the tundish is poured within a preset weight range.
[0009] Furthermore, the method also includes: pre-treating the cold material at the start of the machine.
[0010] Furthermore, the stopper rod opening and closing control of the first furnace of the tundish lifting machine specifically includes: judging whether the pulling speed of the first furnace of the tundish lifting machine is lower than 0.8m / min; if so, closing the stopper rod; if not, opening the stopper rod.
[0011] Furthermore, the argon blowing on and off control of the water inlet of the first furnace of the tundish lifting machine specifically includes: judging whether the pulling speed of the first furnace of the tundish lifting machine is lower than 0.8m / min; if so, closing the water inlet for argon blowing, and adjusting the argon blowing amount between the slides to <2L / min; if not, opening the water inlet for argon blowing.
[0012] Furthermore, the preset weight range is 30 to 40 tons.
[0013] Furthermore, the pretreatment of the cold material at the start of the machine specifically includes: baking the cold material at the start of the machine, wherein the baking temperature is 100-300° C. and the baking time is 60-90 minutes.
[0014] Furthermore, after baking the cold starting material, the method further includes: air cooling the baked cold starting material for 60 minutes.
[0015] The above technical solution has the following beneficial effects:
[0016] In the technical solution of the present invention, the Alt content in the steel is increased by 50-80ppm compared with the ordinary Q235B by adjusting the chemical composition of the raw materials, which effectively ensures that the molten steel is fully deoxidized and avoids bubbles in the casting billet caused by insufficient deoxidation of the molten steel during the start-up process; at the same time, through technical means such as baking the tundish, controlling the weight of the molten steel when the tundish is poured, baking pretreatment of the cold material at the start-up, and controlling the opening and closing of the stopper rod and the upper water inlet argon blowing, the factors causing bubbles to appear at the head of the Q235B slab are effectively avoided, thereby improving the product quality. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] The embodiment of the present invention provides a method for preventing bubbles from appearing in Q235B slabs, comprising: adjusting the chemical composition weight percentage of the Q235B slab raw material to: C: 0.16-0.19Wt%, Si: 0.08-0.12Wt%, Mn: 0.25-0.35Wt%, P: ≤0.030Wt%, S: ≤0.020Wt%, Alt: 0.009-0.012Wt%; before the middle package is put on line, the middle package is baked. The baking of the middle package includes a low-temperature baking process and a high-temperature baking process; wherein, in the low-temperature baking process, the baking temperature is <900°C and the baking time is ≥60min; in the high-temperature baking process, the baking temperature is 900-1300°C and the baking time is 120-180min.
[0019] In the prior art, the general Q235B composition is designed as follows: C: 0.15-0.19%; Si: 0.05-0.20%; Mn: 0.25-0.45%; P: ≤0.035%; S: ≤0.030%; Alt≤0.005%.
[0020] By tracking the actual production situation on site for a long time, it was found that it was not easy to produce bubbles when starting the casting of steel with a higher aluminum content. The inventor analyzed that this was mainly because the Al content in Q235B using conventional technology was low, the molten steel was not fully deoxidized, and the bubbles could not fully float up during the startup process, causing bubbles in the casting. To this end, the present invention increases the Als content of the deoxidizing element in Q235B steel, so the Q235B composition before the start-up furnace is designed to be C: 0.16-0.19%; Si: 0.08-0.12%; Mn: 0.25-0.35%; P: ≤0.030%; S: ≤0.020%; Alt: ≤0.009-0.012%. The Alt content in the steel designed with this composition is increased by 50-80ppm compared with the original design, which effectively ensures that the molten steel is fully deoxidized, avoids the bubbles in the billet caused by insufficient deoxidation of the molten steel during the start-up process, and the basic control of the bubbles in the billet at the start-up head is effectively controlled, which greatly reduces the amount of the billet with bubble defects; but at the same time, it is confirmed by actual measurement that the Al content is not easy to be too high, otherwise the billet is prone to crack defects.
[0021] Research has found that if the water in the tundish coating is not evaporated cleanly, the water will form oxygen and hydrogen when it meets the high-temperature molten steel, which is also a factor that causes bubbles in the ingot. For this reason, this application checks the vent holes of the tundish before the tundish goes online to ensure that the vent holes are unobstructed, and adds baking time for the newly built permanent layer or permanent layer supplement. In order to achieve good results, the baking time and tundish temperature of each stage must be guaranteed. The baking time below 900°C is not less than 60 minutes, and the baking time at 900-1300°C is guaranteed to be 120-180 minutes.
[0022] The reason for the temperature and time limit is that if the baking time is too short below 900℃, it will easily cause the moisture of the refractory to be difficult to be discharged evenly and slowly. At the same time, if the baking temperature is increased quickly, it will easily cause cracks and collapse of the refractory materials. The baking time of 900-1300℃ is guaranteed to be 120-180 minutes, mainly to ensure that the temperature of the middle bag is as close to the temperature of the molten steel as possible in the high temperature stage and reduce the temperature drop of the molten steel. At the same time, the high temperature baking time cannot be too long, which will easily lead to oxidation of the refractory and shorten its life.
[0023] Furthermore, the method also includes: respectively performing stopper rod opening and closing control and upper water inlet argon blowing opening and closing control on the first furnace of the tundish raising machine; the stopper rod opening and closing control on the first furnace of the tundish raising machine specifically includes: judging whether the pulling speed of the first furnace of the tundish raising machine is lower than 0.8m / min; if so, closing the stopper rod; if not, opening the stopper rod; the upper water inlet argon blowing opening and closing control on the first furnace of the tundish raising machine specifically includes: judging whether the pulling speed of the first furnace of the tundish raising machine is lower than 0.8m / min; if so, closing the upper water inlet argon blowing, and adjusting the argon blowing amount between the slides to <2L / min; if not, opening the upper water inlet argon blowing.
[0024] When the pulling speed is lower than 0.8m / min, the stopper rod and the upper water inlet shall be closed for argon blowing, and the argon blowing amount between the slide plates shall be ensured to be less than 2L / min. This is because the pulling speed of the tundish starting furnace is relatively slow, and the gas of the casting machine is not easy to be discharged at the low pulling speed stage. Therefore, reducing the amount of argon blowing or stopping argon blowing at the low pulling speed stage of the casting machine can effectively prevent the generation of bubbles. After the pulling speed exceeds 0.8m / min, the stopper rod and the upper water inlet shall be opened normally for argon blowing.
[0025] Furthermore, the method also includes: controlling the weight of the molten steel when the tundish is poured to be within the range of 30 to 40 tons.
[0026] When the tonnage of the tundish is less than 30 tons, it is not conducive to the bubbling of bubbles, which may cause bubbles when the machine is started; but if the tonnage exceeds 40 tons, the molten steel will stop flowing in the tundish for too long, and the plugging rod head may stick to the steel, causing a pouring accident. Practice has shown that controlling the tonnage of the tundish at 30-40 tons can increase the residence time of the molten steel in the tundish, which is conducive to the bubbles in the molten steel to float fully, and at the same time can avoid the plugging rod sticking to cold steel when pouring.
[0027] Furthermore, the method further comprises: pre-treating the cold material at the start of the machine. The pre-treatment method is baking, wherein the baking temperature is set to 100-300°C, the baking time is set to 60-90 minutes, and then air-cooling for 60 minutes is performed to facilitate the arrangement of the cold material.
[0028] The dampness of the cold material at the start of the machine can easily cause bubbles in the first piece of the billet. Therefore, this pretreatment process can be set to ensure that the auxiliary material is dry and avoid the introduction of moisture, which will decompose into oxygen and hydrogen at high temperature to cause bubbles.
[0029] In a specific embodiment using the technical solution of the present application, the bubble rate of the Q235B starting casting was reduced from 7.7% to 2%, achieving good results.
[0030] In the above detailed description, various features are grouped together in a single embodiment to simplify the disclosure. This method of disclosure should not be interpreted as reflecting an intention that the embodiments of the claimed subject matter require more features than are clearly stated in each claim. On the contrary, as reflected in the appended claims, the invention is in a state of having less than all the features of the disclosed individual embodiments. Therefore, the appended claims are hereby expressly incorporated into the detailed description, with each claim standing on its own as a separate preferred embodiment of the invention.
[0031] The disclosed embodiments are described above to enable any person skilled in the art to implement or use the present invention. Various modifications of these embodiments are obvious to those skilled in the art, and the general principles defined herein may also be applied to other embodiments without departing from the spirit and scope of the present disclosure. Therefore, the present disclosure is not limited to the embodiments given herein, but is consistent with the broadest scope of the principles and novel features disclosed in this application.
[0032] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method to prevent bubbles from appearing in Q235B slabs. It is characterized in that include: The chemical composition weight percentage of Q235B slab raw material is adjusted to: C: 0.16-0.19wt%, Si: 0.08-0.12wt%, Mn: 0.25-0.35wt%, P: ≤0.030wt%, S: ≤0.020wt%, Alt: 0.009-0.012wt%; Before the middle bag goes on line, the middle bag is baked; Among them, it includes a low-temperature baking process and a high-temperature baking process; In the low-temperature baking process, the baking temperature is less than 900°C and the baking time is greater than or equal to 60 minutes; In the high temperature baking process, the baking temperature is 900-1300° C. and the baking time is 120-180 min. Control the weight of molten steel when pouring in the tundish within the preset weight range; The preset weight range is 30 to 40 tons.
2. The method for preventing bubbles from appearing in Q235B slabs as claimed in claim 1, It is characterized in that Also includes: Pre-treat the cold material at the start of the machine.
3. The method for preventing bubbles from appearing in Q235B slabs as claimed in claim 2, It is characterized in that The pretreatment of the cold material at the start of the machine specifically includes: The cold material is baked, wherein the baking temperature is 100-300° C. and the baking time is 60-90 minutes.
4. The method for preventing bubbles from appearing in Q235B slabs as claimed in claim 3, It is characterized in that After the cold material is baked, the method further comprises: The baked starting cold material is air-cooled for 60 minutes.