A preparation method of a cobalt catalyst for hydroformylation reaction, a catalyst and its application

Through the reaction of cobalt salt with dioxane and phosphine ligands, and then adding complex ligands to form a positively charged cobalt catalyst, the problems of low activity and poor selectivity of the cobalt catalyst are solved, and an efficient hydroformylation reaction is achieved , reducing by-product generation and costs.

CN115304649BActive Publication Date: 2024-10-18WANHUA CHEM GRP CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210983721.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-17
Publication Date
2024-10-18
Estimated Expiration
2042-08-17

AI Technical Summary

Technical Problem

Existing cobalt catalysts have low activity and poor selectivity in hydroformylation reactions, resulting in the formation of by-products. They are also costly and difficult to use stably at high temperatures.

Method used

The cobalt salt is reacted with dioxane and phosphine ligands to generate a precursor, and then complexing ligands such as tetrafluoroboric acid or tetraphenylboric acid are added to form a cobalt catalyst with a positively charged metal cobalt center and a macronuclear anion. Preparation under water-free and oxygen-free nitrogen protection.

Benefits of technology

The activity and selectivity of the cobalt catalyst are improved, the formation of by-products is reduced, the cost is lower, it is suitable for high-temperature hydroformylation reactions, and the conversion rate and selectivity are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a method for preparing a cobalt catalyst for hydroformylation reaction, wherein cobalt salt is used as a raw material, dioxane and a phosphine ligand are added, a precursor is obtained by reaction, and the precursor is reacted with at least one of tetrafluoroborate ethyl ether, tetraphenylboric acid, and hexafluorophosphoric acid to obtain a novel cobalt catalyst. The present invention also provides a cobalt catalyst prepared by the method and its application in hydroformylation reaction. Compared with a traditional cobalt catalyst, the novel cobalt catalyst prepared by the method of the present invention has higher catalytic activity, good selectivity, and greater economic value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydroformylation, and in particular to a preparation method of a cobalt catalyst for hydroformylation reaction, the catalyst and application of the catalyst in the hydroformylation reaction. Background Art

[0002] The hydroformylation reaction, also known as the OXO reaction, is a catalytic reaction process in which olefins and synthesis gas (CO+H2) are reacted in the presence of a catalyst to produce aldehydes or alcohols.

[0003] At present, hydroformylation catalysts are divided into two categories: rhodium metal and cobalt metal. The activity of rhodium catalyst is more than 100 times that of cobalt catalyst, and the selectivity is good. However, the price of rhodium catalyst is expensive, which is more than 1000 times that of cobalt catalyst. The industry will consider the cost issue when using it. At present, the systems using rhodium catalyst are mostly short-chain olefins such as propylene and butene. Rhodium catalyst must have a strict recovery process to prevent the loss of cost reduction. Cobalt catalyst has low cost, but low catalyst activity and poor selectivity. By-products such as alkanes, alcohols, and acetals are easily generated during the hydroformylation process. The hydroformylation of high-carbon olefins is still dominated by cobalt catalysts. This is because the boiling point of high-carbon aldehydes and alcohols is very high. The high-carbon aldehydes and alcohols prepared from high-carbon olefins must be separated from the catalyst by flash evaporation at high temperature, and the rhodium catalyst will decompose and lose at high temperature. The separation and recycling process is complicated and the cost is high.

[0004] CN103561869A discloses a catalyst composition for hydroformylation and a hydroformylation method using the catalyst composition, wherein the catalyst composition comprises a monodentate phosphine ligand and a transition metal catalyst. However, the catalyst still has the problems of low activity and poor selectivity of cobalt catalysts.

[0005] In view of the shortcomings of low activity and poor selectivity of current cobalt catalysts, it is necessary to develop a new cobalt catalyst to improve the activity and selectivity of cobalt catalysts in the hydroformylation process. Summary of the invention

[0006] In order to solve the problems existing in the prior art, the purpose of the present invention is to develop a new cobalt catalyst and a preparation method thereof, so as to improve the activity and selectivity of the cobalt catalyst in the hydroformylation process.

[0007] Another object of the present invention is to provide the use of the cobalt catalyst in hydroformylation reaction.

[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solution:

[0009] A method for preparing a cobalt catalyst for hydroformylation reaction comprises the following steps:

[0010] 1) Using cobalt salt as raw material, adding dioxane, heating, stirring to dissolve, adding phosphine ligand, stirring to react for a period of time, cooling to room temperature, removing the remaining dioxane, and obtaining a precursor powder;

[0011] 2) dissolving the precursor powder in a solvent, adding a complexing ligand, wherein the complexing ligand is preferably at least one of tetrafluoroborate ether, tetraphenylboric acid, and hexafluorophosphoric acid, stirring the reaction, removing the solvent, obtaining a red or brown powder, and washing with the solvent to obtain a cobalt catalyst.

[0012] In a specific embodiment, the cobalt salt in step 1) is selected from any one or more of cobalt chloride, cobalt acetate, cobalt nitrate, cobalt sulfate, cobalt tetrafluoroborate, cobalt acetylacetonate, and cobalt isooctanoate.

[0013] In a specific embodiment, the phosphine ligand in step 1) is selected from any one of a monodentate phosphine ligand, a bidentate phosphine ligand or a tridentate phosphine ligand; preferably selected from PPh3, PMe3, PEt3, P(n-bu)3, P(t-bu)3, PCy3, P(OEt)3, P(OPh)3, dppe, dppf, Xantphos, DPEpHos, BINAP, dppbenz, dppm, dmpe, dppb, dcpe, D t Any of BPF.

[0014] In a specific embodiment, after adding dioxane in step 1), the mixture is heated to 60-101°C and stirred to dissolve, a phosphine ligand is added, and the mixture is stirred at 20-80°C for 2-10 hours, then cooled to room temperature and the solvent is removed to obtain a precursor powder; preferably, the precursor is washed with dioxane.

[0015] In a specific embodiment, the solvent in step 2) is selected from at least one of acetone, dichloromethane and acetonitrile; preferably, after adding the complexing ligand, the reaction is stirred at 20-50° C. for 2-10 hours.

[0016] In a specific embodiment, in step 1), the mass ratio of the cobalt salt to dioxane is 1:1-1:30, preferably 1:5-1:10; the mass ratio of the cobalt salt to the phosphine ligand is 1:1-1:10, preferably 1:2-1:5; preferably, the mass ratio of the cobalt salt to the complexing ligand is 1:1-1:5, preferably 1:2-1:3.

[0017] In a specific embodiment, the entire catalyst preparation process requires nitrogen protection and is strictly operated in anhydrous and oxygen-free conditions.

[0018] On the other hand, a cobalt catalyst prepared by the aforementioned preparation method.

[0019] In another aspect, a cobalt catalyst prepared by the aforementioned preparation method is used in a hydroformylation reaction.

[0020] In a specific embodiment, the amount of catalyst added in the hydroformylation reaction is 5-1000ppm, preferably 50-200ppm, calculated as metal, the reaction pressure is 1-30Mpa, and the temperature is 50-200°C; preferably, the olefin feedstock used in the hydroformylation reaction includes C2-C20 straight-chain and branched olefins; more preferably, the olefin conversion rate is above 93% and the selectivity is above 96%.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The cobalt catalyst prepared by the method of the present invention has a metal cobalt center with a positive charge and an anion with a large core on the outside; since the metal cobalt center is always positively charged and is in an electron-deficient state, it has higher activity in coordination with olefins and activation insertion reactions; at the same time, due to the large steric hindrance of the external anion, the steric effect leads to significantly improved selectivity for olefin hydroformylation reactions. DETAILED DESCRIPTION

[0023] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0024] A method for preparing a cobalt catalyst for hydroformylation reaction comprises the following steps:

[0025] 1) Using cobalt salt as raw material, add dioxane, heat to 60-101°C, stir to dissolve, add phosphine ligand, stir to react at 20-80°C for 2-10h, cool to room temperature, remove excess dioxane, obtain precursor powder, and wash with dioxane.

[0026] 2) Dissolve the precursor powder in acetone and / or dichloromethane and / or acetonitrile, add tetrafluoroborate ether and / or tetraphenylboric acid and / or hexafluorophosphoric acid, stir and react at 20-50° C. for 2-10 hours, remove the solvent to obtain a red or brown powder, wash with a solvent to obtain a cobalt catalyst.

[0027] The cobalt salt used is preferably one or more selected from the group consisting of cobalt chloride, cobalt acetate, cobalt nitrate, cobalt sulfate, cobalt tetrafluoroborate, cobalt acetylacetonate, and cobalt isooctanoate.

[0028] The phosphine ligand used is one of the currently disclosed monodentate phosphine ligands, bidentate phosphine ligands and tridentate phosphine ligands, including but not limited to any one selected from PPh3, PMe3, PEt3, P(n-bu)3, P(t-bu)3, PCy3, P(OEt)3, P(OPh)3, dppe, dppf, Xantphos, DPEpHos, BINAP, dppbenz, dppm, dmpe, dppb, dcpe, and DtBPF.

[0029] Among them, the mass ratio of cobalt salt to dioxane is 1:1-1:30, for example, including but not limited to 1:1, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, preferably 1:5-1:10, the overall mass ratio of cobalt salt to tetrafluoroborate ethyl ether and / or tetraphenylboric acid and / or hexafluorophosphoric acid is 1:1-1:5, for example, including but not limited to 1:1, 1:2, 1:3, 1:4, 1:5, preferably 1:2-1:3, the mass ratio of cobalt salt to phosphine ligand is 1:1-1:10, for example, including but not limited to 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, preferably 1:2-1:5.

[0030] The entire catalyst preparation process requires nitrogen protection and strict anhydrous and oxygen-free operation.

[0031] On the other hand, when the cobalt catalyst of the present invention is used for hydroformylation reaction, the amount of hydroformylation reaction catalyst added is 5-1000ppm in terms of metal, for example, including but not limited to 10ppm, 50ppm, 100ppm, 150ppm, 200ppm, 250ppm, 300ppm, 350ppm, 400ppm, 450ppm, 500ppm, 550ppm, 600ppm, 650ppm, 700ppm, 750ppm, 800ppm, 850ppm, 900ppm, 950ppm, preferably 50-200ppm, the hydroformylation reaction pressure is 1-30Mpa, the temperature is 50-200°C, and the olefin raw materials used include C2-C20 straight-chain and branched olefins, which can be selected with reference to the prior art.

[0032] The reaction of the preparation process of the cobalt catalyst is as follows (taking Xantphos ligand and hexafluorophosphoric acid as raw materials as an example):

[0033] n, p, j, q are integers between 1 and 5.

[0034] Cobalt salt is heated and dissolved in dioxane to form a cobalt compound with dioxane ligands. After adding phosphine ligands, the phosphine ligands continue to coordinate with cobalt to form a cobalt precursor compound. After removing the solvent and separating the precursor compound, hexafluorophosphoric acid is added. Due to the strong acid effect, it will exchange with the original coordinated anion, and cobalt will lose its original anion to form a new hexafluorophosphate coordinated cobalt catalyst. The most notable feature of the new catalyst is that the metal cobalt center has a positive charge and there is a large-core anion on the outside.

[0035] The novel cobalt catalyst of the present invention is used to catalyze the hydroformylation reaction mechanism as follows:

[0036]

[0037] In the synthesis gas atmosphere, the cobalt catalyst forms an active intermediate A. A and B are in equilibrium under the synthesis gas conditions. The olefin coordinates with the catalyst intermediate B to form an intermediate C, which then undergoes a hydrogen insertion reaction to form an intermediate D. Intermediate D continues to undergo a carbonyl insertion reaction to form an intermediate E. Intermediate E continues to undergo a coordination addition reaction with hydrogen to generate the final product aldehyde and intermediate B, and B continues to participate in the catalytic cycle.

[0038] The main reason for the improved catalytic activity compared with traditional cobalt catalysts is speculated to be that the metal cobalt center is always positively charged and in an electron-deficient state, which has higher activity in coordination with olefins and activation insertion reactions. The reason for the improved selectivity is that the external anion has large steric hindrance, and the spatial effect leads to improved selectivity for olefin hydroformylation reactions.

[0039] The present invention will be further described in detail below in conjunction with the embodiments, but shall not be construed as limiting in any way.

[0040] The main raw material sources of the embodiment are as follows:

[0041] All cobalt salts, phosphine ligands, tetrafluoroboric acid, tetraphenylboric acid, hexafluorophosphoric acid and solvents in the following examples were purchased from MacLean Reagent Company.

[0042] The analytical instruments and methods used in the examples are as follows:

[0043] Gas chromatograph: Agilent-7820;

[0044] Gas chromatography column: 0.25mm×30m DB-5 capillary column, detector FID, vaporization chamber temperature 280℃, column box temperature 280℃, FID detector temperature 300℃, argon flow rate 2.1mL / min, hydrogen flow rate 30mL / min, air flow rate 400mL / min, injection volume 1.0μL. The conversion rate of olefins and the selectivity of products were calculated using the area normalization method. Heating program: preheat to column temperature 40℃, maintain for 5min, increase from 40℃ to 280℃ at a rate of 15℃ / min, and maintain for 2min.

[0045] All conversion and selectivity statistics below are from chromatographic analysis.

[0046] Example 1

[0047] Add 10g of cobalt acetate and 10g of dioxane to a 500ml three-necked flask, heat to 60°C, stir to dissolve, add 10g of Pcy3 ligand, stir to react at 20°C for 2h, cool to room temperature, remove the solvent, obtain a precursor powder, and wash with ether solvent. Dissolve the precursor powder in acetone, add 10g of tetrafluoroborate ether, stir to react at 20°C for 2h, remove the solvent, obtain a red powder, wash with hexane, and obtain a cobalt catalyst.

[0048] Example 2

[0049] Add 10g of cobalt octanoate and 300g of dioxane to a 1000ml three-necked flask, heat to 101°C and reflux, stir to dissolve, add 50g of DPPE phosphine ligand, stir and react at 80°C for 10h, cool to room temperature, remove the solvent, obtain a precursor powder, and wash with ether. Dissolve the precursor powder in dichloromethane, add 50g of tetraphenylboric acid, stir and react at 50°C for 10h, remove the solvent, obtain a brown powder, wash with hexane, and obtain a cobalt catalyst.

[0050] Example 3

[0051] Add 10g of cobalt acetylacetonate and 50g of dioxane to a 500ml three-necked flask, heat to 80°C, stir to dissolve, add 20g of BINAP phosphine ligand, stir to react at 60°C for 5h, cool to room temperature, remove the solvent, obtain a precursor powder, and wash with ether. Dissolve the precursor powder in dichloromethane acetonitrile, add 20g of hexafluorophosphoric acid, stir to react at 40°C for 5h, remove the solvent, obtain a brown powder, wash with hexane, and obtain a cobalt catalyst.

[0052] Example 4

[0053] Add 10g of cobalt sulfate and 100g of dioxane to a 500ml three-necked flask, heat to 90°C, stir to dissolve, add 40g of dppm phosphine ligand, stir to react at 40°C for 4h, cool to room temperature, remove the solvent, obtain a precursor powder, and wash with ether. Dissolve the precursor powder in acetonitrile, add 30g of hexafluorophosphoric acid, stir to react at 40°C for 5h, remove the solvent, obtain a red powder, wash with hexane, and obtain a cobalt catalyst.

[0054] Comparative Example 1

[0055] Cobalt carbonyl (Aladdin) and RhPAC (Aladdin) catalysts were used respectively to carry out comparative tests with the catalysts of the above four embodiments. The specific operation is as follows: 200g of 1-dodecene was added to 1L parr, and the new cobalt catalyst, cobalt carbonyl and RhPAC in Examples 1-4 were used as catalysts, with the addition amounts of 0.5g, 0.5g, 0.5g, 0.5g, 0.5g, 0.05g respectively. The synthesis reaction pressure was 18MPa (synthesis gas was continuously introduced during the reaction to maintain the reaction pressure of 18MPa), the reaction temperature was 150°C, the stirring speed was 1000r / min, the reaction was carried out for 2h, sampling and analysis were performed, and the results are shown in Table 1.

[0056] Comparative Example 2

[0057] A cobalt precursor was prepared by the method of Example 1: 10 g of cobalt acetate and 10 g of dioxane were added to a 500 ml three-necked flask, heated to 60° C., stirred to dissolve, 10 g of Pcy3 ligand was added, stirred at 20° C. for 2 h, cooled to room temperature, and the solvent was removed to obtain a precursor powder, which was washed with ether solvent.

[0058] The precursor was directly used as a catalyst, and a comparative test was carried out with the catalyst of Example 1. The specific operation was as follows: 200g of 1-dodecene was added to 1Lparr, and the precursor of Comparative Example 2 was used as a catalyst, with the addition amount being 0.5g respectively, the synthesis reaction pressure being 18MPa (synthesis gas was continuously introduced during the reaction to maintain the reaction pressure of 18MPa), the reaction temperature being 150°C, the stirring speed being 1000r / min, the reaction time being 2h, and the sampling analysis being performed. The results are shown in Table 1:

[0059] Table 1 Reaction results of examples and comparative examples

[0060]

[0061]

[0062] It can be seen that the conversion rate and selectivity of the cobalt catalyst of the present invention for hydroformylation reaction are comparable to those of the Rh catalyst, but the cost of using metallic cobalt as the active metal is lower and its performance is far superior to that of the conventional cobalt catalyst.

[0063] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A method for preparing a cobalt catalyst for hydroformylation reaction, characterized in that: The following steps are involved: 1) Take cobalt salt as raw material, add dioxane, heat to 60-101°C, stir to dissolve, add phosphine ligand, stir to react at 20-80°C for 2-10h, cool to room temperature, remove the remaining dioxane, and obtain precursor powder; The mass ratio of the cobalt salt to the dioxane is 1:1-1:30; the mass ratio of the cobalt salt to the phosphine ligand is 1:1-1:10; 2) Dissolve the precursor powder in a solvent, add a complexing ligand, stir and react at 20-50°C for 2-10 hours, remove the solvent to obtain a red or brown powder, and wash with a solvent to obtain a cobalt catalyst; The mass ratio of the cobalt salt to the complexing ligand is 1:1-1:5, and the complexing ligand is selected from at least one of tetrafluoroborate ether, tetraphenylboric acid, and hexafluorophosphoric acid; In step 1), the cobalt salt is selected from any one or more of cobalt chloride, cobalt acetate, cobalt nitrate, cobalt sulfate, and cobalt isooctanoate; In the step 1), the phosphine ligand is selected from any one of PPh3, PMe3, PEt3, P(n-bu)3, P(t-bu)3, PCy3, P(OEt)3, and P(OPh)3.

2. The preparation method according to claim 1, characterized in that: In step 1), dioxane is used to wash the precursor.

3. The preparation method according to claim 1, characterized in that: In the step 2), the solvent is selected from at least one of acetone, dichloromethane and acetonitrile.

4. The preparation method according to claim 1, characterized in that: In the step 1), the mass ratio of the cobalt salt to the dioxane is 1:5-1:10; the mass ratio of the cobalt salt to the phosphine ligand is 1:2-1:

5.

5. The preparation method according to claim 1, characterized in that: The mass ratio of the cobalt salt to the complex ligand is 1:2-1:

3.

6. The preparation method according to claim 1, characterized in that: The entire catalyst preparation process requires nitrogen protection and strict anhydrous and oxygen-free operation.

Citation Information

Patent Citations

  • Catalyst composition for hydroformylation reaction and hydroformylation method using same

    CN103561869A