Chromium oxide functionalized nickel-iron hydrotalcite nanosheets, their preparation methods and electrocatalytic applications

By synthesizing NiFe-LDH nanosheets and depositing CrxOy nanoparticles on nickel foam, a CrxOy-NiFe-LDH/NF heterostructure is formed, which solves the problem of catalyst corrosion under alkaline conditions, achieves efficient and stable seawater electrolysis catalysis, and provides A resource-rich and low-cost bifunctional electrocatalyst was developed.

CN115305481BActive Publication Date: 2024-10-01SUZHOU 30 BILLION TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211032286.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2024-10-01
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

In the existing seawater electrolysis technology, the catalyst is easily corroded by chloride ions under alkaline conditions, leading to activity decay. There is also a lack of efficient and stable cheap electrocatalysts, which limits the wide application of seawater electrolysis.

Method used

NiFe-LDH nanosheets were synthesized on foamed nickel carriers using a solvothermal method, and dense CrxOy nanoparticles were deposited on the surface through galvanostatic technology to form a CrxOy-NiFe-LDH/NF heterostructure to enhance the catalyst's resistance to chloride ion corrosion. capacity and catalytic activity.

Benefits of technology

It improves the stability and catalytic activity of the catalyst in chloride-containing electrolytes, significantly improves the performance of redox reactions and hydrogen generation reactions, and provides a resource-rich and low-cost bifunctional electrocatalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003817583210000011
    Figure HDA0003817583210000011
  • Figure HDA0003817583210000012
    Figure HDA0003817583210000012
  • Figure HDA0003817583210000021
    Figure HDA0003817583210000021
Patent Text Reader

Abstract

A chromium oxide functionalized nickel-iron hydrotalcite nanosheet catalyst for electrolysis of seawater and its preparation method and application. The present invention prepares Cr by hydrothermal and electrodeposition methods. x O y ‑NiFe‑LDH / NF heterostructure bifunctional electrocatalyst. The NiFe‑LDH nanosheets and Cr x O y The synergistic effect and strong electronic interaction between nanoparticles promote electron transfer and enhance the heterostructure Cr x O y OER and HER performance of ‑NiFe‑LDH, and Cr x O y This creates more oxygen vacancies on the catalyst surface, which helps improve the inherent catalytic activity of the catalyst. x O y The dense film composed of nanoparticles improves the catalyst's resistance to chloride ion corrosion, making Cr x O y ‑NiFe‑LDH exhibited better OER catalytic activity and stability in the electrolysis of alkaline chloride-containing aqueous solutions, which has important theoretical significance and potential application value for the development of bifunctional electrocatalysis for seawater electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention belongs to the field of new energy material technology and electrochemical catalysis, and specifically relates to a functional nickel-iron hydrotalcite nanosheet electrocatalyst; it also relates to a method for preparing the catalyst and its electrocatalytic application in the anode oxygen evolution reaction and cathode hydrogen evolution reaction of seawater electrolysis and the complete seawater electrolysis. Background technology:

[0002] Oxygen evolution reaction (OER) is a key electrode process in seawater electrolysis technology, but the large amount of chloride ions (~0.5 mol / L) in seawater poses severe challenges to seawater electrolysis. Under acidic conditions, the equilibrium potential of OER relative to the standard hydrogen electrode is only 130 mV higher than that of chlorine evolution reaction, but the two-electron transfer chlorine evolution reaction has certain kinetic advantages over the four-electron transfer oxygen evolution reaction. Under alkaline conditions of pH>7.5, chloride ions compete with OER for electrons and are oxidized to hypochlorite ions, but the starting potential of this reaction is 490 mV higher than that of OER. Therefore, efficient catalysts are required to achieve selective oxygen evolution from seawater electrolysis at an overpotential far lower than that of hypochlorite generation. Even in alkaline media, a large amount of aggressive chloride ions in seawater will cause severe corrosion to the catalyst, thereby reducing its catalytic activity. To avoid activity decay, the catalyst needs to have a certain resistance to chloride ion corrosion. At present, the precious metal electrode materials IrO2 and RuO2 have the best OER activity under alkaline conditions, but their scarcity and poor electrochemical stability limit their widespread application as seawater electrolysis catalysts in energy storage and conversion systems. Therefore, it is crucial to develop new, efficient, stable and inexpensive electrocatalysts. In recent years, compounds such as transition metal sulfides, phosphides, oxides and hydroxides have attracted widespread attention from researchers due to their abundant reserves, low cost and long-term durability, providing more possibilities for the selection of seawater electrolysis catalysts.

[0003] Due to the structural adjustability of transition metal layered hydroxides (LDH), electrocatalytically active transition metals such as Fe, Ni, Co, Mn, V, and Cr can participate in the construction of LDH layers, and related materials show excellent OER performance in neutral alkaline media. However, LDH as an OER catalyst has the disadvantages of poor conductivity, easy aggregation, insufficient exposure of active sites, and low specific surface area. For this reason, in situ growth of LDH nanocolumns on a conductive substrate is usually used to solve the above problems. Some other transition metal oxides such as MnO x and CeO xThe layer can selectively prevent chloride ions from entering the catalyst surface, thereby improving the corrosion resistance and anti-poisoning performance of the catalyst. Considering that three-dimensional heterostructured catalysts can provide a large surface area and abundant active sites in the electrolysis of seawater, there has been no report on the construction of a heterostructure of a composite of transition metal layered hydroxides and chromium oxide nanoparticles and using it as a bifunctional electrocatalyst for seawater electrolysis.

[0004] The present invention utilizes a solvent thermal method to synthesize NiFe-LDH on a nickel foam (NF) carrier, and under optimal electrodeposition conditions, a layer of Cr is electrodeposited on the surface of NiFe-LDH. x O y The dense film composed of nanoparticles was prepared x O y -NiFe-LDH / NF heterostructure electrocatalyst. NiFe-LDH nanosheets and Cr x O y The synergistic effect and strong electronic interaction between nanoparticles promote electron transfer and enhance the heterostructure Cr x O y -OER and hydrogen evolution (HER) performance of NiFe-LDH, while Cr x O y This creates more oxygen vacancies on the catalyst surface, which helps improve the inherent catalytic activity of the catalyst. x O y The dense film composed of nanoparticles improves the catalyst's resistance to chloride ion corrosion, making Cr x O y -NiFe-LDH has better stability when electrolyzing aqueous solutions containing chloride ions. This invention has important theoretical significance and potential application value for the development of transition metal catalysts for selective catalytic production of hydrogen and oxygen from seawater. Summary of the invention:

[0005] In view of the deficiencies of the prior art and the needs of research and application in this field, one of the purposes of the present invention is to provide a chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure; the composite structure is a heterogeneous structure formed by depositing chromium oxide layer nanoparticles on nickel-iron hydrotalcite nanosheets; the composite structure is prepared by adjusting the composition of the oxide coating layer in the catalyst by changing the time, potential and concentration of electrodeposition during the preparation process; the chromium oxide nanoparticles in the composite structure are prepared by constant current technology under the conditions of optimal deposition time, current density and electrolyte concentration; the composite structure is in-situ grown on nickel foam, denoted as Cr x O y -NiFe-LDH / NF.

[0006] The second object of the present invention is to provide a method for preparing a chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure, which specifically comprises the following steps:

[0007] (a) Preparation of NiFe-LDH / NF

[0008] The specification is 3*2cm 2 The nickel foam was treated with 3 mol / L hydrochloric acid solution, deionized water and ethanol by ultrasound for 20, 5 and 20 min respectively, and dried at 50°C for 6 h; 1 mmol of Ni(NO3)2·6H2O, 0.5 mmol of Fe(NO3)3·9H2O and 5 mmol of urea were weighed and dissolved in 40 mL of deionized water; the mixed solution was transferred to a 100 mL polytetrafluoroethylene reactor, and a piece of pretreated nickel foam was added to react at 120°C for 12 h. After cooling to room temperature, the nickel foam was taken out from the reactor, washed several times with deionized water and anhydrous ethanol respectively, and then dried at 50°C for 5 h to obtain NiFe-LDH / NF;

[0009] (b)Cr x O y Preparation of NiFe-LDH / NF

[0010] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 3-12 mM Cr(NO3)3·9H2O solution is used as an electrolyte, and constant potential deposition is performed under the conditions of a voltage of -0.9 to -1.2 V and a deposition time of 600 to 1800 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain Cr x O y -NiFe-LDH / NF heterostructure;

[0011] The Cr particles with a diameter of less than 10 nm in the chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure x O y The nanoparticles are densely covered on the surface of NiFe-LDH nanosheets with a lateral size of 200-500 nm and a thickness of 10-30 nm. x O y There is abundant phase interface between the nanoparticles and NiFe-LDH nanosheets.

[0012] The third object of the present invention is to provide a chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure for use as a bifunctional electrocatalyst for the anode oxygen evolution reaction and the cathode hydrogen evolution reaction in the electrolysis of seawater and water.

[0013] The present invention prepares Cr under the optimal deposition conditions. x O y -NiFe-LDH / NF heterostructure; the heterostructure promotes electron transfer and produces more oxygen vacancies on the surface, which improves the OER and HER catalytic activity of the catalyst and improves its corrosion resistance and stability in chloride ion-containing electrolytes.

[0014] Compared with the prior art, the present invention has the following main advantages and beneficial effects:

[0015] 1) Cr according to the present invention x O y -NiFe-LDH / NF catalyst is a non-precious metal composite material. The raw materials used are easy to purchase, abundant in resources and low in cost. The experimental method is easy to operate and is convenient for large-scale production;

[0016] 2) The catalyst Cr of the present invention x O y -NiFe-LDH / NF heterostructure has good OER catalytic selectivity and HER catalytic activity, corrosion resistance and stability in chloride ion-containing electrolytes, which has obvious advantages over precious metal catalysts. Description of the drawings:

[0017] Figure 1 The Cr obtained in Example 1 is x O y -SEM image of NiFe-LDH / NF (left) and Cr obtained in Example 1 x O y -Transmission electron microscopy image (middle) and high-resolution transmission electron microscopy image (right) of NiFe-LDH / NF.

[0018] Figure 2 Cr obtained in Example 1 x O y -XPS full spectra of NiFe-LDH / NF and NiFe-LDH / NF obtained in Comparative Example 1, including Ni 2p spectrum, Fe 2p spectrum, O 1s spectrum and Cr 2p spectrum.

[0019] Figure 3 OER linear sweep voltammograms of catalysts obtained at different electrodeposition times: Examples 1-3 and Comparative Example 1 in 0.5M NaCl+1M KOH electrolyte.

[0020] Figure 4OER linear sweep voltammograms of catalysts obtained with different Cr(NO3)3·9H2O solution concentrations: Example 1 and Examples 4-6 in 0.5M NaCl+1M KOH electrolyte.

[0021] Figure 5 OER linear sweep voltammograms of the catalysts obtained at different electrodeposition potentials: Example 1 and Examples 7-9 in 0.5M NaCl+1M KOH electrolyte.

[0022] Figure 6 Cr obtained in Example 1 x O y -OER linear sweep voltammogram of NiFe-LDH / NF, NiFe-LDH / NF obtained in Comparative Example 1 and nickel foam in 0.5MNaCl+1M KOH (a) and OER linear sweep voltammogram of NiFe-LDH / NF in 1M KOH (b).

[0023] Figure 7 Cr obtained in Example 1 x O y -Constant voltage it test graph of NiFe-LDH / NF in 0.5M NaCl+1M KOH (a) and constant voltage it test graph in 1M KOH (b).

[0024] Figure 8 Cr obtained in Example 1 x O y -NiFe-LDH / NF, HER linear sweep voltammogram of NiFe-LDH / NF and nickel foam obtained in Comparative Example 1 in 0.5MNaCl+1M KOH (a) and HER linear sweep voltammogram in 1M KOH (b).

[0025] Fig. 9 Cr obtained in Example 1 x O y -Constant voltage it test diagram of NiFe-LDH / NF in 0.5M NaCl+1M KOH (a) and constant voltage it test diagram in 1M KOH (b), and the linear scanning voltammetry curve of the two-electrode electrolytic cell composed of anode and cathode to completely split water in 0.5M NaCl+1M KOH and 1M KOH electrolytes respectively (c). Specific implementation method:

[0026] For a further understanding of the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments, but the present invention is not limited in any way.

[0027] Embodiment 1:

[0028] (a) Preparation of NiFe-LDH / NF

[0029] Specification: 2×3cm 2 The nickel foam was ultrasonically treated with 3 mol / L hydrochloric acid solution, ethanol and deionized water for 20, 10 and 10 min respectively, and dried at 60°C for 6 h; 0.2908 g Ni(NO3)2·6H2O (nickel nitrate hexahydrate), 0.2020 g Fe(NO3)2·9H2O (iron nitrate nonahydrate) and 0.3003 g CH4N2O (urea) were weighed at room temperature, dispersed in 30 mL deionized water, and stirred to form a transparent light yellow uniform solution; a piece of nickel foam was immersed in a polytetrafluoroethylene autoclave containing 30 ml of the mixed solution, hydrothermally treated at 120°C for 12 h, naturally cooled to room temperature, washed with deionized water and dried at 50°C for 6 h to obtain a brown-yellow catalyst NiFe-LDH / NF;

[0030] (b)Cr x O y Preparation of NiFe-LDH / NF

[0031] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 6 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -1.0 V and a deposition time of 900 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain Cr x O y -NiFe-LDH / NF heterostructure.

[0032] Embodiment 2:

[0033] (a) Preparation of NiFe-LDH / NF

[0034] Prepared according to the method and conditions of step (a) in Example 1;

[0035] (b)Cr x O y Preparation of NiFe-LDH / NF-600

[0036] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 6 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed under the conditions of a voltage of -1.0 V and a deposition time of 600 s to grow Cr on its surface. xO y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-600;

[0037] Embodiment 3:

[0038] (a) Preparation of NiFe-LDH / NF

[0039] Prepared according to the method and conditions of step (a) in Example 1;

[0040] (b)Cr x O y Preparation of NiFe-LDH / NF-1800

[0041] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 6 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -1.0 V and a deposition time of 1800 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-1800;

[0042] Example 4

[0043] (a) Preparation of NiFe-LDH / NF

[0044] Prepared according to the method and conditions of step (a) in Example 1;

[0045] (b)Cr x O y Preparation of NiFe-LDH / NF-3

[0046] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 3 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -1.0 V and a deposition time of 900 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-3;

[0047] Embodiment 5:

[0048] (a) Preparation of NiFe-LDH / NF

[0049] Prepared according to the method and conditions of step (a) in Example 1;

[0050] (b)Cr x O y Preparation of NiFe-LDH / NF-9

[0051] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 9 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -1.0 V and a deposition time of 900 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-9;

[0052] Embodiment 6:

[0053] (a) Preparation of NiFe-LDH / NF

[0054] Prepared according to the method and conditions of step (a) in Example 1;

[0055] (b)Cr x O y Preparation of NiFe-LDH / NF-12

[0056] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 12 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -1.0 V and a deposition time of 900 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-12;

[0057] Embodiment 7:

[0058] (a) Preparation of NiFe-LDH / NF

[0059] Prepared according to the method and conditions of step (a) in Example 1;

[0060] (b)Cr x O y Preparation of NiFe-LDH / NF-0.9

[0061] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 6 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -0.9 V and a deposition time of 900 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-0.9;

[0062] Embodiment 8:

[0063] (a) Preparation of NiFe-LDH / NF

[0064] Prepared according to the method and conditions of step (a) in Example 1;

[0065] (b)Cr x O y Preparation of NiFe-LDH / NF-1.1

[0066] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 6 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -1.1 V and a deposition time of 900 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-1.1;

[0067] Embodiment 9:

[0068] (a) Preparation of NiFe-LDH / NF

[0069] Prepared according to the method and conditions of step (a) in Example 1;

[0070] (b)Cr x O y Preparation of NiFe-LDH / NF-1.2

[0071] In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 6 mM Cr(NO3)3·9H2O solution was used as an electrolyte, and constant potential deposition was performed at a voltage of -1.2 V and a deposition time of 900 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain heterogeneous structure Cr x O y -NiFe-LDH / NF-1.2;

[0072] Comparative Example 1:

[0073] (a) Preparation of NiFe-LDH / NF

[0074] Prepared according to the method and conditions of step (a) in Example 1;

[0075] Figure 1 The Cr obtained in Example 1 is x O y -SEM image of NiFe-LDH / NF (left), Cr obtained in Example 1 x O y -NiFe-LDH / NF transmission electron microscopy (middle) and high-resolution transmission electron microscopy (right). As can be seen from the left figure, Cr x O y -NiFe-LDH presents a distinct sheet structure with good crystallinity. The nanosheets are assembled in situ on the nickel foam substrate in a flower-like shape. The thickness of the nanosheets is 10-30 nm, and the surface has a certain degree of roughness, which may be the Cr generated by electrodeposition. x O y Nanoparticles. From the transmission electron microscope image, it is obvious that the flaky structure and the particle size of Cr are less than 10nm x O y The nanoparticles are densely assembled on the LDH nanosheets (middle), indicating that the catalyst has a two-phase heterogeneous structure after electrodeposition, and high-resolution transmission electron microscopy shows that there is a rich phase interface between the two phases (right). This structure is beneficial to the OER catalytic performance and stability.

[0076] Figure 2 Cr obtained in Example 1 x O y -XPS graph (a), Ni 2p spectrum (b), Fe 2p spectrum (c), O 1s spectrum (d) and Cr 2p spectrum (e) of NiFe-LDH / NF and NiFe-LDH / NF obtained in Comparative Example 1. Figure (a) is the total element spectrum of the two materials, Cr x Oy -NiFe-LDH / NF catalyst contains Ni, Fe, Cr, C, N and O elements with contents of 6.87at.%, 4.88at.%, 2.12at.%, 36.53at.%, 9.88at.%, and 39.73at.%, respectively. Ni 2p shows that both catalysts have Ni at about 853.45eV and 871.1eV. 3+ and Ni 2+ The introduction of Cr species has basically not changed the valence state of Ni. The Fe2p spectrum shows that there is Fe at 718.95eV. 3+ The peak area of ​​the component is slightly larger than that of the Fe 2+ Compared with NiFe-LDH / NF, Cr x O y -Ni in NiFe-LDH / NF 2+ The proportion of Cr x O y -The peak of NiFe-LDH / NF moves toward the low binding energy direction, proving that the electron cloud density around the iron element in the electrodeposited NiFe-LDH / NF increases, and electrons flow from other elements to the iron element, indicating that electrons are rearranged inside the material during the electrodeposition process. x O y -The main forms of O in NiFe-LDH / NF are metal oxide MO and lattice oxygen. Among them, the fitting peak at 530.10eV corresponds to the existence of lattice oxygen, and the fitting peak at 528.70eV corresponds to the existence of metal oxide. The formation of lattice oxygen indicates that there are some oxygen vacancies in the target catalyst, which is beneficial to increase the active specific surface area of ​​the material, expose more active sites, and help to regulate the electronic structure and improve the catalytic activity of the product. Compared with NiFe-LDH / NF that has not been electrodeposited, the obvious change in the peak area corresponding to the metal oxide indicates that its content and proportion have increased significantly after the electrodeposition process, which can prove that the electrodeposition has successfully wrapped the metal oxide on the nickel-iron hydrotalcite grown in situ on the nickel foam, which is beneficial to the improvement of the overall catalytic activity of the target catalyst and the enhancement of corrosion resistance and stability in chlorine-containing alkaline solutions. The peaks of 576.7 and 578.1eV in the Cr 2p spectrum correspond to Cr 2p 3 / 2 Cr 3+ -O and Cr 3+ -OH, the peaks at 586.5 and 589.2 eV belong to Cr 2p 1 / 2and its satellite peaks, demonstrating that Cr species were assembled onto the NiFe-LDH surface in the form of oxides and hydroxides.

[0077] Figure 3-5 The OER linear sweep voltammetry curves of the catalysts obtained under different electrodeposition times, different Cr(NO3)3·9H2O solution concentrations and different electrodeposition potentials in 0.5M NaCl+1M KOH electrolyte are shown in the figure. It can be seen that when the electrodeposition time is 900 seconds, the concentration of the electrodeposition electrolyte solution is 9mM and the electrodeposition potential is -1.0V, the Cr x O y -NiFe-LDH / NF catalyst has the best OER catalytic performance in 0.5M NaCl+1M KOH electrolyte.

[0078] Figure 6 Cr obtained in Example 1 x O y -NiFe-LDH / NF, NiFe-LDH / NF obtained in Comparative Example 1 and nickel foam in 0.5MNaCl+1M KOH at a scan rate of 5mV / s (a) and OER linear scan voltammetry curve in 1M KOH (b). As can be seen from Figure (a), the current density reaches 10mA / cm 2 and 100mA / cm 2 When Cr x O y -NiFe-LDH / NF catalyst has overpotentials of 1.440 and 1.462 V in the two media, which are both lower than the overpotentials of 1.528 and 1.470 V corresponding to NiFe-LDH / NF, indicating that the electrodeposited Cr x O y The layer plays a synergistic role in promoting the OER performance of the catalyst, promoting the migration of electrons, improving the properties of the catalyst surface, and enhancing the catalytic performance.

[0079] Figure 7 Cr obtained in Example 1 x O y - NiFe-LDH / NF constant voltage it test graph in 0.5M NaCl+1M KOH (a) and constant voltage it test graph in 1M KOH (b). Cr x O y -NiFe-LDH / NF underwent 12 h of OER stability test in two media, and the catalytic performance did not show obvious attenuation, indicating that the catalyst has excellent long-term stability.

[0080] Figure 8 Cr obtained in Example 1 xO y -NiFe-LDH / NF, HER linear sweep voltammetry curves of NiFe-LDH / NF and nickel foam obtained in comparative example 1 in 0.5MNaCl+1M KOH (a) and HER linear sweep voltammetry curves in 1M KOH (b). It can be seen from the figure that the current density reaches 10mA / cm 2 When Cr x O y -NiFe-LDH / NF catalyst showed significantly better electrocatalytic performance than the other two materials in both media, i.e., it had the lowest overpotential, which indicates that the presence of the electrodeposition layer also promotes the HER performance of the catalyst, not only improving the properties of the catalyst surface, but also improving the catalytic performance.

[0081] Fig. 9 Cr obtained in Example 1 x O y -NiFe-LDH / NF constant voltage it test graph in 0.5M NaCl+1M KOH (a) and constant voltage it test graph in 1M KOH (b), and the linear scanning voltammetric curve of the two-electrode electrolytic cell composed of anode and cathode to split water in 0.5M NaCl+1M KOH and 1M KOH electrolytes respectively (c). Target catalyst Cr x O y -NiFe-LDH / NF underwent a 12-hour stability test, and the HER catalytic performance did not show a significant attenuation, indicating that the catalyst has excellent HER long-term stability. As shown in Figure (c), when the current density reaches 10 mA / cm 2 The required electrolysis potential of the target catalyst is smaller in both media and slightly smaller in 0.5M NaCl+1M KOH than in alkaline solution, indicating that the rich phase interface of the heterostructure promotes the transfer of electrons, thereby improving the electrocatalytic performance. However, chromium oxide does not completely cover the LDH nanosheets, so the performance in chloride ion-containing electrolytes is reduced.

Claims

1. A chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure, characterized in that The composite structure is a heterogeneous structure formed by depositing chromium oxide nanoparticles on nickel-iron hydrotalcite nanosheets; the composition of the oxide coating layer in the catalyst is adjusted by changing the time, potential and concentration of electrodeposition during the preparation process; the chromium oxide nanoparticles in the composite structure are prepared by constant current technology under the conditions of optimal deposition time, current density and electrolyte concentration; the composite structure is in-situ grown on nickel foam, denoted as Cr x O y -NiFe-LDH / NF; The method for preparing the chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure is characterized by comprising the following specific steps: (a) Preparation of NiFe-LDH / NF The specification is 3*2cm 2 The nickel foam was treated with 3 mol / L hydrochloric acid solution, deionized water and ethanol by ultrasound for 20, 5 and 20 min respectively, and dried at 50°C for 6 h; 1 mmol of Ni(NO3)2·6H2O, 0.5 mmol of Fe(NO3)3·9H2O and 5 mmol of urea were weighed and dissolved in 40 mL of deionized water; the mixed solution was transferred to a 100 mL polytetrafluoroethylene reactor, and a piece of pretreated nickel foam was added to react at 120°C for 12 h. After cooling to room temperature, the nickel foam was taken out from the reactor, washed several times with deionized water and anhydrous ethanol respectively, and then dried at 50°C for 5 h to obtain NiFe-LDH / NF; (b)Cr x O y Preparation of NiFe-LDH / NF In a three-electrode system with a platinum wire electrode as a counter electrode, a HgO / Hg electrode as a reference electrode, and the NiFe-LDH / NF obtained in step (a) as a working electrode, a 3-12 mM Cr(NO3)3·9H2O solution is used as an electrolyte, and constant potential deposition is performed under the conditions of a voltage of -0.9 to -1.2 V and a deposition time of 600 to 1800 s to grow Cr on its surface. x O y The nanoparticles were rinsed repeatedly with deionized water and dried at 60 °C for 6 h to obtain Cr x O y -NiFe-LDH / NF heterostructure; The Cr particles with a diameter of less than 10 nm in the chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure x O y The nanoparticles are densely covered on the surface of NiFe-LDH nanosheets with a lateral size of 200-500 nm and a thickness of 10-30 nm. x O y There is abundant phase interface between the nanoparticles and NiFe-LDH nanosheets.

2. The chromium oxide functionalized nickel-iron hydrotalcite nanosheet composite structure according to claim 1, characterized in that The composite structure is used as a bifunctional electrocatalyst for the anode oxygen evolution reaction and the cathode hydrogen evolution reaction in the electrolysis of seawater and water.

Citation Information

Patent Citations

  • Heterostructures for ultra-active hydrogen evolution electrocatalysis

    CN106605011A

  • Preparation method of metal oxide-LDH loading catalyst

    CN109046357A

  • High-stability alkaline solution hydrogen evolution electrocatalyst as well as preparation method and application thereof

    CN114395765A

  • Facile formation of highly active and stable hydrogen evolution catalysts

    US20200407861A1

  • Trimetallic layered double hydroxide composition

    US20220002887A1