Optical fiber sensor manufacturing method based on MnO2 / ZnO composite film and sensor and DMMP gas concentration detection method
Through the optical fiber sensor technology based on MnO2/ZnO composite film, the problem of insufficient portable remote sensing monitoring and anti-interference capabilities in the prior art is solved, and high sensitivity detection of DMMP gas is realized, which is of great significance and application in the field of nerve agent detection. potential.
Patent Information
- Application Number
- CN202210939708.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-08-05
AI Technical Summary
The prior art is difficult to provide a portable, microstructure remote sensing monitoring high-sensitivity sensor for detecting low-concentration sarin gas simulant DMMP, and there is a problem of insufficient anti-interference ability.
Using the optical fiber sensor production method based on MnO2/ZnO composite film, the composite film layer is formed by welding and silver film coating of single-mode and multi-core optical fibers, combined with the preparation of MnO2/ZnO sensitive materials, and the composite film layer is formed to achieve high sensitivity to DMMP gas concentration. Test.
It realizes sensors with strong anti-interference, high sensitivity and fast response time, which can provide high sensitivity and selectivity in the field of nerve agent detection, and has significant application potential.
Smart Images

Figure CN115308134B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sensors, and in particular to a method for manufacturing an optical fiber sensor based on a MnO2 / ZnO composite film and a method for detecting the concentration of a sensor and DMMP gas. Background Art
[0002] Sarin is an organophosphorus G-type nerve agent. Due to its colorless, odorless and highly toxic characteristics, it is listed as a weapon of mass destruction by UN Resolution 687. Studies have found that low concentrations of sarin aerosol (0.5ppb) can cause pupil constriction, difficulty seeing in the dark, chest tightness, headache and nausea within 2 minutes. The toxicity will accumulate in the body, and at higher concentrations it can cause dizziness, mental damage, muscle spasms, breathing difficulties, and even death. Within 10 minutes, the disability and lethality of sarin occurred at 15ppb and 64ppb and above, respectively. Therefore, it is very necessary to develop a highly sensitive sensor that can monitor sarin gas in real time.
[0003] Sarin is extremely toxic and difficult to handle directly in the laboratory. Since non-toxic dimethyl methylphosphonate (DMMP) has a similar chemical structure to sarin, it has become a recognized sarin gas simulant. The detection methods of DMMP, a sarin gas simulant, mainly include gas chromatography-mass spectrometry, enzyme-based biosensors, chemical resistors / capacitors, microcantilever beams, and quartz crystal microbalance sensors. In 2015, an electrochemical sensor composed of single-walled nanotubes and polyaniline was proposed to detect the nerve agent simulant DMMP at room temperature. At 10ppm DMMP, the response amount and response time were 27.1% and 5.5s, respectively. In 2018, a domestic laboratory made a sensor for DMMP, a sarin simulant, based on a wireless electrodeless quartz crystal microbalance, and realized the dynamic observation of DMMP concentration changes. In 2020, a new multifunctional fluorescent probe was developed that can achieve high sensitivity and selective rapid identification of DMMP molecules. Although these detection methods have obtained meaningful detection results in high sensitivity and fast response detection, they are difficult to meet the needs of portable and microstructure remote sensing monitoring. Compared with the above detection technologies, the sensing technology using optical fiber as the transmission medium not only has the advantages of anti-electromagnetic interference and high-precision detection, but also has the advantages of miniaturization, easy integration, and suitability for remote sensing monitoring. In recent years, with the rapid development of optical fiber sensing technology and functional materials, optical fiber sensors have shown great potential in the measurement of trace nerve gas. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the technical problem to be solved by the present invention is: how to provide a method for manufacturing an optical fiber sensor based on a MnO2 / ZnO composite film, which is easy to manufacture and has strong anti-interference ability, high detection accuracy and sensitivity, and fast response time.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A method for preparing an optical fiber sensor based on a MnO2 / ZnO composite film comprises the following steps: obtaining a single-mode optical fiber and a multi-core optical fiber, fusing one end of the single-mode optical fiber with one end of the multi-core optical fiber to form a coarse cone structure, and coating a silver film on one end of the multi-core optical fiber away from the single-mode optical fiber; then obtaining a MnO2 / ZnO sensitive material, dispersing it evenly in deionized water to obtain a MnO2 / ZnO dispersion, then immersing the multi-core optical fiber in the MnO2 / ZnO dispersion, taking it out and drying it to a constant weight, forming a MnO2 / ZnO composite film layer on the surface of the multi-core optical fiber, and thus preparing the optical fiber sensor.
[0007] As an optimization, a coreless optical fiber is obtained, one end of the coreless optical fiber is fused with an end of the multi-core optical fiber away from the single-mode optical fiber, and then a silver film is coated on the end of the coreless optical fiber away from the multi-core optical fiber.
[0008] As an optimization, the preparation method of the MnO2 / ZnO sensitive material is as follows: manganese sulfate and potassium permanganate in a mass ratio of (2-5) : (1-2) are dissolved in deionized water, and the obtained solution is placed at a temperature of 120-140°C and a pressure of 190-220 kPa for reaction. After the reaction is completed, the filtered solid product is washed with deionized water and dried to constant weight to obtain manganese dioxide nanowires; manganese dioxide nanowires are added to deionized water, stirred to make them uniformly dispersed, and then continuously stirred, and zinc nitrate and hexamethylenetetramine are added during the stirring process, wherein the mass ratio of manganese dioxide nanowires, zinc nitrate and hexamethylenetetramine is (2-3) : (1-3) : (1-3), after mixing evenly, ammonia water is added to the mixed solution to adjust the pH value to 8-10, and then the mixed solution is placed at a temperature of 90-95°C for reaction. After the reaction is completed, the filtered solid product is washed with deionized water and dried to constant weight to obtain the MnO2 / ZnO sensitive material.
[0009] As an optimization, the thickness of the MnO2 / ZnO composite film layer is 440-690 nm.
[0010] A DMMP sensor is made by any one of the above-mentioned methods for making an optical fiber sensor based on the interference structure of a MnO2 / ZnO composite film.
[0011] A method for detecting DMMP gas concentration comprises the following steps:
[0012] (1) obtaining the above-mentioned DMMP sensor, connecting one end of the single-mode optical fiber in the DMMP sensor away from the multi-core optical fiber to a circulator, connecting a light source and a spectrometer to the circulator, and obtaining a spectrum in the absence of DMMP gas;
[0013] (2) preparing a plurality of DMMP gases of different concentrations and placing them in different gas chambers;
[0014] (3) placing the DMMP sensor in step (1) into each gas chamber in step (2) respectively, and recording the spectra of the DMMP sensor under different DMMP gas concentrations;
[0015] (4) Select a trough in the spectrum in step (1), record the central wavelength of the trough and the corresponding trough interference intensity, and select a trough near the corresponding central wavelength in the spectrum of DMMP gas with different concentrations in step (3), respectively record the interference intensity corresponding to each trough, and obtain y=a+bx through linear fitting, with a linearity of 0.97308, that is, x=(ya) / b, where y is the interference intensity of the trough in the DMMP gas chamber detection spectrum, a is the interference intensity of the trough in the detection spectrum without DMMP gas, b is the interference intensity offset of each 1ppm DMMP gas in the spectrum, and x is the concentration of DMMP gas;
[0016] (5) Place the DMMP sensor in step (1) into the gas chamber to be detected and obtain the detection spectrum of the gas chamber, select the interference intensity of the corresponding trough in step (4), and substitute it into the formula x=(ya) / b to obtain the concentration of DMMP gas.
[0017] When the light input into the single-mode fiber enters the coarse cone, the optical signal diverges, with one part entering the core of the multi-core fiber and the other part entering the cladding of the multi-core fiber. The two optical signals are reflected at the silver film on the end face of the sensor, converge after returning to the coarse cone, and enter the spectrum analyzer through the single-mode fiber; after the two optical signals enter the coreless fiber, they excite the high-order mode of the coreless fiber and propagate in the high-order mode. When the light is transmitted from the core of the single-mode fiber to the coarse cone, it is difficult to completely diverge the light in the core to each core and cladding of the multi-core fiber, but after it continues to transmit and is reflected by the end face of the coreless fiber, it will enter the core and cladding of the multi-core fiber again, resulting in an optical path difference and interference. The existence of the coreless fiber will greatly increase the intensity of the interference spectrum. Due to the optical path difference between the core mode and the cladding mode of the multi-core fiber, when the two optical signals are coupled into the single-mode fiber again, interference occurs, which appears as peaks and troughs on the spectrum. The interference light intensity can be expressed as:
[0018]
[0019] Among them, Icore represents the core light intensity, represents the mth order light intensity of the cladding, φ m Represents the phase difference between the core light intensity and the m-th order light intensity of the cladding, R represents the reflectivity of the coreless optical fiber end face, and the formula of R is as follows:
[0020]
[0021] Among them, n core is the effective refractive index of the coreless optical fiber core, n is the effective refractive index of the medium around the end face of the coreless optical fiber, and after the end face is coated with silver film, R becomes a constant.
[0022] φ m Represents the phase difference between the core light intensity and the m-th order light intensity of the cladding, which can be defined as:
[0023]
[0024] in and represent the effective refractive index of the core and cladding of the multi-core optical fiber, L represents the effective length of the sensor, and λ m represents the wavelength of the mth-order incident light, Δn eff is the effective refractive index difference between the core and cladding of a multi-core optical fiber. m =2(m+1)π, the interference destructive condition is met, and an interference trough is generated. When the multi-core optical fiber area is coated with MnO2 / ZnO composite material, the cladding and sensitive film coating of the multi-core optical fiber are equivalent to a new cladding. After the adsorption of DMMP molecules, the cladding mode light intensity in the optical fiber transmission will change, and the evanescent field energy radiated outward will decrease, resulting in the cladding mode Increased, but the core mode I core The light intensity of the sensor will increase, and the desorption of DMMP is a reverse process. The concentration of DMMP in the gas chamber can be determined by monitoring the changes in the light intensity of the reflectance spectrum.
[0025] Compared with the prior art, the present invention has the following beneficial effects: the sensor produced by the present invention has the advantages of strong anti-interference, high sensitivity, remote measurement, simple operation, etc., and has great significance and application potential in the field of high-sensitivity detection of nerve agents. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a linear fitting diagram of the sensor in the present invention for the offset near the wavelength of 1580nm and the measured gas concentration in the range of DMMP gas concentration of 0-30ppm;
[0027] Figure 2The detection spectra of DMMP gas with concentrations of 0ppm, 5ppm, 10ppm and 15ppm in the present invention correspond to the wavelengths corresponding to the troughs in the range of 1580nm to 1584nm;
[0028] Figure 3 The detection spectra of DMMP gas with a concentration of 20ppm, 25ppm and 30ppm in the present invention correspond to the wavelength of the trough corresponding to 1580nm to 1584nm;
[0029] Figure 4 This is the response-recovery diagram of the sensor in the present invention under 30ppm concentration of DMMP gas;
[0030] Figure 5 This is a graph showing the light intensity changes of the sensor under different gases in the present invention;
[0031] Figure 6 The dispersion diagram of the light intensity variation of the valley near the wavelength of 1580nm monitored by the sensor in the present invention between 30-80°C;
[0032] Figure 7 This is a dispersion diagram of the change in the light intensity of the valley near the wavelength of 1580nm monitored by the sensor in the present invention at different humidity levels;
[0033] Figure 8 It is a dispersion point diagram of the variation of the light intensity of the valley near the wavelength of 1580nm monitored by the sensor of the present invention over time. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. The components of the embodiments of the present invention generally described and shown in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.
[0035] The method for making an optical fiber sensor based on a MnO2 / ZnO composite film in this specific embodiment comprises the following steps: obtaining a single-mode optical fiber and a four-core optical fiber, fusing one end of the single-mode optical fiber with one end of the four-core optical fiber to form a coarse cone structure, and coating a silver film on one end of the four-core optical fiber away from the single-mode optical fiber; then obtaining a MnO2 / ZnO sensitive material, dispersing it evenly in deionized water to obtain a MnO2 / ZnO dispersion, and then immersing the four-core optical fiber in the MnO2 / ZnO dispersion, taking it out and drying it to constant weight, forming a MnO2 / ZnO composite film layer on the surface of the four-core optical fiber, and thus obtaining a optical fiber sensor.
[0036] In this specific implementation, a coreless optical fiber is obtained, one end of the coreless optical fiber is fused with an end of a four-core optical fiber away from the single-mode optical fiber, and then a silver film is plated on the end of the coreless optical fiber away from the four-core optical fiber.
[0037] In this specific embodiment, the preparation method of the MnO2 / ZnO sensitive material is as follows: manganese sulfate and potassium permanganate in a mass ratio of 2:1 are dissolved in deionized water, and the obtained solution is placed at a temperature of 120°C and a pressure of 200 kPa for reaction. After the reaction is completed, the filtered solid product is washed clean with deionized water and dried to constant weight to obtain manganese dioxide nanowires; manganese dioxide nanowires are added to deionized water, stirred to make them evenly dispersed, and then continuously stirred, and zinc nitrate and hexamethylenetetramine are added during the stirring process, wherein the mass ratio of manganese dioxide nanowires, zinc nitrate and hexamethylenetetramine is 1:1:1. After mixing evenly, ammonia water is added to the mixed solution to adjust the pH value to 10, and then the mixed solution is placed at a temperature of 95°C for reaction. After the reaction is completed, the filtered solid product is washed clean with deionized water and dried to constant weight to obtain MnO2 / ZnO sensitive material.
[0038] In this specific implementation manner, the thickness of the MnO2 / ZnO composite film layer is 460nm.
[0039] A DMMP sensor is made by any one of the above-mentioned methods for making an optical fiber sensor based on the interference structure of a MnO2 / ZnO composite film.
[0040] A method for detecting DMMP gas concentration comprises the following steps:
[0041] (1) obtaining the above-mentioned DMMP sensor, connecting one end of the single-mode optical fiber in the DMMP sensor away from the four-core optical fiber to a circulator, connecting a light source and a spectrometer to the circulator, and obtaining a spectrum in the absence of DMMP gas;
[0042] (2) preparing a plurality of DMMP gases of different concentrations and placing them in different gas chambers;
[0043] (3) placing the DMMP sensor in step (1) into each gas chamber in step (2) respectively, and recording the spectra of the DMMP sensor under different DMMP gas concentrations;
[0044] (4) Select a trough in the spectrum in step (1), record the central wavelength of the trough and the corresponding trough interference intensity, and select a trough near the corresponding central wavelength in the spectrum of DMMP gas with different concentrations in step (3), respectively record the interference intensity corresponding to each trough, and obtain y=a+bx through linear fitting, with a linearity of 0.97308, as shown in FIG. Figure 1 As shown, that is, x = (y-a) / b, where y is the interference intensity of the trough in the DMMP gas chamber detection spectrum, a is the interference intensity of the trough in the detection spectrum without DMMP gas, b is the interference intensity offset of each 1ppm DMMP gas in the spectrum (i.e., the sensor sensitivity), and x is the concentration of DMMP gas;
[0045] (5) Place the DMMP sensor in step (1) into the gas chamber to be detected and obtain the detection spectrum of the gas chamber, select the interference intensity of the corresponding trough in step (4), and substitute it into the formula x=(ya) / b to obtain the concentration of DMMP gas.
[0046] Using N2 as diluent, DMMP gas with concentrations of 0ppm, 5ppm, 10ppm, 15ppm, 20ppm, 25ppm, and 30ppm were prepared respectively. The sensor response spectra are shown in Figure 2 and Figure 3 As shown. It can be observed that as the DMMP concentration increases, the monitored trough interference intensity continues to increase, with a maximum change of 10.24 dB. The trough intensity is linearly fitted, with a linearity of 0.97308 and a DMMP sensitivity of 0.3413 dB / ppm. The detection limit can be calculated using formula (4):
[0047]
[0048] Where σ is the standard deviation of the slope (0.0244dB), K is the sensitivity (0.3413dB / ppm), and the calculated LOD is 0.2145ppm. The sensor was tested for response recovery with 30ppm DMMP, and the results are as follows Figure 4 As shown. The response time t of the sensor to DMMP r is 180s, and the recovery time t f is 100s.
[0049] 30ppm of DMMP, hydrogen, hydrogen sulfide, oxygen, ammonia, carbon monoxide, and argon were introduced into the gas chamber, and the corresponding light intensity changes of the sensor were as follows: Figure 5The results show that the light intensity changes caused by other gases are less than 20% of the light intensity changes caused by the same concentration of DMMP, indicating that the sensor has excellent selectivity for DMMP. Figure 6 The sensor monitors the intensity variation of the light at the trough near the wavelength of 1580nm between 30-80℃, and the intensity variation caused by temperature is 1.940dB. The corresponding sensitivity is 0.0388dB / ℃, which is much lower than the sensitivity to DMMP, indicating that the sensor has good temperature stability. Figure 7 This is the sensor humidity stability test result. In the humidity range of 45%-60%, the maximum intensity change of the trough is only 0.124dB. Figure 8 The time stability test results of the sensor show that the maximum change in spectral intensity within 180 minutes is 0.176 dB, which is negligible compared to the change caused by DMMP concentration. It can be seen that the sensor has good stability in temperature, humidity and time.
[0050] The results of the sensing test show that the sensitivity of the sensor to DMMP is 0.3413dB / ppm, the response time is about 180s, and the detection limit is 0.2145ppm. Compared with common gases, the sensor has excellent selectivity for DMMP and good temperature, humidity and time stability. At present, there are no reports on the detection of trace nerve gas with sensitive membrane integrated optical fiber sensing structure. The sensor has the advantages of strong anti-interference, high sensitivity, remote sensing, and simple operation. It has great significance and application potential in the field of high-sensitivity detection of nerve agents.
[0051] Three DMMP gas samples of unknown concentration were obtained, and then the sensors were placed into the three DMMP gas samples respectively to obtain interference spectra. The trough of the interference spectrum near 1580nm was selected, and the interference intensities of the three DMMP gas samples at the trough were obtained to be -49.527dBm, -50.417dBm and -56.007dBm, respectively. Furthermore, the gas concentrations of the three DMMP gas samples were calculated to be 24ppm, 21ppm and 6ppm, respectively.
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing an optical fiber sensor based on a MnO2 / ZnO composite film, characterized in that: A single-mode optical fiber and a multi-core optical fiber are obtained, one end of the single-mode optical fiber is fused with one end of the multi-core optical fiber to form a thick cone structure, and a silver film is plated on the end of the multi-core optical fiber away from the single-mode optical fiber; then a MnO2 / ZnO sensitive material is obtained, and it is evenly dispersed in deionized water to obtain a MnO2 / ZnO dispersion liquid, and then the multi-core optical fiber is immersed in the MnO2 / ZnO dispersion liquid, taken out and dried to constant weight, and a MnO2 / ZnO composite film layer is formed on the surface of the multi-core optical fiber, so that a fiber optic sensor is prepared.
2. The method for preparing an optical fiber sensor based on a MnO2 / ZnO composite film according to claim 1, characterized in that: A coreless optical fiber is obtained, one end of the coreless optical fiber is fused with an end of the multi-core optical fiber away from the single-mode optical fiber, and then a silver film is plated on the end of the coreless optical fiber away from the multi-core optical fiber.
3. The method for preparing an optical fiber sensor based on a MnO2 / ZnO composite film according to claim 1, characterized in that: The preparation method of the MnO2 / ZnO sensitive material is as follows: dissolving manganese sulfate and potassium permanganate in a mass ratio of (2-5) : (1-2) in deionized water, placing the obtained solution at a temperature of 120-140°C and a pressure of 190-220 kPa for reaction, and after the reaction is completed, washing the filtered solid product with deionized water, and drying it to constant weight to obtain manganese dioxide nanowires; adding the manganese dioxide nanowires into deionized water, stirring to make it uniformly dispersed, and then continuously stirring, and adding zinc nitrate and hexamethylenetetramine during the stirring process, wherein the mass ratio of manganese dioxide nanowires, zinc nitrate and hexamethylenetetramine is (2-3) : (1-3) : (1-3), after mixing evenly, adding ammonia water to the mixed solution to adjust the pH value to 8-10, and then placing the mixed solution at a temperature of 90-95°C for reaction, and after the reaction is completed, washing the filtered solid product with deionized water, and drying it to constant weight to obtain the MnO2 / ZnO sensitive material.
4. The method for manufacturing an optical fiber sensor based on a MnO2 / ZnO composite film according to claim 1, characterized in that: The thickness of the MnO2 / ZnO composite film layer is 440-690nm.
5. A DMMP sensor, characterized in that: The optical fiber sensor is manufactured by the method for manufacturing an optical fiber sensor based on a MnO2 / ZnO composite film as described in any one of claims 1 to 4.
6. A method for detecting DMMP gas concentration, characterized in that: The following steps are involved: (1) obtaining the DMMP sensor of claim 5, wherein one end of the single-mode optical fiber in the DMMP sensor away from the multi-core optical fiber is connected to a circulator, a light source and a spectrometer are connected to the circulator, and a spectrum diagram in the absence of DMMP gas is obtained; (2) preparing a plurality of DMMP gases of different concentrations and placing them in different gas chambers; (3) placing the DMMP sensor in step (1) into each gas chamber in step (2), respectively, and recording spectra of the DMMP sensor under different DMMP gas concentrations; (4) Select a trough in the spectrum in step (1), record the central wavelength of the trough and the corresponding trough interference intensity, and select a trough near the corresponding central wavelength in the spectrum of DMMP gas with different concentrations in step (3), respectively record the interference intensity corresponding to each trough, and obtain y=a+bx through linear fitting, with a linearity of 0.97308, that is, x=(ya) / b, where y is the interference intensity of the trough in the DMMP gas chamber detection spectrum, a is the interference intensity of the trough in the detection spectrum without DMMP gas, b is the interference intensity offset of each 1ppm DMMP gas in the spectrum, and x is the concentration of DMMP gas; (5) Place the DMMP sensor in step (1) into the gas chamber to be detected and obtain the detection spectrum of the gas chamber, select the interference intensity of the corresponding trough in step (4), and substitute it into the formula x=(ya) / b to obtain the concentration of DMMP gas.