Soldering method for high thermal capacity through-hole components on circuit boards

Through simulation technology and thermal analysis, the welding quality problem of high-heat capacitance through-hole devices in circuit boards is solved, the welding efficiency and quality are improved, and resource waste is avoided.

CN115315094BActive Publication Date: 2024-11-22GREE ELECTRIC APPLIANCE INC OF ZHUHAI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210860326.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-21
Publication Date
2024-11-22
Estimated Expiration
2042-07-21

AI Technical Summary

Technical Problem

In circuit boards, the welding quality of high-heat capacitance through-hole devices is often affected. The existing methods rely on repeated design of templates and tests, with long cycles and poor results, making it difficult to ensure the reliability and welding quality of solder joints.

Method used

Using simulation technology to conduct thermal analysis and local welding effect evaluation of the welding process. By designing the pads, building PCBA 3D models, conducting transient thermal analysis on the ANSYS platform, adjusting simulation parameters and temperature division, temperature testing and welding optimization, ensuring The solder joints meet the process requirements.

Benefits of technology

The wave soldering efficiency of high-heat capacitance through-hole devices is improved, resource waste is avoided, and effective evaluation and optimization of solder joint quality is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115315094B_ABST
    Figure CN115315094B_ABST
Patent Text Reader

Abstract

The present application relates to a method for soldering a high thermal capacity through-hole device on a circuit board, and the specific steps are: pad design; constructing a PCBA model; importing a 3D model of a PCBA circuit board into an ANSYS platform; setting simulation parameters and rules on the ANSYS platform; performing simulation analysis on the 3D model on the ANSYS platform to determine whether the temperature in the preheating stage meets the process requirements; preparing a circuit board sample according to the constructed 3D model of the PCBA circuit board; performing a temperature test on the circuit board sample; and performing local solder joint analysis. The method analyzes the soldering process of a high thermal capacity through-hole device and uses simulation technology to achieve efficient evaluation of solder joint wave soldering effects from thermal analysis and local soldering effect analysis, thereby achieving wave soldering of high thermal capacity through-hole devices, improving work efficiency, and avoiding a large amount of waste of time, money and other resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of circuit board manufacturing, and in particular to a method for welding high heat capacity through-hole devices of a circuit board. Background Art

[0002] Through-hole devices on circuit boards are mainly welded by wave soldering to achieve lead-free solder joints. Among through-hole devices, there are some components with large volume and large pin size (such as chokes, large capacitors, large inductors, etc.). These devices also have relatively large thermal capacity and often have welding quality problems. With so many components, how to ensure the reliability of the device itself and the quality of solder joints has become a major problem. At present, the conventional practice is to design different samples and conduct repeated welding tests, which has a long test cycle and poor improvement effect. Summary of the invention

[0003] The purpose of the present invention is to provide a method for welding high thermal capacity through-hole components of a circuit board in view of the above shortcomings.

[0004] A technical solution adopted by the present invention to solve the technical problem is to provide a method for welding a high thermal capacity through-hole device of a circuit board, comprising the following steps:

[0005] S1: Pad design: Design the pad according to the circuit board configuration and the required high thermal capacity components;

[0006] S2: Build PCBA model: Build the 3D model of the PCBA circuit board according to the circuit board configuration, PCB design drawings and component layout;

[0007] S3: Import the 3D model of the PCBA circuit board into the ANSYS platform;

[0008] S4: Set simulation parameters and rules on the ANSYS platform;

[0009] S5: On the ANSYS platform, a transient thermal analysis model of the PCBA wave soldering process is established, and simulation analysis is performed to obtain the heat distribution and temperature change of the entire board during the wave soldering process, and to determine whether the temperature in the preheating stage meets the process requirements;

[0010] S5.1, if it meets the process requirements, proceed to S6;

[0011] S5.2, if it does not meet the process requirements, return to S4 to adjust the setting parameters;

[0012] S6: preparing circuit board samples according to the constructed 3D model of the PCBA circuit board;

[0013] S7: Conduct temperature test on the circuit board sample, and judge whether the preheating and welding requirements are met according to the test temperature curve obtained at the temperature measurement point;

[0014] S7.1, if the requirements are not met, return to step S1 and redesign;

[0015] S7.2, if the requirements are met, proceed to step S8;

[0016] S8: Local solder joint analysis: Perform wave soldering on the circuit board sample, and after completion, perform appearance inspection and slice observation on the high thermal capacity through-hole device solder joints to determine whether the solder joint assembly appearance meets the tin penetration height requirements for through-hole device solder joints in the IPC-A-610E standard;

[0017] S8.1, if the requirements are not met, return to step S1 and redesign;

[0018] S8.2, if the requirements are met, complete the soldering of the high thermal capacity through-hole device on the circuit board.

[0019] Furthermore, in step S1, the pad is designed as a heat-concentrating pad, and a plurality of metallized holes are arranged between the plug-in hole and the heat-concentrating hole, and the metallized holes are evenly distributed around the plug-in hole.

[0020] Furthermore, in step S3, the 3D model is partitioned into hexahedral structured grids using a sweep partitioning method on the ANSYS platform;

[0021] In step S3, the 3D model features need to be simplified, and the THT component pins, component shapes, and PCB body need to be block-processed.

[0022] Further, in step S4, the simulation parameter setting is to divide the temperature zones of the preheating section and the welding section of the wave soldering according to the wave soldering structure and the thermal analysis requirements, and divide the preheating section into the first preheating section, the second preheating section, and the third preheating section along the welding conveying direction, and set the area between the preheating section and the welding section as the transition zone, simplify the welding section to a fixed heat source treatment, and set it as the welding zone, and the output side of the welding section is set as the cooling zone;

[0023] In step S4, convection boundary conditions are set at the bottom and top of the first preheating zone, the second preheating zone, the third preheating zone, the transition zone, and the cooling zone; the bottom of the welding zone adopts a temperature boundary condition, and the top adopts a convection boundary condition.

[0024] Furthermore, in step S4, the rule setting is to implement load step loading in a specific area and at a specific time. In convective heat transfer, loading in other time periods is suppressed according to the temperature settings of each section. Unnecessary time periods are selected for suppression operations. The suppressed load steps will not load the corresponding boundary conditions; otherwise, the activated load steps can be loaded normally.

[0025] Further, in step S5, the process requirement is that the PCBA circuit board temperature is between 90-125°C for not less than 20 seconds, and the temperature of the high-temperature container solder joint is greater than 85°C in the preheating section;

[0026] In step S5.2, the parameters that need to be adjusted are the temperature of each temperature zone and the conveyor chain speed. If the temperature is too low / too high, the temperature of the corresponding temperature zone is gradually increased / decreased with a gradient of 5°C; if the duration is too low, the conveyor chain speed is correspondingly reduced.

[0027] Furthermore, in step S7, during the temperature test, the wave soldering parameter settings refer to the simulation parameter settings, and a K-type thermocouple is used to test the temperature of high heat capacity solder joints to complete the actual temperature test of the circuit board.

[0028] Furthermore, in step S7, the number of points is no less than 3, and the temperature measurement points must include 1 high thermal capacity component pin solder point, 1 bottom chip resistor / capacitor solder point, and 1 QFP / SOP / SOJ solder point; after the points are arranged, the K-shaped thermocouple is connected to the temperature recorder, and the furnace temperature setting parameters are set according to the simulation results to complete the PCBA temperature test record.

[0029] Further, in step S7, the preheating requirement is that the temperature measured at the temperature measuring point in the preheating section is between 90°C and 125°C for a duration of not less than 20 seconds, and the temperature of the high-temperature container welding point in the preheating section is greater than 85°C;

[0030] In step S7, welding requires that the temperature measured at the temperature measuring point of the welding section is 260±5°C and the duration at this temperature is 3-5s.

[0031] Furthermore, in steps S7.1 and S8.1, the redesigned parameters are the number of heat focusing holes and the size of the heat focusing holes. The diameter of the heat focusing holes is gradually increased / decreased by 0.2 mm according to the high / low measured temperature.

[0032] Compared with the prior art, the present invention has the following beneficial effects: by analyzing the welding process of high thermal capacity through-hole devices and using simulation technology, efficient evaluation of solder joint wave soldering effects is achieved from thermal analysis and local welding effect analysis, thus wave soldering of high thermal capacity through-hole devices is achieved, work efficiency is improved, and a large amount of waste of time, money and other resources is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention is further described below in conjunction with the accompanying drawings.

[0034] Figure 1 Schematic diagram of the process of this method.

[0035] Figure 2 This is a simplified model diagram of PCBA.

[0036] Figure 3 Schematic diagram of model meshing.

[0037] Figure 4 This is a schematic diagram of temperature zones.

[0038] Figure 5 Design schematic for pad.

[0039] Figure 6 This is the overall temperature time history diagram of PCBA.

[0040] Figure 7 Temperature distribution on the PCBA surface at 4.4s.

[0041] Figure 8 Temperature distribution on the bottom of the PCBA board at 4.4s.

[0042] Fig. 9 The PCBA board surface temperature distribution at 38.4s.

[0043] Fig.10 Temperature distribution on the bottom of the PCBA board at 38.4s.

[0044] Fig.11 The PCBA board surface temperature distribution at 133.05s.

[0045] Fig.12 Temperature distribution on the bottom of the PCBA board at 133.05s.

[0046] Fig.13 Temperature distribution of CBA board surface at 135.64s.

[0047] Fig.14 Temperature distribution on the bottom of the PCBA board at 135.64s. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0049] Embodiment 1:

[0050] like Figure 1 As shown, a method for soldering a high thermal capacity through-hole device on a circuit board comprises the following steps:

[0051] S1: Pad design: Design the pad according to the circuit board configuration and the required high thermal capacity components;

[0052] S2: Build PCBA model: Build the 3D model of the PCBA circuit board according to the circuit board configuration, PCB design drawings and component layout;

[0053] In practical applications, the layout must meet the circuit arrangement requirements and process requirements; considering the large thermal capacity of components, in principle, components should not be too concentrated to prevent excessive temperature differences during the welding process. Other component layout requirements should be adjusted according to the actual welding situation;

[0054] S3: Import the 3D model of the PCBA circuit board into the ANSYS platform;

[0055] S4: Set simulation parameters and rules on the ANSYS platform;

[0056] S5: On the ANSYS platform, a transient thermal analysis model of the PCBA wave soldering process is established, and simulation analysis is performed to obtain the heat distribution and temperature change of the entire board during the wave soldering process, and to determine whether the temperature in the preheating stage meets the process requirements;

[0057] S5.1, if it meets the process requirements, proceed to S6;

[0058] S5.2, if it does not meet the process requirements, return to S4 to adjust the setting parameters;

[0059] S6: preparing circuit board samples according to the constructed 3D model of the PCBA circuit board;

[0060] S7: Conduct temperature test on the circuit board sample, test the temperature of the high heat capacity solder joint, complete the actual temperature test of the circuit board, and judge whether the preheating and welding requirements are met according to the test temperature curve obtained at the temperature measurement point;

[0061] S7.1, if the requirements are not met, return to step S1 and redesign;

[0062] S7.2, if the requirements are met, proceed to step S8;

[0063] S8: Local solder joint analysis: Perform wave soldering on the circuit board sample, and after completion, perform appearance inspection and slice observation on the high thermal capacity through-hole device solder joints to determine whether the solder joint assembly appearance meets the tin penetration height requirements for through-hole device solder joints in the IPC-A-610E standard;

[0064] S8.1, if the requirements are not met, return to step S1 and redesign;

[0065] S8.2, if the requirements are met, complete the soldering of the high thermal capacity through-hole device on the circuit board.

[0066] In this embodiment, if Figure 5 As shown, in step S1, the pad adopts a heat-concentrating pad design, and a plurality of metallized holes 2 are arranged between the plug-in hole 3 and the heat-concentrating hole 1, and the metallized holes are evenly distributed around the plug-in hole.

[0067] In this embodiment, if Figure 2 , 3 In step S3, the 3D model is divided into hexahedral structured grids using the sweep partitioning method on the ANSYS platform to ensure calculation accuracy and improve calculation speed;

[0068] In step S3, PCBA involves a large number of components, so the 3D model features need to be simplified and the THT component pins, component shapes, and PCB body need to be block-processed.

[0069] In this embodiment, if Figure 4 As shown, in step S4, the simulation parameter setting is based on the wave soldering structure and thermal analysis requirements, the preheating section and the welding section of the wave soldering are divided into temperature zones, the preheating section is divided into a first preheating zone 4, a second preheating zone 5, and a third preheating zone 6 along the welding conveying direction, the area between the preheating section and the welding section is set as a transition zone 7, the welding section is simplified to a fixed heat source treatment and is set as a welding zone 8, and the output side of the welding section is set as a cooling zone 9;

[0070] In step S4, convection boundary conditions are set at the bottom and top of the first preheating zone, the second preheating zone, the third preheating zone, the transition zone, and the cooling zone; the bottom of the welding zone adopts a temperature boundary condition, and the top adopts a convection boundary condition.

[0071] In this embodiment, in order to achieve separate loading of the temperature of each area at a fixed time without interfering with each other, in step S4, the rule setting is to achieve load step loading in a specific area and at a specific time. In the convective heat transfer, the loading of other time periods is suppressed according to the temperature settings of each section, and unnecessary time periods are selected for suppression operation. The suppressed load step will not load the corresponding boundary conditions; otherwise, the activated load step can be loaded normally.

[0072] In this embodiment, in step S5, the process requirement is that the PCBA circuit board temperature is between 90°C and 125°C for not less than 20 seconds, and the temperature of the high-temperature container solder joint is greater than 85°C in the preheating stage;

[0073] In step S5.2, the parameters that need to be adjusted are the temperature of each temperature zone and the conveyor chain speed. If the temperature is too low / too high, the temperature of the corresponding temperature zone is gradually increased / decreased with a gradient of 5°C; if the duration is too low, the conveyor chain speed is correspondingly reduced.

[0074] In this embodiment, in step S7, during the temperature test, the wave soldering parameter settings refer to the simulation parameter settings, and a K-type thermocouple is used to test the temperature of high heat capacity solder joints to complete the actual temperature test of the circuit board.

[0075] In this embodiment, in step S7, the number of points is not less than 3. When arranging the points, the temperature measuring points are pasted to the test positions with high temperature resistant glue. The temperature measuring points must include 1 high thermal capacity component pin solder point, 1 bottom chip resistor / capacitor solder point, and 1 QFP / SOP / SOJ solder point. After the points are arranged, the K-shaped thermocouple is connected to the temperature recorder, the furnace temperature setting parameters are set according to the simulation results, and the PCBA temperature test record is completed.

[0076] In this embodiment, in step S7, the preheating requirement is that the temperature measured at the temperature measuring point in the preheating section is between 90°C and 125°C for not less than 20 seconds, and the temperature of the high-temperature container welding point in the preheating section is greater than 85°C;

[0077] In step S7, welding requires that the temperature measured at the temperature measuring point of the welding section is 260±5°C and the duration at this temperature is 3-5s.

[0078] In this embodiment, in steps S7.1 and S8.1, the redesigned parameters are the number of heat focusing holes and the size of the heat focusing holes. The diameter of the heat focusing holes is gradually increased / decreased by 0.2 mm according to the high / low measured temperature.

[0079] This method analyzes the welding process of high thermal capacity through-hole devices and uses simulation technology to achieve efficient evaluation of solder joint wave soldering effects from thermal analysis and local welding effect analysis, thereby achieving wave soldering of high thermal capacity through-hole devices, avoiding the traditional design method that is completely based on experience and continuous trial and error, improving work efficiency, and avoiding a lot of waste of time, money and other resources.

[0080] Embodiment 2:

[0081] Embodiment 2 provides a simulation example based on embodiment 1.

[0082] In this embodiment, the conveyor chain speed of the wave soldering structure is 120 cm / min.

[0083] In this embodiment, the boundary setting parameters are designed as follows:

[0084] The length of the first preheating zone is 80 cm, the zone residence time is 40 s, the top temperature is 30 ° C, and the top convection heat transfer coefficient is 5 W / m 2 ℃, bottom temperature is 120℃, bottom convection heat transfer coefficient is 25W / m 2 ℃;

[0085] The length of the second preheating zone is 80 cm, the zone residence time is 40 s, the top temperature is 30 ° C, and the top convection heat transfer coefficient is 5 W / m 2 ℃, bottom temperature is 170℃, bottom convection heat transfer coefficient is 25W / m 2 ℃;

[0086] The length of the third preheating zone is 80 cm, the zone residence time is 40 s, the top temperature is 30 ° C, and the top convection heat transfer coefficient is 5 W / m 2 ℃, bottom temperature is 180℃, bottom convection heat transfer coefficient is 25W / m 2 ℃;

[0087] The length of the transition zone is 20 cm, the zone residence time is 10 s, the top temperature is 30 °C, and the top convection heat transfer coefficient is 5 W / m 2 ℃, bottom temperature is 60℃, bottom convection heat transfer coefficient is 10W / m 2 ℃;

[0088] The length of the welding zone is 8 cm, the zone residence time is 4 s, the top temperature is 30 ° C, and the top convection heat transfer coefficient is 20 W / m 2 ℃, the bottom temperature is 265℃, and there is no bottom convection heat transfer coefficient;

[0089] The length of the cooling zone is 80 cm, the zone residence time is 40 s, the top temperature is 30 °C, the top convection heat transfer coefficient is 10 W / m2·°C, the bottom temperature is 30 °C, and the bottom convection heat transfer coefficient is 25 W / m2·°C.

[0090] In this embodiment, if Figure 5 As shown, when designing the pad, 8 metalized holes with a diameter of 0.6mm are evenly distributed around the plug-in hole at a hole margin of 0.4-0.6mm between the 2mm plug-in hole and the heat-collecting hole.

[0091] During the simulation analysis, the transient thermal analysis model of PCBA wave soldering process was established to solve the heat distribution and temperature change of the whole board during the wave soldering process of PCBA. The overall time-temperature history is as follows: Figure 6 As shown;

[0092] Preheating section:

[0093] 0-40s is the first preheating zone. From the PCBA temperature distribution, it can be seen that Figure 7 , 8 As shown in the figure, the temperature of the bottom patch rises faster at 4.4s, and the temperature of the chip rises fastest, reaching 100°C. The bottom temperature is significantly higher than the board surface, and the large components on the board absorb a lot of heat and heat up slowly.

[0094] When the first preheating zone is about to end (38.4s), if Fig. 9 , 10As shown, it can be clearly seen that the overall temperature distribution of the PCB board is uneven. Specifically, the temperature of the patch gathering area is higher than that of the THT component gathering area. This is mainly due to the difference in heat capacity. This shows that PCBA will generate thermal stress during the preheating process, which is easy to cause PCB warping or deformation.

[0095] Welding section:

[0096] 130-134s is the welding area, such as Fig.11 , 12 As shown in the figure, from the PCBA temperature distribution, it can be seen that at 133.05s, the bottom of the PCBA is evenly heated as a whole, and the temperature reaches 260°C. The area where large components gather on the board absorbs a lot of heat, and the temperature of the board bonding part is about 150°C.

[0097] Cooling section:

[0098] 134-180s is the cooling area, such as Fig.13 , 14 As shown in the figure, from the PCBA temperature distribution, it can be seen that at 135.64s, the overall maximum temperature of the PCBA has dropped to 200°C, and the overall temperature of the PCB is relatively high, indicating that the heat dissipation of components is fast, while the heat dissipation of the PCB board is relatively slow.

[0099] During the temperature test, the sample is prepared according to the above PCBA model, the wave soldering parameter settings refer to the simulation parameter settings, and K-type thermocouples (temperature sensors) are used to distribute points (the number of distribution points is not less than 3) to test the temperature of high heat capacity solder points, complete the actual temperature test of the circuit board, and judge whether the preheating (90℃-125℃) and welding requirements (260℃±5℃, 3-5s) are met according to the test temperature curve.

[0100] During the local solder joint analysis, wave soldering is performed on the circuit board that has completed the temperature test. After completion, the solder joints of high thermal capacity through-hole devices are visually inspected and sliced ​​to determine whether the appearance of the solder joint assembly meets the tin penetration height requirements for through-hole device solder joints in the IPC-A-610E standard.

[0101] For PCBAs that do not meet the requirements of local solder joints, adjust and optimize the pad design. If the temperature is too low / too high, gradually increase / reduce 2 heat-collecting holes until the requirements are met, and complete the welding of high thermal capacity through-hole devices.

[0102] If this patent discloses or involves components or structural parts that are fixedly connected to each other, then, unless otherwise stated, the fixed connection can be understood as: a detachable fixed connection (for example, connected by bolts or screws), or as: a non-detachable fixed connection (for example, riveting, welding). Of course, the fixed connection can also be replaced by an integrated structure (for example, manufactured by a casting process) (except where it is obviously impossible to use an integrated forming process).

[0103] In the description of this patent, it should be understood that the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing this patent, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this patent.

[0104] The preferred embodiments listed above further illustrate the objectives, technical solutions and advantages of the present invention in detail. It should be understood that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for soldering high thermal capacity through-hole components on a circuit board, characterized in that: The following steps are involved: S1: Pad design: Design the pad according to the circuit board configuration and the required high thermal capacity components; S2: Build PCBA model: Build the 3D model of the PCBA circuit board according to the circuit board configuration, PCB design drawings and component layout; S3: Import the 3D model of the PCBA circuit board into the ANSYS platform; S4: Set simulation parameters and rules on the ANSYS platform; S5: On the ANSYS platform, a transient thermal analysis model of the PCBA wave soldering process is established, and simulation analysis is performed to obtain the heat distribution and temperature change of the entire board during the wave soldering process, and to determine whether the temperature in the preheating stage meets the process requirements; S5.1, if it meets the process requirements, proceed to S6; S5.2, if it does not meet the process requirements, return to S4 to adjust the setting parameters; S6: preparing circuit board samples according to the constructed 3D model of the PCBA circuit board; S7: Conduct temperature test on the circuit board sample, and judge whether the preheating and welding requirements are met according to the test temperature curve obtained at the temperature measurement point; S7.1, if the requirements are not met, return to step S1 and redesign; S7.2, if the requirements are met, proceed to step S8; S8: Local solder joint analysis: Perform wave soldering on the circuit board sample, and after completion, perform appearance inspection and slice observation on the high thermal capacity through-hole device solder joints to determine whether the solder joint assembly appearance meets the tin penetration height requirements for through-hole device solder joints in the IPC-A-610E standard; S8.1, if the requirements are not met, return to step S1 and redesign; S8.2, if the requirements are met, complete the soldering of the high thermal capacity through-hole device on the circuit board.

2. The method for soldering high thermal capacity through-hole components of a circuit board according to claim 1, characterized in that: In step S1, the pad adopts a heat-concentrating pad design, and a plurality of metallized holes are arranged between the plug-in hole and the heat-concentrating hole, and the metallized holes are evenly distributed around the plug-in hole.

3. The method for soldering high thermal capacity through-hole components of a circuit board according to claim 1, characterized in that: In step S3, the 3D model is divided into hexahedral structured grids using the sweep partitioning method on the ANSYS platform; In step S3, the 3D model features need to be simplified, and the THT component pins, component shapes, and PCB body need to be block-processed.

4. The method for soldering high thermal capacity through-hole components of a circuit board according to claim 1, characterized in that: In step S4, the simulation parameter setting is to divide the temperature zones of the preheating section and the welding section of the wave soldering according to the wave soldering structure and thermal analysis requirements, and divide the preheating section into the first preheating section, the second preheating section, and the third preheating section along the welding conveying direction, and set the area between the preheating section and the welding section as the transition zone, simplify the welding section to a fixed heat source treatment, and set it as the welding zone, and the output side of the welding section is set as the cooling zone; In step S4, convection boundary conditions are set at the bottom and top of the first preheating zone, the second preheating zone, the third preheating zone, the transition zone, and the cooling zone; the bottom of the welding zone adopts a temperature boundary condition, and the top adopts a convection boundary condition.

5. The method for soldering a circuit board high thermal capacity through-hole device according to claim 1 or 4, characterized in that: In step S4, the rule setting is to implement load step loading in a specific area and at a specific time. In convective heat transfer, loading in other time periods is suppressed according to the temperature settings of each section. Unnecessary time periods are selected for suppression operations. The suppressed load step will not load the corresponding boundary conditions; otherwise, the activated load step can be loaded normally.

6. The method for soldering a circuit board high thermal capacity through-hole device according to claim 1, characterized in that: In step S5, the process requirement is that the PCBA circuit board temperature is between 90-125°C for not less than 20 seconds, and the temperature of the high-temperature container solder joint is greater than 85°C in the preheating stage; In step S5.2, the parameters that need to be adjusted are the temperature of each temperature zone and the conveyor chain speed. If the temperature is too low / too high, the temperature of the corresponding temperature zone is gradually increased / decreased with a gradient of 5°C; if the duration is too low, the conveyor chain speed is correspondingly reduced.

7. The method for soldering high thermal capacity through-hole components of a circuit board according to claim 1, characterized in that: In step S7, during the temperature test, the wave soldering parameter settings refer to the simulation parameter settings, and a K-type thermocouple is used to test the temperature of high heat capacity solder joints to complete the actual temperature test of the circuit board.

8. The method for soldering a circuit board high thermal capacity through-hole device according to claim 7, characterized in that: In step S7, the number of points to be laid out is no less than 3, and the temperature measurement points must include 1 high thermal capacity component pin solder point, 1 bottom chip resistor / capacitor solder point, and 1 QFP / SOP / SOJ solder point; after the points are laid out, connect the K-shaped thermocouple to the temperature recorder, set the furnace temperature setting parameters according to the simulation results, and complete the PCBA temperature test record.

9. The method for soldering a circuit board high thermal capacity through-hole device according to any one of claims 1, 7 and 8, characterized in that: In step S7, the preheating requirement is that the temperature measured at the temperature measuring point in the preheating section is between 90°C and 125°C for not less than 20 seconds, and the temperature of the high-temperature container welding point in the preheating section is greater than 85°C; In step S7, welding requires that the temperature measured at the temperature measuring point of the welding section is 260±5°C and the duration at this temperature is 3-5s.

10. The method for soldering a circuit board high thermal capacity through-hole device according to claim 1, characterized in that: In steps S7.1 and S8.1, the redesigned parameters are the number of heat focusing holes and the size of the heat focusing holes. The diameter of the heat focusing holes is gradually increased / decreased by 0.2 mm according to the high / low measured temperature.