Lithium sulfide-polymer composite positive electrode material and preparation method thereof and lithium-sulfur battery
By using lithium sulfide and polymer composite materials with core-shell structure in the positive electrode material of lithium sulfur battery, the problems of poor conductivity and structural instability of lithium sulfur batteries are solved, and higher battery performance and longer service life are achieved. It is suitable for use in the positive electrode material of lithium sulfur batteries. Mass production.
Patent Information
- Application Number
- CN202211035197.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-26
AI Technical Summary
Due to the low conductivity of elemental sulfur, the "shuttle effect" of polysulfide and large-volume changes in the positive electrode structure, lithium-sulfur batteries have short service life, which limits their large-scale commercial applications.
The lithium sulfide and polymer composite material with core-shell structure is used to form a conductive polymer cladding layer through ball milling and heat treatment, which improves the conductivity and electrochemical activity of the material and ensures the stability of the electrode structure.
The stable structure and excellent conductivity of the lithium-sulfur battery positive electrode material are realized, the discharge performance and service life of the battery are improved, and the preparation method is simple and low-cost, which is suitable for large-scale production.
Smart Images

Figure CN115332514B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials for lithium-sulfur batteries, and in particular to the technical field of positive electrode materials for lithium-sulfur batteries that are composites of lithium sulfide and polymers. Background Art
[0002] With the development of society, especially the emergence of new concepts such as 5G and new energy vehicles, traditional lithium-ion batteries have become increasingly difficult to meet the high-standard energy storage needs of the future. Therefore, new energy systems must be required to have greater specific energy and longer service life. Lithium-sulfur batteries are secondary batteries composed of sulfur as the positive electrode and lithium as the negative electrode. Among them, elemental sulfur as the positive electrode material has the advantages of abundant reserves, easy access, low price, and green environmental protection. It also ensures that lithium-sulfur batteries have large specific capacity and high energy density. The energy density of commercial lithium-ion batteries is currently about 200-250Wh / Kg, while the theoretical specific energy of lithium-sulfur batteries is five times that of these lithium-ion batteries, about 2600Wh / Kg, and the specific capacity is also about 1675mAh / g, far exceeding traditional commercial lithium batteries.
[0003] However, lithium-sulfur batteries have a short service life due to problems such as the low conductivity of elemental sulfur, the "shuttle effect" of polysulfides, and large volume changes in the positive electrode structure, making their actual large-scale commercial application not yet fully realized. Summary of the invention
[0004] In view of the problems of poor conductivity, unstable structure and poor electrochemical performance of lithium sulfide electrodes in the prior art, the purpose of the present invention is to provide a new positive electrode material for lithium-sulfur batteries, which is a composite material of lithium sulfide with a core-shell structure and a polymer, has a stable electrode structure, excellent conductivity and electrochemical activity, and the preparation method is simple and fast, the raw materials are abundant, the cost is low, it is green and environmentally friendly, and it is easy to realize large-scale production.
[0005] The technical solution of the present invention is as follows:
[0006] A lithium sulfide-polymer composite positive electrode material has a core-shell structure in which the core is micro-nano lithium sulfide obtained by ball milling and the shell is a conductive polymer. The conductive polymer is formed by combining lithium sulfide and a polymer coating the lithium sulfide, and the polymer contains a cyano group.
[0007] Under this technical solution, the CN- of the polymer can be combined with the Li in Li2S + The ions form a chemical bond, thereby obtaining a stable structure in which the core is lithium sulfide and the shell is a conductive polymer after polymer cyclization, while ensuring the conductive properties and electrochemical activity of the material.
[0008] According to some specific embodiments of the present invention, the polymer is selected from polyacrylonitrile.
[0009] In this specific embodiment, the CN- of polyacrylonitrile and the Li in Li2S + The ions form a chemical bond, thereby cyclizing the polyacrylonitrile to form a coating of conductive polymer.
[0010] The present invention further provides a method for preparing a lithium sulfide-polymer composite positive electrode material, which comprises:
[0011] (1) in an inert atmosphere, polyacrylonitrile and lithium sulfide are uniformly mixed, and then sealed high-speed ball milling is performed at 300 to 800 r / min for 6 to 14 hours to obtain a base material;
[0012] (2) adding the base material to a dimethylformamide solution of polyacrylonitrile for uniform dissolution, then evaporating the solvent and vacuum drying, then sintering in an inert atmosphere, and cooling the sintered material to room temperature to obtain the lithium sulfide-polymer composite positive electrode material.
[0013] Under the above technical scheme, the high-speed ball milling in step (1) can make CN- in the polymer and Li in Li2S + The ions form a basic chemical bond, and the polymer is cyclized into a conductive polymer coating layer, but the coating layer is not complete. Then, a secondary physical coating can be further achieved through step (2), and the outer layer forms a cyclized polyacrylonitrile coating layer again, which can further ensure the integrity of the material structure and form a composite structure of lithium sulfide, conductive polymer and cyclized polyacrylonitrile.
[0014] According to some preferred embodiments of the present invention, the high-speed ball milling time is 8 hours.
[0015] According to some preferred embodiments of the present invention, the sintering temperature is 300-900°C.
[0016] According to some preferred embodiments of the present invention, the sintering temperature is 350° C., and the sintering time is 12 hours.
[0017] According to some preferred embodiments of the present invention, in step (1), the mass of the polyacrylonitrile accounts for 5%-30% of the total mass of the polyacrylonitrile and the lithium sulfide.
[0018] According to some preferred embodiments of the present invention, in step (2), the mass of the polyacrylonitrile accounts for 5%-30% of the total mass of the polyacrylonitrile and the dimethylformamide.
[0019] According to some preferred embodiments of the present invention, the average molecular weight of the polyacrylonitrile is 150,000 g / mol.
[0020] According to some preferred embodiments of the present invention, the average molecular weight of the polyacrylonitrile is 150,000 g / mol; the mass ratio of the polyacrylonitrile to the lithium sulfide is 1:9; the ball milling rate is 500 r / min, and the time is 8 h; the mass ratio of the base material to the PAN is 1:0.2, and the sintering is performed at 350° C. for 12 h in an argon atmosphere.
[0021] According to the obtained lithium sulfide-polymer composite positive electrode material, a lithium-sulfur battery containing the positive electrode material can be further obtained.
[0022] The present invention has the following beneficial effects:
[0023] (1) The positive electrode material obtained by the present invention has a complete core-shell structure, which can ensure the stability of the electrode structure.
[0024] (2) The preparation method of the present invention can make polymers such as PAN cyclize on the surface of Li2S to form conductive polymers with electron pathways, thereby improving the electrochemical activity of the positive electrode material.
[0025] (3) The preparation method of the present invention is simple, fast, low-cost, green and environmentally friendly, and easy to achieve mass production.
[0026] (4) The lithium-sulfur battery obtained by the present invention improves the capacity of the original material, and the discharge performance at different discharge rates far exceeds that of the original material. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 : This is the XRD pattern of the lithium sulfide / polymer base material obtained in Example 1.
[0028] Figure 2 This is a comparison chart of infrared spectra of the lithium sulfide / polymer base material obtained in Example 1, ball-milled pure PAN, and un-ball-milled PAN.
[0029] Figure 3 The SEM images of the ball-milled base material obtained in Example 1 and the final lithium sulfide / polymer composite positive electrode material.
[0030] Figure 4 This is a rate performance diagram of the lithium sulfide / polymer composite positive electrode material obtained in Example 1 and the original lithium sulfide material. DETAILED DESCRIPTION
[0031] The present invention is described in detail below in conjunction with the embodiments and drawings, but it should be understood that the embodiments and drawings are only used to exemplify the present invention and do not constitute any limitation on the protection scope of the present invention. All reasonable changes and combinations within the scope of the inventive concept of the present invention fall within the protection scope of the present invention.
[0032] According to the technical solution of the present invention, some specific implementations of the method for preparing the lithium sulfide-polymer composite positive electrode material include:
[0033] (1) Ball milling: In an inert atmosphere, polyacrylonitrile (PAN) and lithium sulfide are mixed evenly, placed in a ball mill and sealed, and subjected to high-speed ball milling for 6 to 14 hours to obtain a base material, which is denoted as A.
[0034] (2) Heating treatment: Under an inert atmosphere, PAN is added to dimethylformamide (DMF) solvent until it is fully dissolved, and then material A is added. After continuing to stir evenly, the DMF solvent is evaporated and vacuum dried at 60°C; then sintered in a tubular furnace with an inert atmosphere, and cooled to room temperature to obtain a lithium sulfide / polymer composite positive electrode material.
[0035] Some of the preferred embodiments are as follows:
[0036] The rotation speed of the high-speed ball mill is 300-800 r / min, and the time is preferably 8 hours.
[0037] The sintering temperature is 300-900°C, more preferably 350°C; the sintering time is preferably 12h.
[0038] In step (1), the mass of polyacrylonitrile accounts for 5%-30% of the total mass of polyacrylonitrile and lithium sulfide.
[0039] In step (2), the mass of polyacrylonitrile accounts for 5%-30% of the total mass of polyacrylonitrile and dimethylformamide.
[0040] The inert atmosphere includes argon and / or nitrogen, preferably argon with a purity of >99%.
[0041] The average molecular weight of PAN is 150,000 g / mol.
[0042] The technical solution of the present invention is further demonstrated through embodiments below.
[0043] Example 1
[0044] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0045] (1) Ball milling:
[0046] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 8 h to obtain a base material;
[0047] (2)Heat treatment:
[0048] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0049] The obtained basic material was subjected to XRD and infrared tests. In the infrared test, pure PAN material ball-milled under the same ball-milling conditions and PAN not ball-milled were used as comparisons, as shown in the attached figure. Figure 1 , 2 As shown, the obtained ball-milled base material and the final lithium sulfide-polymer composite positive electrode material were characterized by SEM (see Appendix Figure 3 As shown). The original lithium sulfide, the basic material obtained by ball milling, and the final lithium sulfide-polymer composite positive electrode material were assembled into button batteries. The assembly order was positive electrode shell-spring-gasket-positive electrode sheet-diaphragm-lithium sheet-gasket-spring-negative electrode shell. The electrolyte was DOL and DME (V:V=1:1) dissolved with 1MolLiTFSI, and 2% LiNO3 was dissolved. The rate performance of the assembled battery was tested by the test method of charging to 4V at a rate of 0.05C for the first time, and then charging and discharging tests were carried out continuously for 10 weeks at rates of 0.1C, 0.2C, 0.5C, 1C, 2C, and 0.1C. The charging voltage was 3V and the discharge voltage was 1.5V. The specific capacity of the battery at different rates was obtained (as shown in the attached figure). Figure 4 shown).
[0050] pass Figure 1 It can be seen that ball milling does not change the structure of lithium sulfide. Figure 2 It can be seen that under the promotion of lithium sulfide, PAN undergoes cyclization under high-speed ball milling, and the two combine to form a conductive polymer shell. Figure 3 It can be seen that (a) (b) are SEM images of the ball-milled base material at different magnifications. It can be seen that the surface of the ball-milled material has many holes, the structure is incomplete, and it is difficult to inhibit the shuttling of polysulfides. (c) (d) are SEM images of the final composite material at different magnifications. It can be seen that after the material is secondary coated, the voids are filled, and the surface has secondary PAN particles after re-coating, which has good spherical coating structure integrity. Figure 4 It can be seen from the rate performance that the material has a very good rate performance. At different rates, the discharge capacity is far superior to that of the original material and the material obtained by ball milling. After being discharged at different rates, it returns to the 0.1C rate and still has a specific capacity of about 660mAh / g.
[0051] Example 2
[0052] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0053] (1) Ball milling:
[0054] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 2:8 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 8 h to obtain a base material;
[0055] (2)Heat treatment:
[0056] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0057] Example 3
[0058] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0059] (1) Ball milling:
[0060] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 3:7 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 8 h to obtain a base material;
[0061] (2)Heat treatment:
[0062] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0063] Example 4
[0064] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0065] (1) Ball milling:
[0066] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 6 h to obtain a base material;
[0067] (2)Heat treatment:
[0068] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0069] Example 5
[0070] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0071] (1) Ball milling:
[0072] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 10 h to obtain a base material;
[0073] (2)Heat treatment:
[0074] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0075] Example 6
[0076] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0077] (1) Ball milling:
[0078] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 12 h to obtain a base material;
[0079] (2)Heat treatment:
[0080] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0081] Example 7
[0082] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0083] (1) Ball milling:
[0084] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 14 h to obtain a base material;
[0085] (2)Heat treatment:
[0086] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0087] Example 8
[0088] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0089] (1) Ball milling:
[0090] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 8 h to obtain a base material;
[0091] (2)Heat treatment:
[0092] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.04 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0093] Example 9
[0094] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0095] (1) Ball milling:
[0096] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 8 h to obtain a base material;
[0097] (2)Heat treatment:
[0098] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.06 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 350°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0099] Example 10
[0100] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0101] (1) Ball milling:
[0102] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 8 h to obtain a base material;
[0103] (2)Heat treatment:
[0104] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir and heat to evaporate, and dry. The dried product is placed in a tubular furnace protected by argon atmosphere, sintered at 300°C for 12 hours, and cooled to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0105] Embodiment 11
[0106] The lithium sulfide-polymer composite cathode material was prepared by the following steps:
[0107] (1) Ball milling:
[0108] PAN with a molecular weight of 150,000 and lithium sulfide were weighed in a mass ratio of 1:9 with a total mass of 0.8 g, placed in a ball mill under an argon atmosphere, and ball milled at a rate of 500 r / min for 8 h to obtain a base material;
[0109] (2)Heat treatment:
[0110] Take 0.2 g of the obtained base material and place it in a DMF solution containing 0.02 g of PAN, stir, heat, evaporate, and dry. Place the dried product in a tubular furnace protected by argon atmosphere, sinter at 400°C for 12 hours, and cool to room temperature to obtain a black lithium sulfide-polymer composite positive electrode material.
[0111] The above Examples 1-11 all have the same structure. The change in PAN content only changes the amount of conductive polymer and the thickness of the outer cyclized polyacrylonitrile, which will affect the transmission of ions and the performance of the battery. The change in ball milling parameters will affect the sufficiency of the reaction to generate the conductive polymer, and the heating method parameters will affect the degree of cyclization of the outer polyacrylonitrile. After exploration, the optimal parameters are a mass ratio of 1:9. Weigh polyacrylonitrile and lithium sulfide with a molecular weight of 150,000, ball mill at 500 r / min for 8 hours, dissolve 0.04 g PAN in DMF (that is, the mass ratio of the base material to the PAN is 0.2:0.04), and calcine at 350°C for 12 hours under argon atmosphere.
[0112] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a lithium sulfide-polymer composite positive electrode material, It is characterized in that It includes: (1) In an inert atmosphere, polyacrylonitrile and lithium sulfide are uniformly mixed, and then sealed high-speed ball milling is performed at a ball milling rate of 500 r / min for 8 hours to obtain a base material; (2) adding the base material to a dimethylformamide solution of polyacrylonitrile having an average molecular weight of 150,000 g / mol for uniform dissolution, then evaporating the solvent and vacuum drying, then sintering in argon at 350° C. for 12 h, cooling the sintered material to room temperature and then grinding it to obtain a lithium sulfide-polymer composite positive electrode material; The mass ratio of the polyacrylonitrile to the lithium sulfide is 1:9; the mass ratio of the base material to the polyacrylonitrile is 1:0.2; the mass of the polyacrylonitrile accounts for 5%-30% of the total mass of the polyacrylonitrile and the dimethylformamide; The lithium sulfide-polymer composite positive electrode material is a core-shell structure in which the core is micro-nano lithium sulfide obtained by ball milling and the shell is a conductive polymer, and the conductive polymer is formed by combining lithium sulfide with a polymer polyacrylonitrile coated with lithium sulfide.
2. The lithium sulfide-polymer composite positive electrode material prepared by the preparation method according to claim 1.
3. A lithium-sulfur battery containing the lithium sulfide-polymer composite positive electrode material according to claim 2.
Citation Information
Cited By
Method for preparing vulcanized polyacrylonitrile by adopting microwave sintering process and product
CN120040631A