A method for increasing the energy proportion of a mid-infrared supercontinuum light source in the long-wavelength spectral region
By using fluorotellurite glass or chalcogenide glass fiber as a nonlinear medium in the mid-infrared band, combined with red-shifted dispersion wave and cascade Raman amplification technology in the fiber, the long-wavelength spectral energy share of the mid-infrared supercontinuum light source is increased. Ratio, solves the problem of insufficient energy ratio in the existing technology, and realizes an efficient broadband mid-infrared supercontinuum light source.
Patent Information
- Application Number
- CN202211054198.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-08-31
AI Technical Summary
The long-wavelength spectral region of the mid-infrared broadband supercontinuum light source has a low energy proportion, which limits its application range.
Using low transmission loss fluorotellurite glass fiber or chalcogenide glass fiber as the nonlinear medium, by optimizing the design of nonlinear fiber and pump laser parameters, using the red-shifted dispersion wave generation effect in the fiber and cascade Raman amplification technology, Increase the energy proportion of the broadband mid-infrared supercontinuum light source in the long-wavelength spectral region.
An all-fiber broadband mid-infrared supercontinuum light source with ultra-high energy ratio in the long-wavelength spectral region has been realized. The system has a compact structure, simple operation, and stable operation.
Smart Images

Figure CN115360580B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of broadband supercontinuum light sources, and in particular relates to a method for increasing the energy proportion of a mid-infrared supercontinuum light source in a long-wavelength spectral region. Background Art
[0002] A supercontinuum light source is a broadband laser light source obtained when a high-peak power pulsed laser is transmitted in a highly nonlinear medium, and the spectrum is greatly broadened due to the combined effects of dispersion and multiple nonlinear optical effects. This light source not only has high brightness and coherence, but also has an ultra-wide spectrum with a spectral width of up to thousands of nanometers, which makes it have important applications in basic scientific research, medical treatment, environment, national defense and security. Compared with supercontinuum light sources based on liquids, gases and bulk solids, supercontinuum light sources based on optical fibers have become the main direction of broadband supercontinuum light source research in recent years because of their high efficiency, good beam quality, compact structure, good reliability, high stability, long life, small size, light weight, and easy portability and integration.
[0003] The mid-infrared band contains several important optical transmission windows in the atmosphere and characteristic spectral lines of many important molecules. All-fiber broadband supercontinuum light sources operating in the mid-infrared band can be widely used in spectroscopy, biomedicine, biophotonics, pollution monitoring, chemical gas and hazardous goods monitoring, atmospheric communications, infrared guidance, optoelectronic countermeasures and other fields. At present, broadband supercontinuum light sources with working wavelengths covering the entire mid-infrared band have been developed using tellurite glass fibers, fluorotellurite glass fibers, fluoride glass fibers or chalcogenide glass fibers with low transmission loss in the mid-infrared band as nonlinear media. However, the energy proportion of the long-wavelength spectral region is low, which limits the application scope of this type of light source. Therefore, it is of great significance to explore new methods to increase the energy proportion of the long-wavelength spectral region of broadband supercontinuum light sources, and then realize all-fiber broadband mid-infrared supercontinuum light sources with high energy proportion of the long-wavelength spectral region. Summary of the invention
[0004] In order to solve the problem of low energy proportion in the long-wavelength spectral region of the current broadband supercontinuum light source in the mid-infrared band, the present invention provides a method for increasing the energy proportion of the mid-infrared supercontinuum light source in the long-wavelength spectral region. The method uses fluorotellurite glass optical fiber or chalcogenide glass optical fiber with low transmission loss in the mid-infrared band as a nonlinear medium, optimizes the design of nonlinear optical fiber and pump laser parameters, obtains a broadband mid-infrared supercontinuum light source based on the red-shifted dispersion wave generation effect in the optical fiber, and simultaneously uses cascaded Raman amplification technology to increase the energy proportion of the broadband mid-infrared supercontinuum light source in the long-wavelength spectral region, thereby developing an all-fiber broadband mid-infrared supercontinuum light source with ultra-high energy proportion in the long-wavelength spectral region.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for increasing the energy proportion of a mid-infrared supercontinuum light source in a long-wavelength spectral region comprises the following steps:
[0007] Step 1: Build a broadband mid-infrared supercontinuum light source, including a pump source 1, an isolator 2 and a nonlinear optical fiber 3. The output optical fiber of the pump source 1 is connected to the input optical fiber of the isolator 2, and the output optical fiber of the isolator 2 is connected to the nonlinear optical fiber 3. The isolator 2 is used to ensure unidirectional transmission of the laser to prevent the system return light from damaging the pump light source.
[0008] Step 2: Increase the energy proportion in the long-wavelength spectral region based on a broadband mid-infrared supercontinuum light source, as follows:
[0009] After passing through the isolator 2, the pump light 1 is coupled into the nonlinear optical fiber 3; the spectrum is broadened under the action of multiple nonlinear optical effects to obtain broadband mid-infrared supercontinuum light output; specifically, the incident end of the nonlinear optical fiber 3 has a double zero dispersion wavelength, and the output end is full positive dispersion; the working wavelength of the pump source 1 is located in the negative dispersion region of the incident end of the nonlinear optical fiber 3, close to the second zero dispersion wavelength position; when the pump light 1 is coupled into the nonlinear optical fiber 3, the pump light 1 is located in the anomalous dispersion region of the nonlinear optical fiber 3, and in the high-order soliton splitting and soliton self-frequency shift Under the action of the effect, the generated optical solitons move toward the long wave. Since the working wavelength of the pump source 1 is close to the second zero dispersion wavelength position of the nonlinear optical fiber 3, the generated optical solitons can quickly encounter the second zero dispersion wavelength of the nonlinear optical fiber 3, and radiate dispersion waves toward the long wave region to generate red-shifted dispersion waves. In the normal dispersion region of the nonlinear optical fiber 3, the above-mentioned red-shifted dispersion waves serve as seed light, and under the cascade action of the stimulated Raman scattering effect and the Raman amplification effect, their energy increases, and finally a fiber-based broadband mid-infrared supercontinuum light source with a high energy proportion in the long wavelength spectral region is realized.
[0010] Furthermore, the output optical fiber of the pump source 1 is connected to the input optical fiber of the isolator 2 by direct fusion splicing, and the output optical fiber of the isolator 2 is connected to the nonlinear optical fiber 3 by direct fusion splicing or mechanical docking.
[0011] Furthermore, the pump source 1 is a femtosecond fiber laser, the central wavelength of the femtosecond fiber laser is 1.9-4 μm, the pulse width is 10 fs-10 ps, and the repetition frequency is 1 kHz-10 GHz.
[0012] Furthermore, the nonlinear optical fiber 3 is a fluorotellurate glass optical fiber or a chalcogenide glass optical fiber with a gradually decreasing core diameter.
[0013] Compared with the prior art, the advantages of the present invention are as follows:
[0014] The invention discloses a broadband mid-infrared supercontinuum light source with ultra-high energy proportion in the long-wavelength spectral region. By optimizing the design parameters of a pump source and a nonlinear optical fiber, the nonlinear optical effect in the optical fiber is managed, and the red-shifted dispersion wave generation effect in the double-zero-dispersion wavelength optical fiber is utilized to obtain the broadband mid-infrared supercontinuum light source. The cascade Raman amplification effect in the optical fiber is utilized to increase the energy proportion in the long-wavelength spectral region of the supercontinuum light source, thereby achieving the purpose of increasing the energy proportion of the mid-infrared supercontinuum light source in the long-wavelength spectral region. The light source system has a compact structure, simple operation, and stable operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.
[0016] Figure 1 : A schematic structural diagram of a broadband mid-infrared supercontinuum light source with an ultra-high long-wavelength spectral region energy ratio according to the present invention;
[0017] In the figure: pump source 1, isolator 2, nonlinear optical fiber 3;
[0018] Figure 2 : A graph showing the variation of the core diameter of the fluorotellurite glass optical fiber with the length of the optical fiber in Example 1 of the present invention;
[0019] Figure 3 : Group velocity dispersion curves of fluorotellurite glass optical fibers with different core diameters in Example 1 of the present invention;
[0020] Figure 4 : The evolution diagram of the output spectrum of the supercontinuum light source in Example 1 of the present invention with the pump power of the 1.98 μm femtosecond fiber laser;
[0021] Figure 5 : Output spectrum diagram of the mid-infrared supercontinuum light source with energy proportion in the high and long wavelength region in Example 1 of the present invention (in linear coordinates). DETAILED DESCRIPTION
[0022] In order to clearly and completely describe the technical solution and its specific working process of the present invention, the specific implementation methods of the present invention are as follows in conjunction with the accompanying drawings of the specification:
[0023] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0024] Example 1
[0025] A method for increasing the energy proportion of a mid-infrared supercontinuum light source in a long-wavelength spectral region in this embodiment is:
[0026] Step 1: Build a broadband mid-infrared supercontinuum source, such as Figure 1 As shown, it includes a pump source 1, an isolator 2 and a nonlinear optical fiber 3. The output optical fiber of the pump source 1 is connected to the input optical fiber of the isolator 2, and the output optical fiber of the isolator 2 is connected to the nonlinear optical fiber 3. The isolator 2 is used to ensure unidirectional transmission of laser light to prevent the system return light from damaging the pump light source.
[0027] Step 2: Increase the energy proportion in the long-wavelength spectral region based on a broadband mid-infrared supercontinuum light source, as follows:
[0028] After passing through the isolator 2, the pump light 1 is coupled into the nonlinear optical fiber 3; the spectrum is broadened under the action of multiple nonlinear optical effects to obtain broadband mid-infrared supercontinuum light output; specifically, the incident end of the nonlinear optical fiber 3 has a double zero dispersion wavelength, and the output end is full positive dispersion; the working wavelength of the pump source 1 is located in the negative dispersion region of the incident end of the nonlinear optical fiber 3, close to the second zero dispersion wavelength position; when the pump light 1 is coupled into the nonlinear optical fiber 3, the pump light 1 is located in the anomalous dispersion region of the nonlinear optical fiber 3, and in the high-order soliton splitting and soliton self-frequency shift Under the action of the effect, the generated optical solitons move toward the long wave. Since the working wavelength of the pump source 1 is close to the second zero dispersion wavelength position of the nonlinear optical fiber 3, the generated optical solitons can quickly encounter the second zero dispersion wavelength of the nonlinear optical fiber 3, and radiate dispersion waves toward the long wave region to generate red-shifted dispersion waves. In the normal dispersion region of the nonlinear optical fiber 3, the above-mentioned red-shifted dispersion waves serve as seed light, and under the cascade action of the stimulated Raman scattering effect and the Raman amplification effect, their energy increases, and finally a fiber-based broadband mid-infrared supercontinuum light source with a high energy proportion in the long wavelength spectral region is realized.
[0029] In this embodiment, the coupling between the output optical fiber of the isolator 2 and the fluorotellurate glass optical fiber 3 is performed by direct fusion splicing.
[0030] In this embodiment, the pump source 1 is a femtosecond fiber laser, and the central wavelength of the femtosecond fiber laser is ˜1.98 μm, the pulse width is ˜300 fs, and the repetition frequency is ˜50 MHz.
[0031] In this embodiment, the nonlinear optical fiber 3 is a core diameter tapered fluorotellurate glass optical fiber, which has a step refractive index structure, and its core and cladding materials are TeO2-BaF2-Y2O3 and AlF3-BaF2-CaF2-YF3-SrF2-MgF2-TeO2 glass respectively;
[0032] The fluorotellurate glass optical fiber has a total length of 3 m, an initial core diameter of 1.64 μm, and a terminal core diameter of 0.9 μm. The core diameter varies with the length of the optical fiber as shown in the following figure: Figure 2 As shown in the figure, it can be seen that as the length of the optical fiber increases, the core diameter of the optical fiber gradually decreases.
[0033] Figure 3 The group velocity dispersion curves of fluorotellurite glass optical fibers with different core diameters are shown in the figure. It can be seen that when the core diameters are 1.64, 1.5, 1.4, 1.3 and 1.2 μm, the first zero dispersion wavelength of the optical fiber is 1.192, 1.185, 1.18, 1.173 and 1.158 μm, and the second zero dispersion wavelength is 2.096, 1.876, 1.655, 1.547 and 1.348 μm respectively; when the core diameter is 1.64, 1.5, 1.4, 1.3 and 1.2 μm, the first zero dispersion wavelength of the optical fiber is 1.192, 1.185, 1.18, 1.173 and 1.158 μm, and the second zero dispersion wavelength is 2.096, 1.876, 1.655, 1.547 and 1.348 μm respectively. When the core diameter of the fluorotellurite glass fiber is less than 1.5μm, the pump laser wavelength is in the normal dispersion region of the fiber; when the core diameter of the fiber is less than 1.2μm, the fiber has a full positive dispersion characteristic; when the core diameter of the fluorotellurite glass fiber is 1.64, 1.5, 1.4, 1.3, 1.2, 1.1, 1.0 and 0.9μm, its nonlinear coefficient at a wavelength of 1.98μm is 539, 593, 632, 668, 689, 703, 721 and 745km respectively. -1 W -1 .
[0034] Figure 4The output spectrum of the broadband mid-infrared supercontinuum light source in this embodiment evolves with the pump power of the 1.98μm femtosecond fiber laser; it can be seen from the figure that with the increase of the pump laser power, the spectrum gradually broadens; this is because the pump laser wavelength is located in the anomalous dispersion region of the fluorotellurite glass fiber (incident end), and when the average power of the pump laser increases, the spectrum gradually broadens under the action of nonlinear optical effects such as self-phase modulation, high-order soliton splitting, and soliton self-frequency shift. Since the pump laser wavelength is close to the second zero dispersion wavelength position of the optical fiber, the generated soliton quickly encounters the second zero dispersion wavelength of the optical fiber during the frequency shift process, and the soliton self-frequency shift cancellation effect occurs, generating a red-shifted dispersion wave. When the pump light and the generated red-shifted dispersion wave are transmitted in the fluorotellurite glass fiber, they quickly enter the normal dispersion region of the optical fiber (transmission distance>0.5m, fiber core diameter<1.5μm). As the pump laser power increases, the optical signal generated at a wavelength of 2.34μm gradually increases due to the Raman amplification effect, and then it is used as a pump light to amplify the optical signal at a wavelength of 2.7μm. When the average power of the pump laser is 500mW, a broadband supercontinuum light source with an output spectrum ranging from 1.08 to 3.065μm is obtained, and the long-wavelength region in the spectrum has an ultra-high energy share.
[0035] Figure 5 Under linear coordinates, when the pump laser power is 500mW, the light source output spectrum is obtained, in which the energy in the long wavelength region (2.5-3.065μm) of the spectrum accounts for about 85%, achieving a significant increase in the energy proportion of the long wavelength spectral region of the mid-infrared supercontinuum.
[0036] In summary, the present invention uses the above-mentioned femtosecond fiber laser as a pump source, the above-mentioned core diameter gradually decreasing fluorotellurite glass fiber or chalcogenide glass fiber as a nonlinear medium, and comprehensively utilizes the red-shifted dispersion wave generation and cascade Raman amplification effect in the optical fiber to increase the energy proportion of the broadband mid-infrared supercontinuum light source in the long wavelength spectrum region. The above-mentioned fluorotellurite glass fiber or chalcogenide glass fiber initially has two zero dispersion wavelengths. As the length of the optical fiber increases, its core diameter becomes smaller, and the optical fiber dispersion gradually evolves into full positive dispersion. The operating wavelength of the pump laser is located in the anomalous dispersion region adjacent to the second zero dispersion wavelength of the nonlinear optical fiber (at the incident end). When the pump laser is transmitted in the nonlinear optical fiber, the spectrum is first broadened due to the self-phase modulation effect, and then under the action of high-order soliton splitting and soliton self-frequency shift effects, the generated optical solitons quickly encounter the second zero dispersion wavelength of the nonlinear optical fiber and radiate dispersion waves to the long wavelength region. In addition to having a large nonlinear coefficient, fluorotellurite glass fiber and chalcogenide glass fiber also have a large Raman gain coefficient. In the normal dispersion region of the optical fiber, stimulated Raman scattering plays a dominant role. When the pump light and the generated red-shifted dispersion wave are transmitted in the positive dispersion fluorotellurite glass fiber or chalcogenide glass fiber, the red-shifted dispersion wave is amplified under the cascade Raman amplification effect, thereby obtaining a broadband mid-infrared supercontinuum light source with a high energy proportion in the long wavelength spectral region.
[0037] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0038] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0039] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for increasing the energy proportion of a mid-infrared supercontinuum light source in the long-wavelength spectral region, characterized in that: The specific steps include: Step 1: constructing a broadband mid-infrared supercontinuum light source, including a pump source (1), an isolator (2) and a nonlinear optical fiber (3), wherein the output optical fiber of the pump source (1) is connected to the input optical fiber of the isolator (2), and the output optical fiber of the isolator (2) is connected to the nonlinear optical fiber (3); the isolator (2) is used to ensure unidirectional transmission of laser light and prevent system return light from damaging the pump light source; Step 2: Increase the energy proportion in the long-wavelength spectral region based on a broadband mid-infrared supercontinuum light source, as follows: After passing through the isolator (2), the pump light (1) is coupled into the nonlinear optical fiber (3); the spectrum is broadened under the action of multiple nonlinear optical effects to obtain broadband mid-infrared supercontinuum light output; specifically, the incident end of the nonlinear optical fiber (3) has a double zero dispersion wavelength, and the output end is full positive dispersion; the working wavelength of the pump source (1) is located in the negative dispersion region of the incident end of the nonlinear optical fiber (3), close to the second zero dispersion wavelength position; when the pump light (1) is coupled into the nonlinear optical fiber (3), the pump light (1) is located in the anomalous dispersion region of the nonlinear optical fiber (3), and in the high-order soliton splitting, the pump light (1) is located in the anomalous dispersion region of the nonlinear optical fiber (3). Under the action of the soliton self-frequency shift effect, the generated optical soliton moves toward the long wave. Since the working wavelength of the pump source (1) is close to the second zero dispersion wavelength position of the nonlinear optical fiber (3), the generated optical soliton can quickly encounter the second zero dispersion wavelength of the nonlinear optical fiber (3) and radiate dispersion waves toward the long wave region to generate red-shifted dispersion waves. In the normal dispersion region of the nonlinear optical fiber (3), the red-shifted dispersion waves serve as seed light. Under the cascade action of the stimulated Raman scattering effect and the Raman amplification effect, their energy is increased, and finally a fiber-based broadband mid-infrared supercontinuum light source with a high energy proportion in the long wavelength spectral region is realized.
2. A method for increasing the energy proportion of a mid-infrared supercontinuum light source in the long-wavelength spectral region as claimed in claim 1, characterized in that: The output optical fiber of the pump source (1) is connected to the input optical fiber of the isolator (2) by direct fusion splicing, and the output optical fiber of the isolator (2) is connected to the nonlinear optical fiber (3) by direct fusion splicing or mechanical docking.
3. A method for increasing the energy proportion of a mid-infrared supercontinuum light source in a long-wavelength spectral region as claimed in claim 1, characterized in that: The pump source (1) is a femtosecond fiber laser, the central wavelength of the femtosecond fiber laser is 1.9-4 μm, the pulse width is 10 fs-10 ps, and the repetition frequency is 1 kHz-10 GHz.
4. A method for increasing the energy proportion of a mid-infrared supercontinuum light source in a long-wavelength spectral region as claimed in claim 1, characterized in that: The nonlinear optical fiber (3) is a fluorotellurite glass optical fiber or a chalcogenide glass optical fiber with a gradually decreasing core diameter.
5. A method for increasing the energy proportion of a mid-infrared supercontinuum light source in a long-wavelength spectral region as claimed in claim 4, characterized in that: The fluorotellurate glass optical fiber has a step refractive index structure, its core material is TeO2-BaF2-Y2O3, and its cladding material is AlF3-BaF2-CaF2-YF3-SrF2-MgF2-TeO2 glass; the total length of the optical fiber is 3m, the initial core diameter is 1.64μm, and the end core diameter is 0.9μm.