Salt bath composition, salt bath system and method for strengthening glass products
By using specific salt bath compositions and structural designs in the strengthening process of glass products, the problem of reduced chemical durability of glass in conventional processes is solved and higher chemical durability and mechanical strength are achieved.
Patent Information
- Application Number
- CN202180022483.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-02-24
AI Technical Summary
Conventional glass strengthening processes can reduce the chemical durability of the glass, especially due to surface damage and loss of mechanical strength caused by decomposition products of the molten salt bath.
Using a salt bath composition containing 90% to 99.9% alkali metal salts and 0.1% to 10% silicic acid aggregates, the silicic acid aggregates having an average size of 50 μm to 400 μm, and passing through a salt bath tank and sieve structure defining an internal volume, And a stirring device to control the distribution and reaction of silicic acid aggregates in the molten salt bath to reduce the generation of alkali metal oxides.
Effectively neutralizes the molten salt bath, reduces surface damage to glass products, improves chemical durability and mechanical strength, and prevents silicic acid aggregates from settling and adhering too quickly, extending the life of the salt bath.
Smart Images

Figure CN115362138B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority under 35 USC §119 to U.S. Provisional Application Serial No. 62 / 990,730, filed on March 17, 2020, the contents of which are hereby relied upon and incorporated herein by reference in their entirety. Technical Field
[0003] The present description relates generally to methods for chemically strengthening glass articles and, more particularly, to salt bath compositions, salt bath systems, and processes for strengthening glass articles. Background Art
[0004] Tempered or strengthened glass can be used in various applications. For example, due to the physical durability and crack resistance of strengthened glass, it can be used in consumer electronic devices, such as smart phones and tablet computers. Strengthened glass can also be used in pharmaceutical packaging. In such applications, in addition to physical durability, the chemical durability of glass is also important for preventing contamination of the contents of pharmaceutical packaging. However, conventional strengthening processes (e.g., conventional ion exchange processes) may reduce the chemical durability of glass. This may be due, at least in part, to degradation and / or decomposition of the molten salt bath used for ion exchange.
[0005] Therefore, there is a need for alternative salt bath compositions for strengthening glass articles. Summary of the invention
[0006] According to the first aspect, a salt bath composition for strengthening a glass article comprises: 90 wt % to 99.9 wt % of one or more alkali metal salts, based on the total weight of the salt bath composition; and 0.1 wt % to 10 wt % of silicic acid aggregates, based on the total weight of the salt bath composition, wherein the silicic acid aggregates have an average size of 50 μm to 200 μm.
[0007] A second aspect includes the salt bath composition of the first aspect, wherein at least 50% of the silicic acid aggregates have an average size of less than or equal to 200 μm.
[0008] A third aspect includes the salt bath composition of any of the first or second aspects, wherein at least 50% of the silicic acid aggregates have an average particle size of less than or equal to 50 μm.
[0009] The fourth aspect includes the salt bath composition of any one of the first to third aspects, wherein the specific surface area of the silicic acid aggregate is greater than or equal to 200 m 2 / g.
[0010] A fifth aspect includes the salt bath composition of any one of aspects 1 to 4, wherein the one or more alkali metal salts comprises potassium nitrate, sodium nitrate, lithium nitrate, or a combination thereof.
[0011] According to a sixth aspect, a salt bath system for strengthening a glass article comprises: a salt bath tank defining an interior volume enclosed by at least one sidewall; and a salt bath composition within the interior volume, the salt bath composition comprising: 90 wt % to 99.5 wt % of one or more alkali metal or alkaline earth metal salts, based on the total weight of the salt bath composition; and 0.1 wt % to 10 wt % of silicic acid aggregates, based on the total weight of the salt bath composition, wherein the silicic acid aggregates have an average size of 50 μm to 400 μm.
[0012] A seventh aspect includes the salt bath system of aspect six, wherein the system further comprises one or more screens connected to the sidewalls, wherein at least a portion of the silicic acid aggregates are contained within the one or more screens.
[0013] An eighth aspect includes the salt bath system of aspect 7, wherein the one or more screens have a screen number of 70 or greater.
[0014] A ninth aspect includes the salt bath system of any one of the seventh or eighth aspects, wherein the part of the silicic acid aggregates accounts for 25% to 80% of the total amount of the silicic acid aggregates.
[0015] A tenth aspect includes the salt bath system of any one of aspects 6 to 9, wherein the system further comprises a stirring device.
[0016] The 11th aspect comprises the salt bath system according to the 10th aspect, wherein the stirring device comprises a stirrer.
[0017] A twelfth aspect comprises the salt bath system of the tenth aspect, wherein the stirring device comprises a gas injection system.
[0018] A 13th aspect includes the salt bath system of any one of aspects 6 to 12, wherein the silicic acid aggregates have an average size of 50 μm to 200 μm.
[0019] A fourteenth aspect includes the salt bath system of any one of aspects 6 to 12, wherein the silicic acid aggregates have an average size of 200 μm to 400 μm.
[0020] A fifteenth aspect includes the salt bath system of any one of aspects six to fourteen, wherein at least 50% of the silicic acid aggregates have an average size of less than or equal to 400 μm.
[0021] A sixteenth aspect includes the salt bath system of any one of aspects six to fifteen, wherein at least 50% of the silicic acid aggregates have an average size greater than or equal to 50 μm.
[0022] A 17th aspect includes the salt bath system of any one of aspects 6 to 16, wherein the average surface area of the silicic acid aggregates is greater than or equal to 200 m 2 / g.
[0023] An eighteenth aspect includes the salt bath system of any one of aspects six to seventeen, wherein the one or more alkali metal salts comprise potassium nitrate, sodium nitrate, lithium nitrate, or a combination of these.
[0024] According to the 19th aspect, a method for strengthening a glass article comprises: heating a salt bath composition to an ion exchange temperature to form a molten salt bath composition, the salt bath composition comprising one or more alkali metal or alkaline earth metal salts; circulating the molten salt bath composition through a neutralization zone comprising silicic acid aggregates, the silicic acid aggregates having an average size of 50 μm to 400 μm; and immersing the glass article in the molten salt bath composition to cause ion exchange between the molten salt bath composition and the glass article.
[0025] Aspect 20 includes the method of aspect 19, wherein the neutralization zone comprises a packed bed of silicic acid aggregates.
[0026] Aspect 21 includes the method of aspect 20, wherein the packed bed is surrounded by a screen having a mesh number greater than or equal to 70.
[0027] Aspect 22 includes the method of any one of aspects 19 to 21, wherein the salt bath composition is circulated through the neutralization zone at a rate of 0.05 vol / hr (volume / hour) to 10 vol / hr.
[0028] Aspect 23 includes the method of any one of aspects 19 to 22, wherein at least 50% of the silicic acid aggregates have an average size of less than or equal to 400 μm.
[0029] A 24th aspect includes the method of any one of aspects 19 to 23, wherein at least 50% of the silicic acid aggregates have an average size greater than or equal to 50 μm.
[0030] A 21st aspect includes the method of any one of aspects 19 to 24, wherein the average surface area of the silicic acid aggregates is greater than or equal to 200 m 2 / g.
[0031] A 26th aspect includes the method of any one of aspects 19 to 25, wherein the one or more alkali metal salts comprises potassium nitrate, sodium nitrate, lithium nitrate, or a combination of these.
[0032] A twenty-seventh aspect includes the method of any one of aspects 19 to 26, wherein the salt bath composition comprises 90 wt % to 99.5 wt % of the one or more alkali metal or alkaline earth metal salts, based on the total weight of the salt bath composition.
[0033] Aspect 28 includes the method of any of aspects 19 to 27, wherein the neutralization zone comprises 0.1 wt % to 10 wt %, based on the total weight of the salt bath composition.
[0034] According to aspect 29, a method for loading a salt bath composition for strengthening a glass article comprises: adding a first solid layer comprising one or more alkali metal salts to the salt bath; adding a second solid layer comprising silicic acid aggregates to the salt bath; and adding a third solid layer comprising one or more alkali metal salts to the salt bath so that the second solid layer comprising silicic acid aggregates is located between the first solid layer and the third solid layer, wherein the sum of the weight percentage of the first solid layer and the weight percentage of the third solid layer accounts for 90 wt % to 99.5 wt % of the salt bath composition; and wherein the ratio of the weight percentage of the first solid layer to the weight percentage of the third solid layer is 1:4 to 4:1.
[0035] A 30th aspect includes the method of aspect 29, wherein the weight percentage of the second solid layer is 0.5 wt % to 10 wt %, based on the total weight of the salt bath composition.
[0036] Aspect 31 includes the method of any of aspects 29 or 30, wherein the method further comprises: heating the first solid layer, the second solid layer, and the third solid layer to form a molten salt bath.
[0037] A 32nd aspect includes the method of aspect 31, wherein the first solid layer, the second solid layer, and the third solid layer are heated to a temperature of 350°C to 500°C.
[0038] A 33rd aspect includes the method of any one of aspects 29 to 32, wherein the silicic acid aggregates have an average size of 50 μm to 400 μm.
[0039] A 34th aspect includes the method of any of aspects 29 to 33, wherein at least 50% of the silicic acid aggregates have an average size less than or equal to 400 μm.
[0040] Aspect 35 includes the method of any of aspects 29 to 34, wherein at least 50% of the silicic acid aggregates have an average size greater than or equal to 50 μm.
[0041] A 36th aspect includes the method of any one of aspects 29 to 35, wherein the average surface area of the silicic acid aggregates is greater than or equal to 200 m2 / g.
[0042] A 37th aspect includes the method of any one of aspects 29 to 36, wherein the one or more alkali metal salts comprises potassium nitrate, sodium nitrate, magnesium nitrate, calcium nitrate, or a combination of these.
[0043] According to the 38th aspect, a method for strengthening a glass article comprises: heating a salt bath composition to an ion exchange temperature to form a molten salt bath composition, the salt bath composition comprising one or more alkali metal or alkaline earth metal salts; immersing the glass article in the molten salt bath composition to cause ion exchange between the molten salt bath composition and the glass article; contacting the molten salt bath composition with silicic acid aggregates, the silicic acid aggregates having an average size of 50 μm to 400 μm; and immersing a second glass article in the molten salt bath composition to cause ion exchange between the molten salt bath composition and the second glass article.
[0044] A 39th aspect includes the method of aspect 38, further comprising: contacting the molten salt bath composition with silicic acid aggregates for a second time, the silicic acid aggregates having an average size of 50 μm to 400 μm; and immersing a third glass article in the molten salt bath composition to cause ion exchange between the molten salt bath composition and the third glass article.
[0045] A 40th aspect includes the method of any of aspects 38 or 39, wherein the glass article is removed from the molten salt bath prior to contacting the molten salt bath composition with the silicic acid aggregates.
[0046] Other features and advantages of the compositions, methods, and products described herein will be described in the following detailed description, some of which will be readily apparent to those skilled in the art from the description or recognized by practicing the embodiments described herein, including the following detailed description, claims, and drawings.
[0047] It should be understood that both the foregoing general description and the following detailed description describe various embodiments and are intended to provide an overall review or framework for understanding the nature and characteristics of the claimed subject matter. The included drawings provide a further understanding of the various embodiments, and the drawings are incorporated into and constitute a part of this specification. The drawings illustrate the various embodiments described herein and, together with the description, are used to explain the principles and operations of the claimed subject matter. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1A According to one or more embodiments shown and described herein, a portion of an ion exchange process is schematically depicted;
[0049] Figure 1B According to one or more embodiments shown and described herein, a portion of an ion exchange process is schematically depicted;
[0050] Figure 2A According to one or more embodiments shown and described herein, the surface hydrolysis resistance (SHR) of a glass article that has undergone ion exchange is illustrated;
[0051] Figure 2B According to one or more embodiments shown and described herein, the compressive stress (CS) of a glass article that has undergone ion exchange is illustrated;
[0052] Figure 2C According to one or more embodiments shown and described herein, the central tension (CT) of a glass article that has undergone ion exchange is illustrated;
[0053] Figure 2D According to one or more embodiments shown and described herein, the depth of compression (DOC) of a glass article that has undergone ion exchange is illustrated;
[0054] Figure 3 According to one or more embodiments shown and described herein, the relative fraction yield of defect-free glass articles produced by an ion exchange process is illustrated;
[0055] Figure 4 According to one or more embodiments shown and described herein, a salt bath system is schematically depicted;
[0056] Figure 5A According to one or more embodiments shown and described herein, a salt bath system is schematically depicted;
[0057] Figure 5B According to one or more embodiments shown and described herein, a salt bath system is schematically depicted;
[0058] Figure 5C According to one or more embodiments shown and described herein, a salt bath system is schematically depicted; and
[0059] Figure 6 According to one or more embodiments shown and described herein, a neutralization zone of a salt bath system is schematically depicted. DETAILED DESCRIPTION
[0060] Embodiments described herein relate to compositions, systems, and methods for strengthening glass products while also minimizing the concentration of decomposition products in a molten salt bath used in an ion exchange process to extend the life of the salt bath and maintain the chemical durability of the strengthened glass products over time. The salt bath composition may generally include 90% to 99.9% by weight of one or more alkali or metal salts and 0.1% to 10% by weight of silicic acid aggregates, based on the total weight of the salt bath composition. Various embodiments of the compositions, systems, and methods will be described herein with specific reference to the accompanying drawings.
[0061] Directional terms used herein, such as up, down, left, right, front, back, top, and bottom, are only used with reference to the drawings in which they are drawn and are not intended to imply an absolute orientation.
[0062] Unless otherwise expressly stated, any method described herein should not be construed as requiring that its steps be performed in a specific order, or requiring that any device have a particular orientation. Thus, if a method claim does not actually recite the order in which its steps are to be followed, or if any device claim does not actually recite the order or orientation of the components, or if the claims or specification do not otherwise specifically state that the steps are limited to a specific order, or if a specific order or orientation of the device components is not recited, then no order or orientation should be inferred in any respect. This applies to any possible non-expressive basis for interpretation, including: logical issues involving the arrangement of steps, operational flow, order of components, or orientation of components; issues of obvious meaning derived from grammatical organization or punctuation; and issues of the number or type of embodiments described in the specification.
[0063] Unless otherwise specified, the terms "ion exchange bath", "salt bath" and "molten salt bath" as used herein are equivalent terms and refer to a solution or medium used to achieve an ion exchange process with a glass (or glass ceramic) article, in which cations within the surface of the glass article are replaced or exchanged with cations present in the salt bath. It should be understood that the salt bath can include at least one alkali metal salt, such as potassium nitrate (KNO3) and / or sodium nitrate (NaNO3), which can be liquefied by heat or otherwise heated to a substantially liquid phase.
[0064] As used herein, the term "chemical durability" refers to the ability of a glass composition to resist degradation after exposure to specified chemical conditions. Specifically, the chemical durability of the glass articles described herein is determined according to USP <660> “Surface Glass Test” in “Containers–Glass”, evaluated in water.
[0065] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly indicates otherwise. Thus, for example, reference to "an" component includes aspects having two or more such components unless the context clearly indicates otherwise.
[0066] First reference Figure 1A and 1B , which schematically depicts a conventional ion exchange process. The ion exchange process includes immersing a glass article 105 in a salt bath 100. In embodiments, the glass article 105 may include a silicate glass, such as a borosilicate glass or an aluminosilicate glass, as described in the United States Pharmacopeia (USP) <660> As described in detail in “Containers—Glass” in USP 105, the glass meets the Type I glass standard. Type I glass generally has relatively high hydrolysis resistance and relatively high thermal shock resistance. In an embodiment, the glass article 105 may include the same as USP <660> Type III glass is generally soda-lime-silica glass. Type III glass has moderate hydrolytic resistance. In an embodiment, the glass article 105 may include the same as USP <660> Type II glass as described in. Type II glass is generally Type III glass that has been surface treated to improve the hydrolytic resistance of the glass.
[0067] Still reference Figure 1A The glass article 105 may include relatively small cations 130, such as alkali metal cations, such as Li + and / or Na + Cations. The salt bath 100 may include a molten salt 101 that is at an elevated temperature and contains relatively large cations 120 (i.e., relative to the cations 130 of the glass article). That is, the atomic radius of the larger cations 120 may be larger than the atomic radius of the smaller cations 130. The larger cations 120 may, for example, include alkali metal cations, such as potassium (K + ) and / or sodium (Na + ) cations. When heated to the elevated temperature of the molten salt 101, larger cations 120 may have dissociated from salts (e.g., alkali metal nitrates) present in the salt bath 100. When the glass article 105 is immersed in the salt bath 100, smaller cations 130 in the glass article 105 may diffuse from the glass article 105 into the molten salt 101. Referring now to Figure 1BAfter the diffusion, the larger cations 120 from the molten salt 101 can replace the smaller cations 130 in the glass article 105. This replacement of the smaller cations 130 in the glass article 105 by the larger cations 120 creates a surface compressive stress (CS) at the surface of the glass article 105, which extends to the depth of layer (DOL), which in turn can increase the mechanical strength of the glass article 105 and improve the crack resistance of the glass article 105.
[0068] It has been found that during the ion exchange process, metal nitrates (e.g., alkali metal nitrates) present in the salt bath can decompose into metal nitrites and / or metal oxides. For example, the following equation indicates the decomposition of alkali metal nitrates into alkali metal nitrites:
[0069] MNO3←→MNO2+1 / 2O2[M:IUPAC Group 1 metal]
[0070] Both alkali metal nitrates and alkali metal nitrites can further decompose into alkali metal oxides as indicated by the following equations:
[0071] MNO2←→M2O+NO x [M: IUPAC Group 1 metals]
[0072] For example, in the case of using potassium nitrate (KNO3) salt in the salt bath, it has been found that KNO3 decomposes into two major decomposition products: potassium nitrite (KNO2) and potassium oxide (K2O) at bath temperatures above about 400°C. It has been found that other alkali metal nitrates, such as sodium nitrate and lithium nitrate, can decompose into corresponding alkali metal nitrites and alkali metal oxides at temperatures lower than KNO3 (i.e., temperatures less than or equal to 400°C).
[0073] It has been determined that the presence of alkali metal oxides (e.g., KO) in a salt bath may degrade the properties of a glass article treated therein. In particular, it has been found that alkali metal oxides in a salt bath may undesirably etch the surface of the glass article during ion exchange. Such etching may damage the surface of the glass article, which in turn may adversely affect various properties of the glass article. For example, it has been found that a glass article subjected to ion exchange in a salt bath comprising KO at a concentration greater than or equal to 0.5 wt % may form visible etching and surface damage on the glass article. Even when the glass article is subjected to ion exchange in a salt bath comprising KO at a concentration less than 0.5 wt %, it has been found that the presence of KO may result in a significant decrease in the mechanical strength of the glass article.
[0074] By neutralizing the salt bath, damage to the surface of the glass article during ion exchange can be reduced or prevented. That is, by reducing or eliminating the alkali metal oxides present in the salt bath, damage to the surface of the glass article during ion exchange can be reduced or prevented. This can be achieved at least in part by including silicic acid in the salt bath. As used herein, the term "silicic acid" can refer to silicic acids, such as orthosilicic acid (Si(OH)4), and corresponding silicates, which are conjugate bases of silicic acid. Silicic acids can generally react with alkali metal oxides to form non-reactive products, as indicated by the following equation:
[0075] M2O+SiO2→M2SiO3[M:IUPAC Group 1 metal]
[0076] Without being bound by any particular theory, it is believed that the surface hydrolysis resistance (SHR) of glass articles that have been ion exchanged in a salt bath may be the most reliable indicator of the degree to which the salt bath has been neutralized. <660> The surface hydrolysis resistance of a glass article is measured by the Surface Glass Test described in detail in . When the surface hydrolysis resistance of a glass article is measured by the Surface Glass Test, a glass vial or container constituting the glass article is filled with water without carbon dioxide or purified water. The filled vial or container is then subjected to an autoclave cycle of about 1 hour at about 121° C. The resulting leachate in the vial or container is then titrated to neutrality by weak hydrochloric acid (e.g., 0.01M HCl) in the presence of methyl red. The volume of titrant per 100 mL of leachate is used to determine the surface hydrolysis resistance of the glass article. In general, a larger titrant volume corresponds to a poorer chemical durability (i.e., the leachate contains more glass components released by the glass, and therefore more titrant is required to compensate for the pH change caused by the presence of the glass components). Poor chemical durability, in turn, generally corresponds to greater damage to the surface of the glass article, and a greater concentration of alkali metal oxides in the salt bath used for ion exchange.
[0077] Low titrant volume and / or high chemical durability may be desired in a strengthened glass article. In general, a titrant volume of less than 1.5 mL is desired for type I glass. However, as described above, the presence of decomposition products (e.g., alkali hydroxides or alkali oxides) in the molten salt bath used for ion exchange may corrode and / or etch the surface of the glass article. Such etching may result in an increase in titrant volume, which corresponds to a decrease in chemical durability. Typically, the titrant volume of a strengthened glass article will increase according to the time spent undergoing ion exchange. That is, the longer the glass article is in contact with the molten salt bath, the larger the titrant volume. For example, a glass article that has undergone about 3 hours of ion exchange may result in a titrant volume of about 0.9 mL, while a glass article that has undergone about 10 hours of ion exchange may result in a titrant volume of about 1.1 mL.
[0078] Reference now Figure 2A , which shows the volume of titrant per 100 mL of leachate (i.e., titrant volume), and by extension, the surface hydrolysis resistance of glass products that have undergone ion exchange in a molten salt bath. Figure 2A As shown, when silicic acid is not present, the titrant volume generally increases over the course of 14 days, indicating the formation of alkali metal oxides in the molten salt bath and, as a result, surface damage to the glass article. Figure 2A It is also shown that the addition of silicic acid (i.e., "after SA") significantly reduces the titrant volume to an amount less than or similar to the initial titrant volume. That is, the inclusion of silicic acid in the salt bath composition or the addition of silicic acid to the molten salt bath has been shown to be able to effectively neutralize the molten salt bath. Similarly, reference is now made to Figure 2B , the compressive stress (CS) of the glass article steadily decreased over the course of 14 days. However, after the addition of silicic acid, the compressive stress achieved during the ion exchange process increased significantly and returned to the compressive stress value achieved when the molten salt bath was still fresh. This conclusion is supported by Figure 2C-2D For further support, Figure 2C-2D It was shown that when silicic acid was added to the molten salt bath used for multiple days, the central tension (CT) and depth of compression (DOC) of the strengthened glass articles increased significantly.
[0079] However, it has been found that when the average particle size of the silicate particles is too large, the silicate may not be able to effectively neutralize the molten salt bath. In particular, it has been found that when the average size of the silicate particles is too large, the silicate particles may quickly sink to the bottom of the molten salt bath, and as a result, the possibility of interaction and reaction between the silicate and the alkali metal oxide may be reduced. Therefore, the average size of the silicate particles can be reduced to increase the buoyancy of the silicate particles in the molten salt bath, and thus reduce the rate at which the silicate particles settle in the molten salt bath.
[0080] On the contrary, it has been found that when the average particle size of the silicic acid particles is too small, the silicic acid particles may adhere to the surface of the glass product subjected to ion exchange in the molten salt bath. Such adhesion of the silicic acid particles to the surface of the glass product may cause defects, making the glass product unsuitable for commercial use, or at least requiring additional processing, which increases production costs and reduces efficiency. For example, referring now to Figure 3 , the relative yield of defect-free strengthened glass articles produced in the molten salt bath gradually decreases over time. However, after the addition of silicic acid (as indicated by the dashed line), the relative yield of defect-free strengthened glass articles produced in the molten salt bath decreases dramatically, indicating that the presence of silicic acid in the molten salt bath may adversely affect the quality of the glass articles strengthened therein.
[0081] Thus, the present disclosure relates to salt bath compositions and salt bath systems for strengthening glass articles, and methods of strengthening glass articles, which use silicic acid to effectively neutralize a molten salt bath while also reducing or preventing silicic acid from adhering to the surface of the glass article undergoing ion exchange in the molten salt bath.
[0082] In an embodiment, the salt bath composition may include one or more alkali metal salts. For example, the salt bath composition may include potassium nitrate (KNO3), sodium nitrate (NaNO3), lithium nitrate (LiNO3), or a combination thereof. In an embodiment, based on the total weight of the salt bath composition, the salt bath composition may include 90 wt% to 99.9 wt% of the one or more alkali metal salts. For example, the salt bath composition can include 90% to 99.5% by weight, 90% to 99% by weight, 90% to 97% by weight, 90% to 95% by weight, 90% to 93% by weight, 93% to 99.9% by weight, 93% to 99.5% by weight, 93% to 99% by weight, 93% to 97% by weight, 93% to 95% by weight, 95% to 99.9% by weight, 95% to 99.5% by weight, 95% to 99% by weight, 95% to 97% by weight, 97% to 99.9% by weight, 97% to 99.5% by weight, 97% to 99% by weight, 99% to 99.9% by weight, 99% to 99.5% by weight, or 99.5% to 99.9% by weight of the one or more alkali metal salts, based on the total weight of the salt bath composition.
[0083] As described above, the salt bath composition may include potassium nitrate, sodium nitrate, lithium nitrate, or a combination thereof. In an embodiment, the salt bath composition may include 5% to 99.9% by weight of potassium nitrate based on the total weight of the salt bath composition. For example, based on the total weight of the salt bath composition, the salt bath composition may include 5% to 75% by weight, 5% to 50% by weight, 5% to 25% by weight, 25% to 99.9% by weight, 25% to 75% by weight, 25% to 50% by weight, 50% to 99.9% by weight, 50% to 75% by weight, or 75% to 99.9% by weight of potassium nitrate. In an embodiment, based on the total weight of the salt bath composition, the salt bath composition may include 5% to 99.9% by weight of sodium nitrate. For example, the salt bath composition may include 5% to 75% by weight, 5% to 50% by weight, 5% to 25% by weight, 25% to 99.9% by weight, 25% to 75% by weight, 25% to 50% by weight, 50% to 99.9% by weight, 50% to 75% by weight, or 75% to 99.9% by weight of sodium nitrate, based on the total weight of the salt bath composition. In embodiments, the concentration of the alkali metal salt in the salt bath composition may be balanced based on the composition of the glass article so that the ion exchange process provided both increases the surface compressive stress at the surface of the glass article after the ion exchange process and increases the compression depth after the ion exchange process. For example, the salt bath composition may include a greater concentration of potassium nitrate than the sodium nitrate concentration, or the salt bath composition may include a greater concentration of sodium nitrate than the potassium nitrate concentration, based on the total concentration of the salt bath composition. Without being bound by any particular theory, it is believed that a greater sodium nitrate concentration than potassium nitrate concentration in the salt bath composition combined with a longer residence time in the molten salt bath can result in a greater depth of compression in the glass article.
[0084] In an embodiment, the salt bath composition may include silicic acid aggregates. As used herein, the term "silicic acid aggregates" may refer to clusters or units formed by aggregating silicic acid nanoparticles into a single mass. As described above, silicic acid aggregates may react with the decomposition products of the one or more alkali metal salts in the salt bath composition to form non-reactive (e.g., non-etching or corroding the surface of the glass article) silicates and water. Therefore, when compared with glass articles subjected to an ion exchange process in a conventional molten salt bath (i.e., a molten salt bath that does not include silicic acid nanoaggregates), silicic acid aggregates may reduce the concentration of decomposition products of alkali metal salts in the molten salt bath, thereby increasing the chemical durability of the glass article.
[0085] The salt bath composition may include an amount of silicic acid aggregates sufficient to effectively reduce the concentration of the at least one decomposition product in the molten salt bath. In an embodiment, the salt bath composition may include 0.1 wt % to 10 wt % of silicic acid aggregates based on the total weight of the salt bath composition. For example, the salt bath composition may include 0.1 wt % to 7 wt %, 0.1 wt % to 5 wt %, 0.1 wt % to 3 wt %, 0.1 wt % to 1 wt %, 0.1 wt % to 0.5 wt %, 0.5 wt % to 10 wt %, 0.5 wt % to 7 wt %, 0.5 wt % to 5 wt %, 0.5 wt % to 3 wt %, 0.5 wt % to 1 wt %, 1 wt % to 10 wt %, 1 wt % to 7 wt %, 1 wt % to 5 wt %, 1 wt % to 3 wt %, 3 wt % to 10 wt %, 3 wt % to 7 wt %, 3 wt % to 5 wt %, 5 wt % to 10 wt %, 5 wt % to 7 wt %, 7 wt % to 10 wt % of silicic acid aggregates, based on the total weight of the salt bath composition. When the salt bath composition includes less silicic acid aggregates (i.e., less than 0.1 wt %), the availability of silicic acid aggregates in the molten salt bath may not be sufficient to effectively interact with the decomposition products. In contrast, when the salt bath composition includes more silicic acid aggregates (ie, greater than 10 wt %), the excess silicic acid aggregates may interfere with the ion exchange process, for example, adhere to and contaminate the surface of the glass article.
[0086] In an embodiment, the silicic acid aggregates may have an average particle size of 50 μm to 400 μm as measured by laser diffraction particle size analysis. For example, the silicic acid aggregates may have an average particle size of 50 μm to 350 μm, 50 μm to 300 μm, 50 μm to 250 μm, 50 μm to 200 μm, 200 μm to 400 μm, 200 μm to 350 μm, 200 μm to 300 μm, 200 μm to 250 μm, 250 μm to 400 μm, 250 μm to 350 μm, 250 μm to 300 μm, 300 μm to 400 μm, 300 μm to 350 μm, or 350 μm to 400 μm as measured by laser diffraction particle size analysis. In such an embodiment, at least 50% of the silicic acid aggregates may have an average particle size of less than 400 μm as measured by laser diffraction particle size analysis. For example, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, or at least 85% of the silicic acid aggregates may have an average particle size of less than 400 μm as measured by laser diffraction particle size analysis. In addition, at least 50% of the silicic acid aggregates may have an average particle size of less than 375 μm, less than 350 μm, less than 325 μm, less than 300 μm, less than 275 μm, less than 250 μm, less than 225 μm, less than 200 μm, or less than 175 μm as measured by laser diffraction particle size analysis. In addition, at least 50% of the silicic acid aggregates may have an average particle size greater than 50 μm as measured by laser diffraction particle size analysis. For example, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, or at least 85% of the silicic acid aggregates may have an average particle size greater than 50 μm, as measured by laser diffraction particle size analysis. Additionally, at least 50% of the silicic acid aggregates may have an average particle size greater than 175 μm, greater than 200 μm, greater than 225 μm, greater than 250 μm, greater than 275 μm, greater than 300 μm, greater than 325 μm, greater than 350 μm, or greater than 375 μm, as measured by laser diffraction particle size analysis. Without being bound by any particular theory, it is believed that silicic acid aggregates with an average particle size smaller (i.e., less than 50 μm) may tend to adhere to the surface of the glass article and cause defects, making the glass article unsuitable for commercial use.
[0087] However, as described above, without some means to ensure the availability of silicic acid aggregates in the molten salt bath, silicic acid aggregates with a larger average particle size (i.e., greater than 200 μm) may not be able to effectively neutralize the molten salt bath. Therefore, in an embodiment, the silicic acid aggregates may have an average particle size of 50 μm to 200 μm as measured by laser diffraction particle size analysis. For example, as measured by laser diffraction particle size analysis, the silicic acid aggregates may have an average particle size of 50 μm to 180 μm, 50 μm to 160 μm, 50 μm to 140 μm, 50 μm to 120 μm, 120 μm to 200 μm, 120 μm to 180 μm, 120 μm to 160 μm, 120 μm to 140 μm, 140 μm to 200 μm, 140 μm to 180 μm, 140 μm to 160 μm, 160 μm to 200 μm, 160 μm to 180 μm, or 180 μm to 200 μm. In an embodiment, at least 50% of the silicic acid aggregates may have an average particle size of less than 200 μm as measured by laser diffraction particle size analysis. For example, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, or at least 85% of the silicic acid aggregates may have an average particle size of less than 200 μm, as measured by laser diffraction particle size analysis. In addition, at least 50% of the silicic acid aggregates may have an average particle size of less than 190 μm, less than 180 μm, less than 170 μm, less than 160 μm, less than 150 μm, less than 140 μm, less than 130 μm, less than 120 μm, or less than 110 μm, as measured by laser diffraction particle size analysis. In an embodiment, at least 50% of the silicic acid aggregates may have an average particle size greater than 50 μm, as measured by laser diffraction particle size analysis. For example, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, or at least 85% of the silicic acid aggregates may have an average particle size greater than 50 μm, as measured by laser diffraction particle size analysis. Additionally, at least 50% of the silicic acid aggregates may have an average particle size greater than 110 μm, greater than 120 μm, greater than 130 μm, greater than 140 μm, greater than 150 μm, greater than 160 μm, greater than 170 μm, greater than 180 μm, or greater than 190 μm, as measured by laser diffraction particle size analysis. Without being bound by any particular theory, it is believed that silicic acid aggregates with an average particle size greater than 400 μm may settle to the bottom of the salt bath too quickly and thus fail to effectively interact with the decomposition products of the alkali metal salt.
[0088] In an embodiment, the specific surface area of the silicic acid aggregates may be greater than or equal to 200 m2 as measured by the Brunauer-Emmett-Teller (BET) method. 2 / g. For example, the specific surface area of silicic acid aggregates can be 200m 2 / g to 600m 2 / g,200m 2 / g to 550m 2 / g,200m 2 / g to 500m 2 / g,200m 2 / g to 450m 2 / g,200m 2 / g to 400m 2 / g,200m 2 / g to 350m 2 / g,200m 2 / g to 300m 2 / g,200m 2 / g to 250m 2 / g,250m 2 / g to 600m 2 / g,250m 2 / g to 550m 2 / g,250m 2 / g to 500m 2 / g,250m 2 / g to 450m 2 / g,250m 2 / g to 400m 2 / g,250m 2 / g to 350m 2 / g,250m 2 / g to 300m 2 / g,300m 2 / g to 600m 2 / g,300m 2 / g to 550m 2 / g,300m 2 / g to 500m 2 / g,300m 2 / g to 450m 2 / g,300m 2 / g to 400m 2 / g,300m 2 / g to 350m 2 / g,350m 2 / g to 600m 2 / g,350m 2 / g to 550m 2 / g,350m 2 / g to 500m 2 / g,350m 2 / g to 450m 2 / g,350m 2 / g to 400m 2 / g,400m 2 / g to 600m 2 / g,400m 2 / g to 550m 2 / g,400m 2 / g to 500m 2 / g,400m 2 / g to 450m 2 / g,450m 2 / g to 600m 2 / g,450m 2 / g to 550m 2 / g,450m 2 / g to 500m 2 / g,500m 2 / g to 600m 2 / g,500m 2 / g to 550m 2 / g, or 550m 2 / g to 600m 2 / g. Without being bound by any particular theory, it is believed that the specific surface area of the silicic acid aggregates can be directly related to the reaction rate constant (k) of the reaction between the silicic acid aggregates and the decomposition products of the alkali metal salt, as described herein. That is, the larger the specific surface area of the silicic acid aggregates, the greater the potential for reaction with the decomposition products present in the molten salt bath. This can allow for better control of the properties of the salt bath composition and increase the chemical durability of the glass article while using less silicic acid aggregates.
[0089] As described above, the salt bath composition of the present disclosure can be used to implement an ion exchange process, so that the alkali metal cations of the glass product are exchanged with the alkali metal cations in the alkali metal salt of the salt bath composition. Therefore, the salt bath composition of the present disclosure can be used in a salt bath system or method for strengthening glass products.
[0090] In practice, the salt bath composition of the present disclosure may first be loaded into a salt bath tank. Figure 4, which generally depicts a salt bath system 200. In embodiments, the salt bath system 200 may include a salt bath tank 210, which generally defines an interior volume, which is bounded by at least one sidewall 220. The salt bath composition of the present disclosure may generally be loaded into the salt bath tank 210 as a single composition, or each component of the salt bath composition (e.g., alkali metal salt and silicate aggregate) may be loaded into the salt bath tank 210 separately. That is, each component of the salt bath composition may be loaded into the salt bath tank 210 as a separate layer. For example, Figure 4 As shown, the salt bath composition can be loaded into the salt bath tank 210 as a first solid layer 270, a second solid layer 280, and a third solid layer 290. That is, the first solid layer 270 can be added to the salt bath tank 210, then the second solid layer 280 can be added to the salt bath tank 210, and then the third solid layer 290 can be added to the salt bath tank 210, so that the second solid layer 280 is located between the first solid layer 270 and the third solid layer 290. It should be understood that any number of layers can be used when loading the salt bath composition into the salt bath tank 210. For example, in an embodiment where the salt bath composition includes three different alkali metal salts and silicic acid aggregates, at least four layers (i.e., one layer of each component) can be used when loading the salt bath tank 210.
[0091] Still reference Figure 4 In an embodiment, the first solid layer 270 may include the one or more alkali metal salts of the salt bath composition. For example, the first solid layer 270 may include potassium nitrate, sodium nitrate, lithium nitrate, or a combination thereof. In an embodiment, the first solid layer 270 may include greater than or equal to 90% by weight of the one or more alkali metal salts of the salt bath composition, based on the total weight of the first solid layer 270. For example, the first solid layer 270 may include greater than or equal to 93% by weight, greater than or equal to 95% by weight, greater than or equal to 97% by weight, greater than or equal to 99% by weight, greater than or equal to 99.5% by weight, or greater than or equal to 99.9% by weight of the one or more alkali metal salts in the salt bath composition, based on the total weight of the first solid layer 270.
[0092] In an embodiment, the second solid layer 280 may include the silicic acid aggregates 240 in the salt bath composition. Accordingly, based on the total weight of the second solid layer 280, the second solid layer 280 may include greater than or equal to 90% by weight of the silicic acid aggregates 240 in the salt bath composition. For example, based on the total weight of the second solid layer 280, the second solid layer 280 may include greater than or equal to 93% by weight, greater than or equal to 95% by weight, greater than or equal to 97% by weight, greater than or equal to 99% by weight, greater than or equal to 99.5% by weight, or greater than or equal to 99.9% by weight of the silicic acid aggregates in the salt bath composition. In an embodiment, the second solid layer 280 may include all or most of the silicic acid aggregates 240 in the salt bath composition. That is, the second solid layer 280 may include greater than or equal to 90% of the silicic acid aggregates 240 in the salt bath composition. For example, the second solid layer 280 may contain greater than or equal to 93%, greater than or equal to 95%, greater than or equal to 97%, greater than or equal to 99%, greater than or equal to 99.5%, or greater than or equal to 99.9% of the silicic acid aggregates 240 in the salt bath composition. Therefore, the weight percentage of the second solid layer 280 may be 0.1 wt % to 10 wt % of the salt bath composition. For example, the weight percentage of the second solid layer 280 can be 0.1 wt % to 7 wt %, 0.1 wt % to 5 wt %, 0.1 wt % to 3 wt %, 0.1 wt % to 1 wt %, 0.1 wt % to 0.5 wt %, 0.5 wt % to 10 wt %, 0.5 wt % to 7 wt %, 0.5 wt % to 5 wt %, 0.5 wt % to 3 wt %, 0.5 wt % to 1 wt %, 1 wt % to 10 wt %, 1 wt % to 7 wt %, 1 wt % to 5 wt %, 1 wt % to 3 wt %, 3 wt % to 10 wt %, 3 wt % to 7 wt %, 3 wt % to 5 wt %, 5 wt % to 10 wt %, 5 wt % to 7 wt %, or 7 wt % to 10 wt %.
[0093] In an embodiment, the third solid layer 290 may include one or more alkali metal salts of the salt bath composition. For example, the third solid layer 290 may include potassium nitrate, sodium nitrate, lithium nitrate, or a combination thereof. In an embodiment, the third solid layer 290 may include greater than or equal to 90% by weight of the one or more alkali metal salts of the salt bath composition, based on the total weight of the third solid layer 290. For example, based on the total weight of the third solid layer 290, the third solid layer 290 may include greater than or equal to 93% by weight, greater than or equal to 95% by weight, greater than or equal to 97% by weight, greater than or equal to 99% by weight, greater than or equal to 99.5% by weight, or greater than or equal to 99.9% by weight of the one or more alkali metal salts of the salt bath composition.
[0094] As described above, in an embodiment, the first solid layer 270 and the third solid layer 290 may each contain one or more alkali metal salts of the salt bath composition. In an embodiment, the first solid layer 270 and the third solid layer 290 together may contain one or more alkali metal salts of all or most of the salt bath composition. That is, the first solid layer 270 and the third solid layer 290 together may contain one or more alkali metal salts of the salt bath composition greater than or equal to 90%. For example, the first solid layer 270 and the third solid layer 290 together may contain greater than or equal to 93%, greater than or equal to 95%, greater than or equal to 97%, greater than or equal to 99%, greater than or equal to 99.5%, or greater than or equal to 99.9% of the salt bath composition. One or more alkali metal salts. Therefore, the sum of the weight percentages of the first solid layer 270 and the third solid layer 290 may be 90% to 99.5% by weight of the salt bath composition. For example, the sum of the first solid layer 270 and the third solid layer 290 can be 90 wt % to 99.5 wt %, 90 wt % to 99 wt %, 90 wt % to 97 wt %, 90 wt % to 95 wt %, 90 wt % to 93 wt %, 93 wt % to 99.9 wt %, 93 wt % to 99.5 wt %, 93 wt % to 99 wt %, 93 wt % to 97 wt %, 93 wt % to 95 wt %, 95 wt % to 99.9 wt %, 95 wt % to 99.5 wt %, 95 wt % to 99 wt %, 95 wt % to 97 wt %, 97 wt % to 99.9 wt %, 97 wt % to 99.5 wt %, 97 wt % to 99 wt %, 99 wt % to 99.9 wt %, 99 wt % to 99.5 wt %, or 99.5 wt % to 99.9 wt % of the salt bath composition.
[0095] In an embodiment, the ratio of the weight percentage of the first solid layer 270 to the weight percentage of the third solid layer 290 may be 1:4 to 4:1. For example, the ratio of the weight percentage of the first solid layer 270 to the weight percentage of the third solid layer 290 may be 1:4 to 3.5:1, 1:4 to 3:1, 1:4 to 2.5:1, 1:4 to 2:1, 1:4 to 1.5:1, 1:4 to 1:1, 1:4 to 1:2, 1:2 to 4:1, 1:2 to 3.5:1, 1:2 to 3:1, 1:2 to 2.5:1, 1:2 to 2:1, 1:2 to 1.5:1, 1:2 to 1:1, 1:1 to 4:1, 1:1 to 3.5:1, 1:1 to 3:1, 1:1 to 2.5:1, 1:1 to 2:1, 1:1 to 1.5:1, 1.5:1 to 4:1, 1.5:1 to 3.5:1, 1.5:1 to 3:1, 1.5:1 to 2.5:1, 1.5:1 to 2:1, 2:1 to 4:1, 2:1 to 3.5:1, 2:1 to 3:1, 2:1 to 2.5:1, 2.5:1 to 4:1, 2.5:1 to 3.5:1, 2.5:1 to 3:1, 3:1 to 4:1, 3:1 to 3.5:1, or 3.5:1 to 4:1.
[0096] Without being bound by any particular theory, it is believed that loading the salt bath tank in this manner (e.g., adding a portion of the alkali metal salt, followed by the addition of the silicic acid aggregates, followed by the remaining alkali metal salt, each of which is added in a layered structure) and then heating the salt bath composition to form a molten salt bath can more effectively include the silicic acid aggregates in the molten salt bath. For example, attempting to add the silicic acid aggregates to the salt bath tank after the molten salt bath has been formed can result in various undesirable effects. In particular, adding the silicic acid aggregates to the molten salt bath may result in a large portion of the silicic acid remaining on the surface of the bath in the form of a solid powder for a period of time. This may result in increased contamination of the glass article because the glass article is removed from the molten salt bath during this period.
[0097] Once the salt bath composition (e.g., first solid layer 270, second solid layer 280, and third solid layer 190) is loaded into salt bath tank 210, the salt bath composition may be heated to an elevated temperature (also referred to as an ion exchange temperature) sufficient to produce a molten salt bath and thereby facilitate an ion exchange process. In an embodiment, the salt bath composition may be heated to a temperature of 350°C to 500°C. For example, the salt bath composition may be heated to a temperature of 350° C. to 475° C., 350° C. to 450° C., 350° C. to 425° C., 350° C. to 400° C., 350° C. to 375° C., 375° C. to 500° C., 375° C. to 475° C., 375° C. to 450° C., 375° C. to 425° C., 375° C. to 400° C., 400° C. to 500° C., 400° C. to 475° C., 400° C. to 450° C., 400° C. to 425° C., 425° C. to 500° C., 425° C. to 475° C., 425° C. to 450° C., 450° C. to 500° C., 450° C. to 475° C., or 475° C. to 500° C. However, if the temperature of the molten salt bath is too high, it may be difficult to adequately control the ion exchange process, and the degradation rate of the alkali metal salt in the salt bath may increase.
[0098] As described above, the silicic acid aggregates can be suspended in the molten salt bath and settle to the bottom of the molten salt bath at different rates. Figure 5A , which depicts the salt bath system 200 after the salt bath composition is heated to the ion exchange temperature and a molten salt bath 230 is formed. Figure 5A As shown, the silicic acid aggregates 240 can be dispersed throughout the molten salt bath 230, wherein a portion of the silicic acid aggregates are suspended and a portion of the silicic acid aggregates are at the bottom of the molten salt bath 230. As described above, silicic acid aggregates with a larger average particle size (i.e., greater than 400 μm) may settle to the bottom of the salt bath tank too quickly and thus fail to effectively interact with the decomposition products of the alkali metal salt. Therefore, in an embodiment, the salt bath system 200 may include one or more means to increase the availability of silicic acid aggregates in the molten salt bath 230.
[0099] For example, now refer to Figure 5B, at least a portion of the silicate aggregates 240 can be contained in one or more screens (e.g., screen 250) connected to the side wall 220 of the salt bath tank 210. The screen 250 can include an opening, a screen structure, and the screen structure accommodates the silicate aggregates while also allowing the molten salt to pass through the screen and interact with the silicate aggregates. The screen can allow the silicate aggregates to be dispersed in various locations in the molten salt bath 230, thereby increasing the overall availability of the silicate aggregates and allowing the molten salt bath 230 to be more effectively neutralized. These screens can also prevent the silicate aggregates from sinking to the bottom of the molten salt bath 230 too quickly, thereby increasing the interaction between the silicate aggregates 240 and the decomposition products formed in the molten salt bath 230.
[0100] In an embodiment, the screen 250 may be composed of a mesh sufficient to allow the molten salt bath 230 to pass through the screen 250 while also preventing the silicic acid aggregates 240 from leaving the screen 250. That is, the average opening size of the mesh is smaller than the average particle size of the silicic acid aggregates contained in the screen 250. Therefore, the silicic acid aggregates 240 can effectively neutralize the molten salt bath 230 while also avoiding contact and contaminating the surface of the glass article. Therefore, the one or more screens (e.g., screen 250) of the salt bath system 200 may have a mesh number greater than or equal to 70. For example, the one or more screens (e.g., screen 250) of the salt bath system 200 may have a mesh number of 70, 80, 100, 120, 140, 170, 200, 230, 270, 325, 400, 450, 500, or 635, based on the American National Standard for Industrial Wire Cloth (ASTM-E11).
[0101] In an embodiment, the one or more screens (e.g., screen 250) of the salt bath system 200 may contain an amount of silicic acid aggregates sufficient to effectively neutralize the molten salt bath 230. Thus, the portion of silicic acid aggregates contained in the one or more screens may account for 25% to 80% of the total amount of silicic acid aggregates in the salt bath composition. For example, the portion of silicic acid aggregates contained in the one or more screens may account for 25% to 75%, 25% to 65%, 25% to 55%, 25% to 45%, 25% to 35%, 35% to 80%, 35% to 75%, 35% to 65%, 35% to 55%, 35% to 45%, 45% to 80%, 45% to 75%, 45% to 65%, 45% to 55%, 55% to 80%, 55% to 75%, 55% to 65%, 65% to 80%, 65% to 75%, or 75% to 80% of the total amount of silicic acid aggregates in the salt bath composition.
[0102] Additionally or alternatively, the salt bath system 200 may include a stirring device, such as a stirrer or a gas injection system, which may function to circulate the molten salt bath 230 in the salt bath tank 210. Referring now to Figure 5C , the salt bath system 200 may include a stirrer 260. The stirrer 260 may stir the molten salt bath 230, thereby causing the silicic acid aggregates 240 to rise from the bottom of the molten salt bath 230, or causing a portion of the molten salt bath 230 (including the decomposition products) to contact the silicic acid aggregates 240. As a result, such stirring may allow the molten salt bath 230 to be effectively neutralized, even in embodiments where the silicic acid aggregates have a large average particle size (i.e., greater than 400 μm) and thus cause the silicic acid aggregates to settle to the bottom of the salt bath tank too quickly.
[0103] In embodiments, the molten salt bath may be circulated through a neutralization zone containing silicic acid aggregates rather than including silicic acid aggregates in the molten salt bath composition. For example, the molten salt bath may be pumped or passed through a packed bed of silicic acid aggregates in order to neutralize the molten salt bath. More simply, the silicic acid aggregates may be used as a filter material to remove decomposition products from the molten salt bath between uses rather than actively reacting with the decomposition products in the molten salt bath. Reference is now made to Figure 6 , which shows an example of a neutralization zone or packed bed of silicate aggregates. Figure 6 As shown, the neutralization zone 310 may include a plurality of silicic acid aggregates 240 confined at either end by a first screen 312 and a second screen 314. A molten salt bath containing decomposition products (e.g., a molten salt bath that has been used to strengthen one or more glass articles) may pass through the neutralization zone 310, and as a result, the decomposition products will contact and react with the silicic acid aggregates 240. For example, Figure 6 As shown by the arrows in , the molten salt bath can enter the neutralization zone 310 by passing through the first screen 312, contact the silicic acid aggregate 240, and leave the neutralization zone 310 by passing through the second screen 314. This can effectively neutralize the molten salt bath.
[0104] As described above, the neutralization zone 310 may include a packed bed of silicic acid aggregates, and in some embodiments, may be surrounded by one or more screens, for example, a first screen 312 and a second screen 314. In an embodiment, the one or more screens may be composed of a mesh sufficient to allow the molten salt bath to pass through the screen while also preventing the silicic acid aggregates 240 from leaving the neutralization zone 310. That is, the average opening size of the mesh may be smaller than the average particle size of the silicic acid aggregates contained in the neutralization zone 310. Therefore, the one or more screens may have a mesh number greater than or equal to 70. For example, the one or more screens may have a mesh number of 70, 80, 100, 120, 140, 170, 200, 230, 270, 325, 400, 450, 500, or 635, based on the American National Industrial Wire Cloth Standard (American Standard ASTM-E11).
[0105] In an embodiment, the molten salt bath may be circulated through the neutralization zone 310 at a rate sufficient to effectively neutralize the molten salt bath. Thus, the molten salt bath may be circulated through the neutralization zone 310 at a rate of 0.05 vol / hr (volume / hour) to 10 vol / hr. More simply, 5% to 1000% of the total volume of the molten salt bath may be circulated through the neutralization zone per hour. In an embodiment, the molten salt bath may be circulated through the neutralization zone 310 at a rate of 0.05 vol / hr to 8 vol / hr, 0.05 vol / hr to 6 vol / hr, 0.05 vol / hr to 4 vol / hr, 0.05 vol / hr to 2 vol / hr, 2 vol / hr to 10 vol / hr, 2 vol / hr to 8 vol / hr, 2 vol / hr to 6 vol / hr, 2 vol / hr to 4 vol / hr, 4 vol / hr to 10 vol / hr, 4 vol / hr to 8 vol / hr, 4 vol / hr to 6 vol / hr, 6 vol / hr to 10 vol / hr, 6 vol / hr to 8 vol / hr, or 8 vol / hr to 10 vol / hr.
[0106] As described above, after the salt bath composition has been heated to an ion exchange temperature to form a molten salt bath, and before or after optional circulation or stirring occurs, the glass article can be immersed in a molten salt bath to achieve ion exchange between the molten salt bath and the glass article. The glass article can be contacted with a molten salt bath for a certain treatment time, which is sufficient to establish a surface compressive stress at the surface of the glass article, and the surface compressive stress extends to a compression depth. In an embodiment, the glass article can be contacted with a molten salt bath for a treatment time of about 20 minutes to about 20 hours. For example, the glass article can be contacted with a molten salt bath for the following treatment time: about 20 minutes to about 15 hours, about 20 minutes to about 10 hours, about 20 minutes to about 5 hours, about 20 minutes to about 1 hour, about 1 hour to about 20 hours, about 1 hour to about 15 hours, about 1 hour to about 10 hours, about 1 hour to about 5 hours, about 5 hours to about 20 hours, about 5 hours to about 15 hours, about 5 hours to about 10 hours, about 10 hours to about 20 hours, about 10 hours to about 15 hours, or about 15 hours to about 20 hours.
[0107] In an embodiment, after the ion exchange process, the contact of the glass article with the molten salt bath is removed. The resulting glass article that has undergone ion exchange may have a compressive stress at its surface that extends to a compression depth. The compressive stress and the compression depth increase the resistance of the glass article to breakage after mechanical damage, and thus, after the ion exchange process, the glass article may be a strengthened glass article. However, due to the neutralization effect of the silicic acid aggregates as described above, the strengthened glass article may retain or even exhibit improved chemical durability, as indicated by the SHR titrant volume after ion exchange. Thus, in embodiments, the SHR titrant volume of the strengthened glass article can be less than 1.5 mL, less than or equal to 1.4 mL, less than or equal to 1.3 mL, less than or equal to 1.2 mL, less than or equal to 1.1 mL, less than or equal to 1 mL, less than or equal to 0.9 mL, less than or equal to 0.8 mL, less than or equal to 0.7 mL, less than or equal to 0.6 mL, less than or equal to 0.5 mL, less than or equal to 0.4 mL, less than or equal to 0.3 mL, less than or equal to 0.2 mL, or even less than or equal to 0.1 mL.
[0108] In embodiments, after removal of contact, the strengthened glass article may be cleaned or washed. Specifically, as described above, the ion exchange process may result in deposition of alkali metal cations on the surface of the glass article. The ion exchange process may also result in deposition of metal oxide nanoparticles on the surface of the glass article as well. Washing of the strengthened glass article may remove at least a portion of the alkali metal cations and / or alkali metal oxide nanoparticles. This may further prepare the glass article for use in a desired application, such as, for example, pharmaceutical packaging.
[0109] The glass articles subjected to the ion exchange process and salt bath composition described herein can have various forms. For example, the glass article can be a glass plate, a glass sheet, a glass tube, a glass container, etc. In an embodiment, the glass article can be a glass pharmaceutical package or pharmaceutical container, which is used to contain a pharmaceutical composition, such as a liquid, a powder, etc. For example, the glass article described herein can be Cartridges, syringes, ampoules, bottles, jars, flasks, vials, tubes, beakers, vials, etc.
[0110] It is obvious to those skilled in the art that various modifications and changes can be made to the embodiments described herein without departing from the spirit and scope of the subject matter of the patent right. Therefore, this specification is intended to cover the modifications and variations of the various embodiments described herein, provided that these modifications and variations fall within the scope of the attached claims and their equivalents.
Claims
1. A salt bath composition for strengthening a glass product, the salt bath composition comprising: 90 wt % to 99.9 wt % of one or more alkali metal salts, based on the total weight of the salt bath composition; and 0.1 to 10 wt. % of silicic acid aggregates, based on the total weight of the salt bath composition, in, The silicic acid aggregates have an average size of 50 μm to 200 μm.
2. The salt bath composition according to claim 1, wherein At least 50% of the silicic acid aggregates have an average size less than or equal to 200 μm.
3. The salt bath composition according to claim 1, wherein At least 50% of the silicic acid aggregates have an average size greater than or equal to 50 μm.
4. The salt bath composition according to claim 1, wherein The specific surface area of silicic acid aggregate is greater than or equal to 200m 2 / g.
5. The salt bath composition according to claim 1, wherein The one or more alkali metal salts include potassium nitrate, sodium nitrate, lithium nitrate, or a combination of these.
6. A salt bath system for strengthening glass products, the salt bath system comprising: a salt bath tank defining an interior volume, the interior volume being enclosed by at least one side wall; and A salt bath composition, the salt bath composition being in the internal volume and comprising: 90 wt % to 99.5 wt % of one or more alkali metal salts, based on the total weight of the salt bath composition; and 0.1 to 10 wt. % of silicic acid aggregates, based on the total weight of the salt bath composition, The silicic acid aggregates have an average size of 50 μm to 400 μm.
7. The salt bath system according to claim 6, wherein: The system further includes one or more screens connected to the sidewall, wherein at least a portion of the silicic acid aggregates are contained within the one or more screens.
8. The salt bath system according to claim 7, wherein: The one or more screens have a screen number greater than or equal to 70.
9. The salt bath system according to claim 7, wherein: The silicic acid aggregates in said part account for 25% to 80% of the total amount of silicic acid aggregates.
10. The salt bath system according to claim 6, wherein: The system also includes a stirring device.
11. The salt bath system according to claim 6, wherein: The silicic acid aggregates have an average size of 50 μm to 200 μm.
12. The salt bath system according to claim 6, wherein: The silicic acid aggregates have an average size of 200 μm to 400 μm.
13. The salt bath system according to claim 6, wherein: At least 50% of the silicic acid aggregates have an average size less than or equal to 400 μm.
14. The salt bath system according to claim 6, wherein: At least 50% of the silicic acid aggregates have an average size greater than or equal to 50 μm.
15. The salt bath system according to claim 6, wherein: The average surface area of the silicate aggregates is greater than or equal to 200 m 2 / g.
16. The salt bath system according to claim 6, wherein: The one or more alkali metal salts include potassium nitrate, sodium nitrate, lithium nitrate, or a combination of these.
17. A method for strengthening a glass product, the method comprising: heating a salt bath composition to an ion exchange temperature to form a molten salt bath composition, the salt bath composition comprising one or more alkali metal salts; circulating the molten salt bath composition through a neutralization zone comprising silicic acid aggregates having an average size of 50 μm to 400 μm; as well as immersing the glass article in the molten salt bath composition to effect ion exchange between the molten salt bath composition and the glass article, wherein, based on the total weight of the salt bath composition, the salt bath composition comprises 90 wt % to 99.5 wt % of the one or more alkali metal salts; The neutralization region accounts for 0.1 wt % to 10 wt % based on the total weight of the salt bath composition.
18. The method of claim 17, wherein: The neutralization zone comprises a packed bed of silicic acid aggregates.
19. The method of claim 18, wherein: The packed bed is surrounded by a screen with a mesh number greater than or equal to 70.
20. The method of claim 17, wherein: The salt bath composition is circulated through the neutralization zone at a rate of 0.05 volume / hour to 10 volume / hour.
21. The method of claim 17, wherein: At least 50% of the silicic acid aggregates have an average size less than or equal to 400 μm.
22. The method of claim 19, wherein: At least 50% of the silicic acid aggregates have an average size greater than or equal to 50 μm.
23. The method of claim 17, wherein: The average surface area of the silicate aggregates is greater than or equal to 200 m 2 / g.
24. The method of claim 17, wherein: The one or more alkali metal salts include potassium nitrate, sodium nitrate, lithium nitrate, or a combination of these.
25. A method of loading a salt bath composition for strengthening a glass article, the method comprising: adding a first solid layer comprising one or more alkali metal salts to a salt bath tank; adding a second solid layer comprising silicic acid aggregates to the salt bath; as well as adding a third solid layer comprising one or more alkali metal salts to the salt bath so that the second solid layer comprising silicic acid aggregates is located between the first solid layer and the second solid layer, wherein the sum of the weight percentage of the first solid layer and the weight percentage of the third solid layer is 90 weight % to 99.5 weight % of the salt bath composition; wherein the ratio of the weight percentage of the first solid layer to the weight percentage of the third solid layer is 1:4 to 4:1; Wherein, based on the total weight of the salt bath composition, the weight percentage of the second solid layer is 0.5 wt % to 10 wt %; The silicic acid aggregates have an average size of 50 μm to 400 μm.
26. The method of claim 25, wherein: The method also includes heating the first solid layer, the second solid layer, and the third solid layer to form a molten salt bath.
27. The method of claim 26, wherein: The first layer, the second solid layer and the third solid layer are heated to a temperature of 350°C to 500°C.
Citation Information
Patent Citations
Strengthened microcrystalline glass with high-pressure stress layer depth and preparation method thereof
CN110845153A
Process for the production of precipitated silica and process for measuring the low abrasion factor
DE102015214344A1