Gas-phase synthesis process of high-purity silicon dioxide
The process of reacting fluorosilicate and quartz sand to generate silicon tetrafluoride gas and performing recycling, solving the problems of high-temperature hydrolysis equipment and scarce raw materials in the existing technology, and achieving low cost of high-purity silica , efficient production and environmentally friendly process flow.
Patent Information
- Application Number
- CN202411192062.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, high-temperature hydrolysis methods have high requirements for equipment, scarce and expensive raw materials, and complex technical control, resulting in high-purity gas-phase silica products with high cost, low activity, great environmental impact, and difficulty in controlling particle performance.
The reaction of fluorosilicate and quartz sand is used to generate silicon tetrafluoride gas, and hydrolyze it through the silicon tetrafluoride hydrolysis tower to generate silica acid, and it is recycled. Combined with filtration, washing and calcining processes, the production of high-purity silica is achieved.
It reduces production costs, improves the purity and efficiency of products, reduces environmental pollution, simplifies equipment requirements, and realizes the recycling of resources.
Smart Images

Figure CN118929679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-purity fumed silicon dioxide production, in particular to a high-purity silicon dioxide gas phase synthesis process. Background Art
[0002] Fumed silica, also known as fumed silica or fumed white carbon black, is a fine, special amorphous silica product produced by hydrolysis of halosilanes at high temperatures. Fumed silica has excellent thickening and thixotropic properties due to its unique structural characteristics, such as small particle size, uniform particle size distribution, large specific surface area, and a large number of silanol groups on the surface.
[0003] In the prior art, fumed silica is mostly prepared by a gas phase method or a precipitation method. The precipitation method is to first use fuel oil or high-quality coal to react quartz sand with soda ash at high temperature to obtain industrial water glass, then prepare the industrial water glass with water into a dilute solution of a certain concentration, and then add a certain acid under certain conditions to precipitate silica, and then wash, filter, dry, and crush to obtain the product. The gas phase method is to mix a homogeneous gas composed of gasified silicon tetrachloride, hydrogen and oxygen and burn it in a hydrolysis furnace to perform a high-temperature hydrolysis reaction. The smoke-like white carbon black is gathered through an aggregator, and then sent to a deacidification furnace through a separator for deacidification treatment to obtain a fumed silica product.
[0004] However, the precipitation process consumes high energy and has high environmental requirements. The product activity is not high, the particles are difficult to control, the affinity is poor, the reinforcement performance is low, the hydrophilic groups on the surface of the particles are severely bonded, which weakens the binding force of the product and the quality of the product is not high. The gas phase method in the existing technology has high requirements for equipment, scarce and extremely expensive raw materials, complex technical control, and a large investment scale. In view of this, we have proposed a high-purity silica gas phase synthesis process. Summary of the invention
[0005] The object of the present invention is to provide a high-purity silicon dioxide gas phase synthesis process to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a high-purity silicon dioxide gas phase synthesis process, comprising the following steps:
[0007] A1. Preparation of fluorosilicic acid: a certain amount of 40% hydrofluoric acid and 90-99% silicon dioxide are placed in a quartz sand reaction tank for reaction to obtain fluorosilicic acid;
[0008] A2, preparing silicon tetrafluoride gas in a reactor: the fluorosilicic acid obtained in A1 is transported to a fluorosilicic acid storage tank, and then quantitatively transported from the fluorosilicic acid storage tank to a reactor, in which 60% volume of 98% concentrated sulfuric acid and quartz sand are pre-added, mixed and continuously heated to produce a mixed gas of silicon tetrafluoride, water vapor and hydrogen fluoride;
[0009] A3, silicon tetrafluoride hydrolysis: the silicon tetrafluoride and hydrogen fluoride mixed gas produced in A2 is introduced into the silicon tetrafluoride hydrolysis tower, and silicon tetrafluoride is hydrolyzed to generate silicic acid and hydrogen fluoride gas under the action of the circulating spray liquid in the silicon tetrafluoride hydrolysis tower, and the circulating spray liquid containing silicic acid is output to the circulation tank, and hydrogen fluoride and steam enter the hydrogen fluoride condensation absorption tower;
[0010] A4. Circulating spray liquid containing silicate is pumped into the filter press for filtration. The produced liquid is returned to the circulating tank for recycling. The produced silicate solid is transported to the silicate washing tank for washing.
[0011] A5, secondary washing and filter pressing treatment: the liquid washed in the silicate washing tank in A4 is pumped into the filter press again for solid-liquid separation, the obtained solid is silicate and is transported to the drying oven for drying, and the obtained residual water and fluorosilicic acid are transported to the silicofluoric acid evaporation concentrator;
[0012] A6. Calcination: The silicic acid dried in the drying oven in A5 is sent to a calcining furnace for calcination. After calcination, the product is cooled, crushed and sieved to obtain a high-purity silicon dioxide product.
[0013] Preferably, a diaphragm pump is used to transport the fluorosilicic acid solution from the fluorosilicic acid storage tank in A2 to the reactor, thereby controlling the amount of fluorosilicic acid solution added, making the reaction in the reactor more balanced, and the reaction temperature in the reactor is set at 100°C to 110°C, and the heat source of the reactor is one of steam, heat transfer oil, and electromagnetic heating. At the same time, the vacuum degree in the reactor is controlled at -0.05MPa, thereby promoting the decomposition of fluorosilicic acid and absorbing hydrogen fluoride to generate fluorosulfonic acid, and the fluorosulfonic acid further reacts with quartz sand to generate fluorosilicic acid, thereby improving the utilization efficiency of hydrogen fluoride. Because the sulfuric acid concentration is under negative pressure conditions at 100°C, the sulfuric acid concentration is always maintained at 80%, ensuring the acid concentration of the fluorosilicic acid reaction.
[0014] Preferably, a high-level tank is provided inside the silicon tetrafluoride hydrolysis tower, and the high-level tank is connected to a diaphragm pump and a circulation tank through a pipeline. The circulating spray liquid entering the circulation tank is transported to the high-level tank by the diaphragm pump, and then sprayed into the silicon tetrafluoride hydrolysis tower via the high-level tank, thereby stabilizing the spraying amount in the silicon tetrafluoride hydrolysis tower. At the same time, the diaphragm pump adopts a full-plastic diaphragm pump. Since the circulating spray liquid contains fluorosilicic acid, it severely corrodes most metals. The corroded metal ions contaminate the silica, resulting in a high content of silicon dioxide impurities that does not meet the standards. In order to ensure the stability of the operation of the device, a full-plastic diaphragm pump is used to have a longer service life.
[0015] Preferably, when washing the silicate solid produced in A3 in the silicate washing tank in A4, the washing liquid is pure water, and the volume ratio of the washing liquid to the silicate solid is 5:1-10:1, so that the fluorosilicic acid on the surface of the silicate solid can be effectively washed.
[0016] Preferably, the temperature of the calcining furnace during high-temperature calcination in A6 can be adjusted according to actual product requirements. When the calcining furnace temperature is controlled at 1300°C and the reaction time is 2 hours, a high-purity silicon dioxide product is obtained after subsequent crushing and screening. When the calcining furnace temperature is controlled at 800°C and the reaction time is 2 hours, a high-purity white carbon black product is obtained after crushing and screening.
[0017] Preferably, the process A3 further comprises a tail gas treatment method after the silicon tetrafluoride hydrolysis operation, and the tail gas treatment method comprises the following steps:
[0018] B1. Hydrogen fluoride absorption: The gas obtained after hydrolysis in A3 enters a hydrogen fluoride absorption tower for absorption. A circulating absorption liquid is used in the hydrogen fluoride absorption tower to continuously spray and absorb hydrogen fluoride, and the concentration of hydrogen fluoride is controlled at 20% to 30%. The circulating absorption liquid is output to a hydrofluoric acid circulation tank;
[0019] B2. Hydrogen fluoride condensation: A small amount of hydrogen fluoride gas discharged from B1 enters the hydrogen fluoride freezer through a pipeline for low-temperature condensation, and the condensate is discharged into the hydrofluoric acid circulation tank;
[0020] B3. Circulation absorption: The hydrofluoric acid circulation tank uses a diaphragm pump to pump the hydrogen fluoride solution obtained by mixing the circulating absorption liquid and the hydrofluoric acid condensate inside into the hydrogen fluoride absorption tower for secondary absorption;
[0021] B4. Preparation of fluorosilicic acid solution: The hydrogen fluoride solution in the hydrofluoric acid circulation tank is pumped into the quartz sand reaction tank through a delivery pump, and the fluorosilicic acid solution is obtained by mixing and reacting;
[0022] B5. Fluosilicic acid concentration and evaporation: The fluosilicic acid solution obtained in B4 and the washing water in the silicic acid washing tank in A4 are transported to the fluosilicic acid evaporation concentrator by a delivery pump to concentrate and evaporate the fluosilicic acid;
[0023] B6. Output pumping: The fluorosilicic acid obtained after concentration and evaporation in B5 is transported back to the fluorosilicic acid storage tank through pipelines and delivery pumps for recycling. Part of the condensate obtained is used as washing water in A4, and the other part of the condensate is used as supplementary water for the circulation tank in A3.
[0024] Preferably, the hydrogen fluoride refrigerator used in B2 is cooled by a refrigerator and a vacuum pump, and the condensation temperature in the hydrogen fluoride refrigerator is controlled at 0-5°C, which is much lower than the boiling point of hydrogen fluoride, 19.51°C, thereby ensuring the full recovery of hydrogen fluoride, reducing tail gas emissions, and improving the production safety of the process.
[0025] Preferably, the evaporation temperature of the fluorosilicic acid evaporation concentrator used in B5 is set at 50° C. to ensure that the concentration of fluorosilicic acid after evaporation and concentration is above 30%, thereby facilitating the continuous use of the production equipment and improving the subsequent reaction efficiency and reaction quality.
[0026] Preferably, the reactor used in A2 is provided with a stirring mechanism, and a shoveling assembly that can shovel the material at the bottom of the reactor is provided at the bottom of the stirring mechanism, and the shoveling assembly is in contact with the bottom inner wall of the reactor, and the stirring mechanism and the shoveling assembly are made of acid-proof and corrosion-resistant materials, so that the quartz sand, sulfuric acid, fluorosilicic acid and other materials in the reactor can fully react, thereby improving the reaction production efficiency of the equipment.
[0027] Preferably, the silicate drying box used in A5 has a waste heat recovery system, and the waste heat recovery system preheats the feed chamber of the silicate drying box, thereby improving the preheating of the silicate solid produced in A5 in subsequent operations, so that it can be dried faster in the silicate drying box, thereby improving the processing efficiency of drying and calcining the silicate solid.
[0028] Compared with the prior art, the present invention provides a high-purity silicon dioxide gas phase synthesis process, which has the following beneficial effects:
[0029] 1. The high-purity silica gas phase synthesis process has a wide range of quartz sand raw materials required for the production of high-purity silica, thereby greatly reducing the production cost of high-purity silica gas phase synthesis. At the same time, hydrofluoric acid is reacted with quartz sand to generate fluorosilicic acid, and fluorosilicic acid and sulfuric acid are heated to produce silicon tetrafluoride gas. Silicon tetrafluoride is hydrolyzed to produce silicic acid, and in the subsequent production process, hydrogen fluoride gas is frozen and absorbed to generate hydrofluoric acid. Hydrofluoric acid reacts with quartz to generate fluorosilicic acid and returns to the system to achieve the recycling of hydrofluoric acid. Silicon tetrafluoride is hydrolyzed to continuously produce high-purity silicic acid liquid, and finally high-purity silicic acid is extracted through solid-liquid separation and filter cake washing of the filter press. After drying and calcination, a high-purity silica product is obtained. The filter cake washing liquid is evaporated and condensed at low temperature to produce high-purity water for washing, realizing the recycling of water. The production process is simpler and more efficient, with lower production requirements for equipment, and improving the efficiency of high-purity silica gas phase synthesis.
[0030] 2. The high-purity silicon dioxide gas phase synthesis process is equipped with a hydrogen fluoride absorption tower and a hydrogen fluoride cooler and other equipment in the production process, so that the hydrogen fluoride waste gas generated during the hydrolysis of silicon tetrafluoride can be fully and completely absorbed and treated, so that the entire process does not generate waste gas and has little impact on the environment. At the same time, the produced hydrogen fluoride solution can also be recycled to reduce the waste of resources.
[0031] 3. The high-purity silica gas phase synthesis process uses a fluosilicic acid concentration evaporator to concentrate and evaporate the washing water of the fluosilicic acid and silicate washing tanks and the filtered water obtained after the secondary filter press, so as to make full use of the hydrogen fluoride that may have been lost in the production process. At the same time, the pure water produced by condensation can be reused and added to the production process, thereby improving the resource utilization rate of the gas phase synthesis process. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the process flow of the present invention;
[0033] Figure 2 This is a schematic diagram of the gas phase synthesis process of silicon dioxide according to the present invention;
[0034] Figure 3 It is a schematic diagram of the tail gas treatment process of the present invention. DETAILED DESCRIPTION
[0035] like Figure 1-Figure 3 As shown, the present invention provides a technical solution: a high-purity silicon dioxide gas phase synthesis process, comprising the following steps:
[0036] A1. Preparation of fluorosilicic acid: a certain amount of 40% hydrofluoric acid and 90-99% silicon dioxide are placed in a quartz sand reaction tank for reaction to obtain fluorosilicic acid;
[0037] A2, reactor mixing: the fluorosilicic acid obtained in A1 is transported to a fluorosilicic acid storage tank, and then quantitatively transported from the fluorosilicic acid storage tank to a reactor, 60% by volume of 98% concentrated sulfuric acid and quartz sand are pre-added into the reactor, mixed and continuously heated to generate a mixed gas of silicon tetrafluoride and hydrogen fluoride;
[0038] A3. Silicon tetrafluoride hydrolysis: The silicon tetrafluoride and hydrogen fluoride mixed gas produced in A2 is introduced into the silicon tetrafluoride hydrolysis tower. Under the action of the circulating spray liquid in the silicon tetrafluoride hydrolysis tower, silicon tetrafluoride is hydrolyzed to generate silicic acid and hydrogen fluoride gas, and the circulating spray liquid containing silicic acid is output to the circulation tank;
[0039] A4. Circulating spray liquid containing silicate is pumped into the filter press for filtration. The produced liquid is pumped into the circulating tank for recycling. The produced silicate solid is transported to the silicate washing tank for washing.
[0040] A5, secondary washing and filter pressing treatment: the liquid washed in the silicate washing tank in A4 is pumped into the filter press again for solid-liquid separation, the obtained solid is silicate and is transported to the drying oven for drying, and the obtained residual water and fluorosilicic acid are transported to the silicofluoric acid evaporation concentrator;
[0041] A6. Calcination: The silicic acid dried in the drying oven in A5 is sent to a calcining furnace for calcination. After calcination, the product is cooled, crushed and sieved to obtain a high-purity silicon dioxide product.
[0042] In one embodiment of the present invention, a diaphragm pump is used to transport the fluorosilicic acid solution from the fluorosilicic acid storage tank in A2 to the reactor, thereby controlling the amount of fluorosilicic acid solution added, making the reaction in the reactor more balanced, and the reaction temperature in the reactor is set at 100°C to 110°C, and the heat source of the reactor is one of steam, heat transfer oil, and electromagnetic heating. At the same time, the vacuum degree in the reactor is controlled at -0.05MPa, thereby promoting the decomposition of fluorosilicic acid and absorbing hydrogen fluoride to generate fluorosulfonic acid, and the fluorosulfonic acid further reacts with quartz sand to generate fluorosilicic acid, thereby improving the utilization efficiency of hydrogen fluoride. The sulfuric acid concentration is always maintained at 80% because of the negative pressure condition at 100°C. , ensuring that the acid concentration of the fluorosilicic acid reaction is high. At the same time, a high-level tank is provided inside the silicon tetrafluoride hydrolysis tower, and the high-level tank is connected to the diaphragm pump and the circulation tank through a pipeline. The circulating spray liquid entering the circulation tank is transported to the high-level tank by the diaphragm pump, and then sprayed into the silicon tetrafluoride hydrolysis tower through the high-level tank, thereby stabilizing the spraying amount in the silicon tetrafluoride hydrolysis tower. At the same time, the diaphragm pump adopts a full plastic diaphragm pump. Since the circulating spray liquid contains fluorosilicic acid, it seriously corrodes most metals. The corroded metal ions contaminate the silica, resulting in a high content of silicon dioxide impurities that does not meet the standards. In order to ensure the stability of the device operation, a full plastic diaphragm pump is used with a longer service life.
[0043] In addition, when washing the silicate solid produced in A3 in the silicate washing tank in A4, the washing liquid is washed with pure water, and the volume ratio of the washing liquid to the silicate solid is 5:1-10:1, so that the fluorosilicic acid on the surface of the silicate solid can be effectively washed. Furthermore, the temperature of the calcining furnace during high-temperature calcination in A6 can be adjusted according to actual product requirements. When the calcining furnace temperature is controlled at 1300°C and the reaction time is 2h, a high-purity silicon dioxide product is obtained after subsequent crushing and screening. When the calcining furnace temperature is controlled at 800°C and the reaction time is 2h, a high-purity white carbon black product is obtained after crushing and screening.
[0044] In an embodiment of the present invention, after the silicon tetrafluoride hydrolysis operation is performed in A3, a tail gas treatment method is also included, and the tail gas treatment method includes the following steps:
[0045] B1. Hydrogen fluoride absorption: The gas obtained after hydrolysis in A3 enters the hydrogen fluoride absorption tower for absorption. The hydrogen fluoride absorption tower uses a circulating absorption liquid to continuously spray and absorb hydrogen fluoride, and the concentration of hydrogen fluoride is controlled at 20% to 30%. The circulating absorption liquid is output to the hydrofluoric acid circulation tank;
[0046] B2. Hydrogen fluoride condensation: A small amount of hydrogen fluoride gas discharged from B1 enters the hydrogen fluoride freezer through a pipeline for low-temperature condensation, and the condensate is discharged into the hydrofluoric acid circulation tank;
[0047] B3. Circulation absorption: The hydrofluoric acid circulation tank uses a diaphragm pump to pump the hydrogen fluoride solution obtained by mixing the circulating absorption liquid and the hydrofluoric acid condensate inside into the hydrogen fluoride absorption tower for secondary absorption;
[0048] B4. Preparation of fluorosilicic acid solution: The hydrogen fluoride solution in the hydrofluoric acid circulation tank is pumped into the quartz sand reaction tank through a delivery pump, and the fluorosilicic acid solution is obtained by mixing and reacting;
[0049] B5. Fluosilicic acid concentration and evaporation: The fluosilicic acid solution obtained in B4 and the washing water in the silicic acid washing tank in A4 are transported to the fluosilicic acid evaporation concentrator by a delivery pump to concentrate and evaporate the fluosilicic acid;
[0050] B6. Output pumping: The fluorosilicic acid obtained after concentration and evaporation in B5 is transported back to the fluorosilicic acid storage tank through pipelines and delivery pumps for recycling. Part of the condensate obtained is used as washing water in A4, and the other part of the condensate is used as supplementary water for the circulation tank in A3.
[0051] In the present invention, the hydrogen fluoride refrigerator used in B2 is cooled by a refrigerator and a vacuum pump, and the condensation temperature in the hydrogen fluoride refrigerator is controlled at 0-5°C, which is much lower than the boiling point of hydrogen fluoride, 19.51°C, thereby ensuring the full recovery of hydrogen fluoride, reducing the emission of tail gas, and improving the production safety of the process. At the same time, the evaporation temperature of the fluorosilicic acid evaporation concentrator used in B5 is set at 50°C, ensuring that the concentration of fluorosilicic acid after evaporation and concentration is above 30%, thereby facilitating the continuous use of the production equipment and improving the subsequent reaction efficiency and reaction quality.
[0052] It is worth noting that the reactor used in A2 is provided with a stirring mechanism, and a shoveling assembly is provided at the bottom of the stirring mechanism for shoveling the material at the bottom of the reactor. The shoveling assembly is in contact with the bottom inner wall of the reactor, and the stirring mechanism and the shoveling assembly are made of acid-proof and anti-corrosion materials, so that the quartz sand, sulfuric acid, fluorosilicic acid and other materials in the reactor can fully react, thereby improving the reaction production efficiency of the equipment. At the same time, the silicate drying box used in A5 has a waste heat recovery system, and the waste heat recovery system preheats the feed chamber of the silicate drying box, thereby improving the preheating of the silicate solid produced in A5 in subsequent operations, so that it can be dried faster in the silicate drying box, thereby improving the processing efficiency of drying and calcining silicate solids.
[0053] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.
Claims
1. A high-purity silicon dioxide vapor phase synthesis process, characterized in that: The synthesis process comprises the following steps: A1. Preparation of fluorosilicic acid: a certain amount of 40% hydrofluoric acid and 90-99% silicon dioxide are placed in a quartz sand reaction tank for reaction to obtain fluorosilicic acid; A2, preparing silicon tetrafluoride gas in a reactor: the fluorosilicic acid obtained in A1 is transported to a fluorosilicic acid storage tank, and then quantitatively transported from the fluorosilicic acid storage tank to a reactor, in which 60% volume of 98% concentrated sulfuric acid and quartz sand are pre-added, mixed and continuously heated to produce a mixed gas of silicon tetrafluoride, water vapor and hydrogen fluoride; A3, silicon tetrafluoride hydrolysis: the silicon tetrafluoride and hydrogen fluoride mixed gas produced in A2 is introduced into the silicon tetrafluoride hydrolysis tower, and silicon tetrafluoride is hydrolyzed to generate silicic acid and hydrogen fluoride gas under the action of the circulating spray liquid in the silicon tetrafluoride hydrolysis tower, and the circulating spray liquid containing silicic acid is output to the circulation tank, and hydrogen fluoride and steam enter the hydrogen fluoride condensation absorption tower; A4. Circulating spray liquid containing silicate is pumped into the filter press for filtration. The produced liquid is returned to the circulating tank for recycling. The produced silicate solid is transported to the silicate washing tank for washing. A5, secondary washing and filter pressing treatment: the liquid washed in the silicate washing tank in A4 is pumped into the filter press again for solid-liquid separation, the obtained solid is silicate and is transported to the drying oven for drying, and the obtained residual water and fluorosilicic acid are transported to the silicofluoric acid evaporation concentrator; A6. Calcination: The silicic acid dried in the drying oven in A5 is sent to a calcining furnace for calcination. After calcination, the product is cooled, crushed and sieved to obtain a high-purity silicon dioxide product.
2. A high-purity silicon dioxide vapor phase synthesis process according to claim 1, characterized in that: A diaphragm pump is used to transport the fluorosilicic acid solution from the fluorosilicic acid storage tank in A2 to the reactor, and the reaction temperature in the reactor is set at 100°C to 110°C, and the heat source of the reactor is one of steam, heat transfer oil, and electromagnetic heating. At the same time, the vacuum degree in the reactor is controlled at -0.05MPa.
3. A high-purity silicon dioxide vapor phase synthesis process according to claim 1, characterized in that: The silicon tetrafluoride hydrolysis tower is provided with a high-level tank inside, and the high-level tank is connected to the diaphragm pump and the circulation tank through a pipeline. The circulating spray liquid entering the circulation tank is transported to the high-level tank by the diaphragm pump, and then sprayed into the silicon tetrafluoride hydrolysis tower through the high-level tank. At the same time, the diaphragm pump adopts a fully plastic diaphragm pump.
4. A high-purity silicon dioxide vapor phase synthesis process according to claim 1, characterized in that: When washing the silicate solid produced in A3 in the silicate washing tank in A4, the washing liquid is pure water, and the volume ratio of the washing liquid to the silicate solid is 5:1-10:
1.
5. A high-purity silicon dioxide vapor phase synthesis process according to claim 1, characterized in that: The temperature of the calcining furnace during high-temperature calcination in A6 can be adjusted according to actual product requirements. When the temperature of the calcining furnace is controlled at 1300°C and the reaction time is 2 hours, a high-purity silicon dioxide product is obtained after subsequent crushing and screening. When the temperature of the calcining furnace is controlled at 800°C and the reaction time is 2 hours, a high-purity white carbon black product is obtained after crushing and screening.
6. A high-purity silicon dioxide vapor phase synthesis process according to claim 1, characterized in that: After the silicon tetrafluoride hydrolysis operation is performed in A3, a tail gas treatment method is also included, and the tail gas treatment method includes the following steps: B1. Hydrogen fluoride absorption: The gas obtained after hydrolysis in A3 enters a hydrogen fluoride absorption tower for absorption. A circulating absorption liquid is used in the hydrogen fluoride absorption tower to continuously spray and absorb hydrogen fluoride, and the concentration of hydrogen fluoride is controlled at 20% to 30%. The circulating absorption liquid is output to a hydrofluoric acid circulation tank; B2. Hydrogen fluoride condensation: A small amount of hydrogen fluoride gas discharged from B1 enters the hydrogen fluoride freezer through a pipeline for low-temperature condensation, and the condensate is discharged into the hydrofluoric acid circulation tank; B3. Circulation absorption: The hydrofluoric acid circulation tank uses a diaphragm pump to pump the hydrogen fluoride solution obtained by mixing the circulating absorption liquid and the hydrofluoric acid condensate inside into the hydrogen fluoride absorption tower for secondary absorption; B4. Preparation of fluorosilicic acid solution: The hydrogen fluoride solution in the hydrofluoric acid circulation tank is pumped into the quartz sand reaction tank through a delivery pump, and the fluorosilicic acid solution is obtained by mixing and reacting; B5. Fluosilicic acid concentration and evaporation: The fluosilicic acid solution obtained in B4 and the washing water in the silicic acid washing tank in A4 are transported to the fluosilicic acid evaporation concentrator by a delivery pump to concentrate and evaporate the fluosilicic acid; B6. Output pumping: The fluorosilicic acid obtained after concentration and evaporation in B5 is transported back to the fluorosilicic acid storage tank through pipelines and delivery pumps for recycling. Part of the condensate obtained is used as washing water in A4, and the other part of the condensate is used as supplementary water for the circulation tank in A3.
7. A high-purity silicon dioxide vapor phase synthesis process according to claim 6, characterized in that: The hydrogen fluoride refrigerator used in B2 is cooled by a refrigerator and a vacuum pump. The condensation temperature in the hydrogen fluoride refrigerator is controlled at 0-5°C, which is much lower than the boiling point of hydrogen fluoride, 19.51°C.
8. A high-purity silicon dioxide vapor phase synthesis process according to claim 6, characterized in that: The evaporation temperature of the fluorosilicic acid evaporation concentrator used in B5 is set at 50° C. to ensure that the concentration of fluorosilicic acid after evaporation and concentration is above 30%.
9. A high-purity silicon dioxide vapor phase synthesis process according to claim 1, characterized in that: The reactor used in A2 is provided with a stirring mechanism, and a shoveling assembly for shoveling the material at the bottom of the reactor is provided at the bottom of the stirring mechanism. The shoveling assembly is fitted with the bottom inner wall of the reactor, and the stirring mechanism and the shoveling assembly are both made of acid-proof and corrosion-resistant materials.
10. A high-purity silicon dioxide vapor phase synthesis process according to claim 1, characterized in that: The silicate drying box used in A5 has a waste heat recovery system, and the waste heat recovery system preheats the feed chamber of the silicate drying box, thereby improving the preheating of the silicate solid produced in A5 in subsequent operations, so that it can be dried faster in the silicate drying box, thereby improving the processing efficiency of drying and calcining the silicate solid.
Citation Information
Cited By
Preparation method of high-purity silicon dioxide
CN120136110A
A method for preparing high-purity silica
CN120136110B
Production process of high-purity nano silicon dioxide
CN122102145A