A packaging structure of a device
By using an airtight layer to fill the storage tank of the epoxy plastic seal in the packaging structure of the IGBT device, blocking the gap between the pin and the epoxy plastic seal, solving the failure problem of IGBT device due to the entry of water vapor. Achieved waterproof effect.
Patent Information
- Application Number
- CN202210822191.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-07-13
AI Technical Summary
The plastic sealing material in IGBT devices has high hygroscopicity, causing water vapor to enter the inside of the device, resulting in failure of the chip and internal circuits.
A packaging structure adopts copper substrate, airtight layer, epoxy plastic sealing material and pins, where the airtight layer is filled in the accommodating groove of the epoxy plastic sealing material, completely covers the internal pins, and blocks the pins and epoxy plastic sealing. The gap between the materials prevents water vapor from entering.
It effectively prevents water vapor from entering the device and avoids device failure problems caused by water vapor.
Smart Images

Figure CN115377019B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of integrated circuits, and in particular to a packaging structure of a device. Background Art
[0002] IGBT (Insulated Gate Bipolar Transistor) is a composite fully controlled voltage-driven electronic device with the characteristics of high switching frequency, large input impedance, good thermal stability, simple driving circuit, low saturation voltage and large current. It is widely used as a power device in the fields of industrial control and power electronics systems.
[0003] Among them, the plastic encapsulation material in the IGBT device is generally a polymer composite material composed of epoxy resin, curing agent, filler and other components. Its inherent organic macromolecular structure makes it highly hygroscopic. Since there is a gap between the plastic encapsulation material and the external lead part of the IGBT device, water vapor will enter the interior of the IGBT device through this gap. The water vapor entering the IGBT device will adhere to the surface of the chip under the action of the plastic encapsulation material, causing the chip and internal circuit to fail. Summary of the invention
[0004] In view of the above problems, embodiments of the present invention are proposed to provide a device packaging structure that overcomes the above problems or at least partially solves the above problems.
[0005] In order to solve the above problems, an embodiment of the present invention discloses a packaging structure of a device, including: a copper substrate, an airtight layer, an epoxy molding compound and pins;
[0006] The pins and the epoxy molding compound are both connected to the copper substrate;
[0007] The epoxy molding compound is provided with a receiving groove, wherein the notch of the receiving groove faces the copper substrate;
[0008] The epoxy molding compound is provided with an external lead-out opening for the pins to extend into the interior of the receiving groove; wherein, part of the pins extend into the interior of the receiving groove through the external lead-out opening to form internal pins;
[0009] The accommodating groove is filled with the airtight layer, wherein the airtight layer completely fits and covers the internal pins, and the airtight layer is used to fill the gap between the epoxy molding compound and the pins.
[0010] Preferably, the airtight layer and the copper substrate are sealed by compression sealing;
[0011] Or the airtight layer and the internal pin are sealed by compression sealing.
[0012] Preferably, the expansion coefficients of the copper substrate and the pins are both greater than the expansion coefficient of the airtight layer.
[0013] Preferably, the packaging structure further includes bonding wires and wafers;
[0014] One end of the bonding wire is connected to the internal pin, and the other end is connected to the wafer; wherein the bonding wire and the wafer are both encapsulated by the epoxy molding compound.
[0015] Preferably, the portion where the bonding wire is connected to the internal pin is arranged in the airtight layer.
[0016] Preferably, a surface of one end of the bonding wire connected to the wafer is provided with texture.
[0017] Preferably, an adhesive layer is provided between the epoxy molding compound and the copper substrate, and the epoxy molding compound is connected to the copper substrate via the adhesive layer;
[0018] Wherein, the bonding layer contains cupric hydroxide and cuprous oxide.
[0019] Preferably, the surface of the copper substrate contains cupric hydroxide and cuprous oxide, but does not contain cupric oxide.
[0020] Preferably, it also includes a solder layer;
[0021] The wafer is connected to the copper substrate through the solder layer.
[0022] Preferably, the airtight layer is made of glass material.
[0023] The embodiment of the present invention has the following advantages: since the airtight layer is arranged in the receiving groove of the epoxy molding compound, and the airtight layer in the receiving groove can completely fit and cover the internal pins in the receiving groove, and the airtight layer can block the gap between the pins and the epoxy molding compound. Since the gap between the pins and the epoxy molding compound has been blocked, it is difficult for water vapor to enter the interior of the device through the gap, which effectively prevents the failure of various components inside the device due to the influence of water vapor. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a structural schematic diagram of a packaging structure embodiment of a device of the present invention.
[0025] The reference numerals in the drawings of the specification are as follows:
[0026] Copper substrate 1; airtight layer 2; solder layer 3; pin 4; epoxy molding compound 5; bonding wire 6; wafer 7; adhesive layer 8. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] Reference Figure 1 , shows a schematic structural diagram of a device packaging structure embodiment of the present invention, which may specifically include: a copper substrate 1, an airtight layer 2, an epoxy molding compound 5 and a pin 4;
[0029] The pins 4 and the epoxy molding compound 5 are both connected to the copper substrate 1;
[0030] The epoxy molding compound 5 is provided with a receiving groove, wherein the notch of the receiving groove faces the copper substrate 1;
[0031] The epoxy molding compound 5 is provided with an external lead-out opening for the pins 4 to extend into the interior of the receiving groove; wherein, part of the pins 4 extend into the interior of the receiving groove through the external lead-out opening to form internal pins;
[0032] The accommodating groove is filled with the airtight layer 2, wherein the airtight layer 2 completely covers the internal pin, and the airtight layer 2 is used to fill the gap between the epoxy molding compound 5 and the pin 4. It should be noted that the airtight layer 2 fills the gap between the epoxy molding compound 5 and the pin 4, which can also be understood as the airtight layer 2 blocking the gap caused by the pin 4 extending into the epoxy molding compound 5.
[0033] In the embodiment of the present application, since the airtight layer 2 is arranged in the receiving groove of the epoxy molding compound 5, and the airtight layer 2 in the receiving groove can completely fit and cover the internal pins in the receiving groove, and the airtight layer 2 can block the gap between the pins 4 and the epoxy molding compound 5. Since the gap between the pins 4 and the epoxy molding compound 5 has been blocked, it is difficult for water vapor to enter the interior of the device through this gap, which effectively prevents the failure of various components inside the device due to the influence of water vapor.
[0034] Next, a packaging structure of a device in this exemplary embodiment will be further described.
[0035] As an example, the airtight layer 2 and the copper substrate 1 are sealed by compression sealing;
[0036] Alternatively, the airtight layer 2 and the internal pin are sealed by compression sealing.
[0037] The expansion coefficients of the copper substrate 1 and the pin 4 are greater than the expansion coefficient of the airtight layer 2. More specifically, since the expansion coefficients of the copper substrate 1 and the pin 4 are greater than the expansion coefficient of the airtight layer 2, during the cooling stage of the compression seal, the contraction of the copper substrate 1 and the pin 4 is greater than the contraction of the airtight layer 2; therefore, when the compression seal is performed, the copper substrate 1 and the pin 4 will generate a compressive stress on the airtight layer 2, and the effect of the sealed connection is achieved through this compressive stress. It should be noted that when one end of the internal pin is completely in contact with the groove wall of the accommodating groove, the compression seal at this time is a sealed connection between the airtight layer 2 and the internal pin.
[0038] As an example, the packaging structure further includes a bonding wire 6 and a wafer 7;
[0039] One end of the bonding wire 6 is connected to the internal pin, and the other end is connected to the wafer 7 ; wherein the bonding wire 6 and the wafer 7 are both encapsulated by the epoxy molding compound 5 .
[0040] The portion where the bonding wire 6 is connected to the internal pin is disposed in the airtight layer 2. More specifically, in order to fix the bonding wire 6, the portion where the bonding wire 6 is connected to the internal pin is also disposed in the airtight layer 2. It should be noted that, in other embodiments, the expansion coefficient of the bonding wire 6 is greater than the expansion coefficient of the airtight layer 2. Therefore, when compression sealing is performed, the bonding wire 6 can also be clamped and fixed by the airtight layer 2 by the difference in expansion coefficient between the bonding wire 6 and the airtight layer 2.
[0041] As an example, the surface of one end of the bonding wire 6 connected to the wafer 7 is a non-smooth surface;
[0042] Specifically, the non-smooth surface is a surface with textures. More specifically, the surface of one end of the bonding wire 6 connected to the wafer 7 is set as a non-smooth surface, which can increase the bonding force between the bonding wire 6 and the epoxy molding compound 5 at the bonding point, thereby reducing the cracking at this position as much as possible; at the same time, the thickness of the epoxy molding compound 5 in the device is increased when the process cost allows, thereby increasing the threshold limit of the epoxy molding compound 5 to withstand water vapor pressure.
[0043] As an example, an adhesive layer 8 is provided between the epoxy molding compound 5 and the copper substrate 1, and the epoxy molding compound 5 is connected to the copper substrate 1 through the adhesive layer 8;
[0044] The adhesive layer 8 contains cupric hydroxide and cuprous oxide. More specifically, in order to further prevent the interface delamination of the components inside the device due to water ingress into the device, an adhesive layer 8 is provided between the epoxy molding compound 5 and the copper substrate 1 to increase the adhesion between the two components.
[0045] As an example, the surface of the copper substrate 1 contains cupric hydroxide and cuprous oxide, but does not contain cupric oxide.
[0046] More specifically, in the preparation of the copper substrate 1, the copper alloy copper substrate 1 is placed in an oven for baking at a baking temperature of 175°C; after baking, it is placed in a drying oven for storage. After baking for 3 to 6 minutes, the surface composition of the copper alloy copper substrate 1 is mainly composed of Cu(OH)2 and Cu2O. It should be noted that the baking time cannot exceed 15 minutes, otherwise copper oxide will appear on the surface. Under the premise of using the adhesive layer 8, the presence of copper oxide will significantly reduce the bonding force between the epoxy molding compound 5 and the copper substrate 1.
[0047] It should be noted that, in other embodiments, the copper substrate 1 is provided with a connection protrusion at the place where it is connected to the pin 4, and the height of the connection protrusion is the same as the thickness of the adhesive layer 8. At this time, the pin 4 will not touch the adhesive layer 8.
[0048] As an example, a solder layer 3 is also included;
[0049] The wafer 7 is connected to the copper substrate 1 through the solder layer 3. More specifically, the wafer 7 is connected to the side of the solder layer 3 away from the copper substrate 1. It should be noted that in other embodiments, a boss is provided in the middle of the copper substrate 1, and the height of the boss is the same as the thickness of the adhesive layer 8. At this time, the solder layer 3 will not touch the adhesive layer 8, and then the wafer 7 will not touch the adhesive layer 8.
[0050] As an example, the airtight layer 2 is made of glass material. More specifically, the glass material has good chemical stability, oxidation resistance, electrical insulation and compactness. When the glass airtight layer 2 and the copper substrate 1 are sealed and connected by compression sealing, no other compounds are required.
[0051] It should be noted that, for the sake of simplicity, the method embodiments are described as a series of action combinations, but those skilled in the art should be aware that the embodiments of the present invention are not limited by the order of the actions described, because according to the embodiments of the present invention, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of the present invention.
[0052] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0053] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.
[0054] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.
[0055] The packaging structure of a device provided by the present invention is introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the present invention and its core ideas. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A packaging structure of a device, It is characterized in that include: Copper substrate, airtight layer, epoxy molding compound and pins; The pins and the epoxy molding compound are both connected to the copper substrate; The epoxy molding compound is provided with a receiving groove, wherein the notch of the receiving groove faces the copper substrate; The epoxy molding compound is provided with an external lead-out opening for the pins to extend into the interior of the receiving groove; wherein, part of the pins extend into the interior of the receiving groove through the external lead-out opening to form internal pins; The accommodating groove is filled with the airtight layer, wherein the airtight layer completely covers the internal pins and is used to fill the gap between the epoxy molding compound and the pins; the airtight layer and the copper substrate or the internal pins are sealed by compression sealing; the expansion coefficients of the copper substrate and the pins are both greater than the expansion coefficient of the airtight layer.
2. The packaging structure according to claim 1, It is characterized in that The packaging structure also includes bonding wires and wafers; One end of the bonding wire is connected to the internal pin, and the other end is connected to the wafer; wherein the bonding wire and the wafer are both encapsulated by the epoxy molding compound.
3. The packaging structure according to claim 2, It is characterized in that The portion where the bonding wire is connected to the internal pin is disposed within the airtight layer.
4. The packaging structure according to claim 2, It is characterized in that The surface of one end of the bonding wire connected to the wafer is provided with textures.
5. The packaging structure according to claim 1, It is characterized in that An adhesive layer is provided between the epoxy molding compound and the copper substrate, and the epoxy molding compound is connected to the copper substrate through the adhesive layer; Wherein, the bonding layer contains cupric hydroxide and cuprous oxide.
6. The packaging structure according to claim 5, It is characterized in that The surface of the copper substrate contains cupric hydroxide and cuprous oxide, but does not contain cupric oxide.
7. The packaging structure according to claim 2, It is characterized in that Also including a solder layer; The wafer is connected to the copper substrate through the solder layer.
8. The packaging structure according to claim 1, It is characterized in that The airtight layer is made of glass material.