Application of heterojunction CdIn2S4 / Bi2WO6 piezoelectric-photocomposite catalyst in piezoelectric photodegradation of organic matter
By introducing CdIn2S4 nanomaterials on Bi2WO6 to form CIS/BWO composite materials, the problems of low degradation efficiency and insufficient stability of piezoelectric catalysts in the existing technology are solved, and efficient organic pollutant degradation and stability improvement are achieved.
Patent Information
- Application Number
- CN202211089067.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-09-07
AI Technical Summary
Existing piezoelectric catalysts have low efficiency and insufficient stability in degrading organic pollutants. In particular, the high recombination rate of photogenerated electrons and holes in pure Bi2WO6 hinders catalytic activity and limits its large-scale application.
A CIS/BWO composite material with type II heterojunction was prepared using a hydrothermal method. CdIn2S4 nanomaterials were introduced on Bi2WO6 to form a flower ball structure integrated with nanosheets, which improved the electron transfer rate and catalytic activity.
Significantly improves the degradation efficiency of organic pollutants under the synergistic effect of piezoelectric-light. The 10% CIS/BWO composite catalyst can degrade most of Rhodamine B within 15 minutes. The degradation capacity is higher than that of pure BWO, and the stability is excellent. Basically Complete degradation achieved.
Smart Images

Figure HDA0003836421740000011 
Figure HDA0003836421740000012 
Figure HDA0003836421740000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of piezoelectric photocatalysts and applications, and specifically relates to a type II heterojunction CdIn2S4 / Bi2WO6 (CIS / BWO) composite catalyst for piezoelectric photodegradation of rhodamine B and a preparation method thereof. Background Art
[0002] In recent years, the problems of ecological environmental pollution and energy resource shortage have become increasingly serious. The pollution caused by organic dyes in industrial wastewater can no longer be underestimated. Therefore, the application of piezoelectric photocatalysis to solve the problem of organic pollutants has received widespread attention. Piezoelectric catalysis refers to the formation of an electric field on the surface of catalyst particles under the induction of mechanical vibration energy of piezoelectric materials, generating active substances with redox ability, and then subjecting the dyes to redox reactions to achieve the purpose of degrading organic pollutants. On the one hand, many factors will affect the efficiency of piezoelectric catalysis, such as catalyst morphology, internal carrier separation efficiency, and active substance types. On the other hand, combining piezoelectric catalysis with photocatalysis can greatly improve the degradation performance of piezoelectric catalysis. However, the construction of efficient piezoelectric photocatalysts is still a major problem so far.
[0003] Recently, Bi2WO6, a layered oxide, has been studied as a photocatalyst with good photocatalytic performance and a band gap of about 2.7 eV under visible light irradiation. It is non-toxic, highly photostable, thermally stable, and environmentally friendly. The photogenerated electrons and holes of pure BWO have a high recombination rate, which hinders the catalytic activity and limits its large-scale application in catalytic performance. The catalytic performance can be effectively improved by constructing a type II heterojunction composite with abundant electron capture as the active site for redox reactions. Among semiconductor photocatalysts, metal sulfides have attracted attention due to their suitable band gap and good coefficients. First, ternary sulfides with strong visible light absorption and narrow band gap are becoming the focus of research. CdIn2S4 nanomaterials are used in many aspects, such as light-emitting diodes, photocatalysts, solar cells, and optoelectronic applications. CdIn2S4 is a family member of AB2C4 ternary compounds with a direct band gap (1.95-2.4 eV) and exhibits good photocatalytic activity under visible light.
[0004] Therefore, the present invention adopts a hydrothermal method to prepare a CIS / BWO composite material with excellent type II heterojunction. The construction of type II heterojunction can more efficiently promote the electron transfer rate between BWO and CIS. The degradation efficiency of CIS / BWO composite materials on organic pollutants in photocatalysis, piezoelectric catalysis and piezoelectric-photocatalysis was further explored. The results show that the CIS / BWO composite material exhibits significant piezoelectric photocatalytic efficiency and strong stability in degrading organic pollutants, confirming that the construction of excellent type II heterojunction composite materials has good application prospects in treating pollutants. Summary of the invention
[0005] The object of the present invention is to provide a CIS / BWO composite catalyst and a preparation method thereof, and to apply the composite catalyst to piezoelectric photodegradation of rhodamine B, which has high catalytic activity and good stability.
[0006] Technical solution of the present invention: The preparation method of the CIS / BWO composite catalyst provided by the present invention is:
[0007] (1) Preparation of Bi2WO6: Bismuth source and tungsten source are added to deionized water, stirred and dissolved at room temperature, and the mixture is transferred to a reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction in an oven; after cooling to room temperature, the mixture is filtered, washed, dried, and ground to obtain a white powder, which is the Bi2WO6 catalyst (BWO);
[0008] Bi(NO3)3·5H2O was used as bismuth source; Na2WO4·2H2O was used as tungsten source; the mass ratio of Bi(NO3)3·5H2O and Na2WO4·2H2O was 2.9:1, the hydrothermal reaction temperature was 190°C, and the reaction time was 2h.
[0009] (2) Preparation of CdIn2S4: Thiourea, cadmium chloride and indium (III) chloride tetrahydrate were added to deionized water and dissolved completely by ultrasonication for 0.5 h. The resulting transparent solution was transferred to a polytetrafluoroethylene-lined reactor and subjected to a hydrothermal reaction in an oven. After cooling to room temperature, the solution was filtered, washed, dried and ground to obtain a yellow powder, which was the CdIn2S4 catalyst.
[0010] The molar ratio of thiourea, cadmium chloride and indium (III) chloride tetrahydrate is 4:1:2; the hydrothermal reaction temperature is 150°C-220°C, preferably 180°C, and the reaction time is 48h.
[0011] (3) Preparation of CIS / BWO composite catalyst: CdIn2S4 catalyst and BWO catalyst were dissolved in anhydrous ethanol, stirred and mixed overnight (10-12 hours) at room temperature until the anhydrous ethanol evaporated, filtered, washed, dried overnight (10-12 hours) in a vacuum drying oven at 60°C, and ground into powder to finally obtain brown powder, which is the CIS / BWO composite catalyst. The mass of CdIn2S4 added is 5%-15% of the mass of Bi2WO6.
[0012] The CIS / BWO composite catalyst prepared by the method has a flower ball-like structure with integrated nanosheets.
[0013] The advantages of using the present invention are:
[0014] (1) The catalyst provided by the present invention is a CIS / BWO composite catalyst, which has the characteristics of simple synthesis conditions, easy operation, rapid and efficient, energy-saving and environmentally friendly, good stability, etc. The introduction of CdIn2S4 catalyst does not change the crystal structure of BWO, and no other diffraction peaks appear, indicating that the CIS / BWO composite material has excellent crystallinity and purity. The addition of CIS changes the piezoelectricity of the composite, and forms a type II heterojunction with BWO, which significantly improves the degradation ability under piezoelectric-optical action.
[0015] (2) The 10% CIS / BWO composite catalyst can degrade most of the organic matter within only 15 minutes under pure photocatalysis, pure piezoelectric catalysis and piezoelectric-photosynergistic action. It has a strong degradation ability and the efficiency of degrading RhB is higher than that of pure BWO, indicating that CdIn2S4 loaded on BWO can improve the degradation efficiency, indicating that the catalyst has a significant effect on degrading RhB under the piezoelectric-photosynergistic action. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 are the XRD patterns of the synthesized CIS / BWO catalysts with different ratios and BWO.
[0017] Figure 2 is a scanning electron microscope image of the BWO catalyst synthesized in Example 1.
[0018] Figure 3 This is a scanning electron microscope image of the 10% CIS / BWO catalyst synthesized in Example 7.
[0019] Figure 4 It is the performance diagram of degradation of Rhodamine B by CIS / BWO catalysts and BWO with different ratios under sunlight irradiation.
[0020] Figure 5 It is the performance diagram of the degradation of Rhodamine B by different ratios of CIS / BWO catalysts and BWO under ultrasonic vibration.
[0021] Figure 6 It is a performance diagram of the degradation of Rhodamine B by CIS / BWO catalysts and BWO in different ratios under sunlight irradiation and ultrasonic vibration at the same time.
[0022] Figure 7 It is the hysteresis loop diagram of 10%CIS / BWO catalyst and BWO. DETAILED DESCRIPTION
[0023] The present invention is described in detail below with reference to specific embodiments.
[0024] The degradation efficiency is calculated according to the following formula:
[0025] R=(C-C0) / C0*100%
[0026] R: Degradation efficiency
[0027] C0: initial concentration
[0028] C: Concentration after degradation reaction
[0029] Example 1
[0030] Weigh 1.94g Bi(NO3)3·5H2O and dissolve it in 50ml deionized water, stir and dissolve it, then add 0.66g Na2WO4·2H2O to the mixture and stir vigorously at room temperature for 1h. Transfer the mixture to a 100ml polytetrafluoroethylene-lined reactor, heat it in an oven at 190℃ for 2h, filter it after cooling to room temperature, wash it, dry it, grind it, and finally obtain a white powder, which is BWO powder.
[0031] Weigh 10 mg of BWO powder catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 min in the dark to reach adsorption-desorption equilibrium, degrade under sunlight for 15 min, take samples every 5 min, measure the absorbance, and calculate the degradation efficiency. The degradation efficiency is 31.8% after analysis and calculation.
[0032] Weigh 10 mg of BWO powder catalyst and 30 ml of 10 mol / L rhodamine B, stir for 30 min in dark conditions to reach adsorption-desorption equilibrium, degrade for 15 min under ultrasonic vibration (240 W, 40 kHz), take samples every 5 min, measure the absorbance, calculate the degradation efficiency, and the degradation efficiency is 19.8% after analysis and calculation.
[0033] Example 2
[0034] Preparation of CdIn2S4: 0.3045g thiourea, 0.2283g cadmium chloride and 0.5864g indium (III) chloride tetrahydrate were added to 30mL deionized water, and the mixture was completely dissolved by ultrasonication for 0.5h. The resulting transparent solution was transferred to a reactor lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 180°C in an oven for 48h. After cooling to room temperature, the mixture was filtered, washed, dried and ground to obtain a yellow powder, which was the CdIn2S4 catalyst.
[0035] The photocatalyst conditions are the same as those in Example 1: 10 mg of CdIn2S4 powder catalyst and 30 ml of 10 mol / L Rhodamine B were weighed, stirred for 30 min in the dark to reach adsorption-desorption equilibrium, and degraded under sunlight for 15 min. Samples were taken every 5 min, and the degradation efficiency was calculated by measuring the absorbance. The degradation efficiency was analyzed and calculated to be 15.8%.
[0036] The ultrasonic vibration conditions are the same as those in Example 1: 10 mg of CdIn2S4 powder catalyst and 30 ml of 10 mol / L Rhodamine B were weighed, stirred for 30 min in the dark to reach adsorption-desorption equilibrium, and degraded under ultrasonic vibration (240 W, 40 kHz) for 15 min. Samples were taken every 5 min, and the degradation efficiency was calculated by measuring the absorbance. The degradation efficiency was analyzed and calculated to be 8.2%.
[0037] Example 3
[0038] The other steps were the same as in Example 1, and a white powder was obtained, namely, BWO powder.
[0039] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 minutes in dark conditions to reach adsorption-desorption equilibrium, and degrade under sunlight and ultrasonic vibration for 15 minutes. Take samples every 5 minutes, measure the absorbance, and calculate the degradation efficiency. The degradation efficiency is 66% after analysis and calculation.
[0040] Example 4
[0041] The rest is the same as in Example 1, and a white powder is obtained, namely BWO powder. Thiourea (4mmol), cadmium chloride (1mmol) and indium (III) chloride tetrahydrate (2mmol) are added to 30mL deionized water, and ultrasonicated for 0.5h to completely dissolve. The mixed solution is transferred to a 100ml polytetrafluoroethylene-lined reactor, heated in an oven at 180°C for 48h, and filtered, washed, dried and ground after cooling to room temperature to finally obtain a yellow powder, namely CdIn2S4 catalyst. Then 1g BWO and 0.05g CdIn2S4 are weighed and dissolved in a certain amount of anhydrous ethanol, and the mixed solution is vigorously stirred at room temperature overnight (12h), filtered, washed, dried at 60°C overnight (12h), and ground at room temperature to finally obtain 5% 1T / 2H MS / BWO brown powder.
[0042] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 min in dark conditions to reach adsorption-desorption equilibrium, degrade under sunlight for 15 min, take samples every 5 min, measure the absorbance, calculate the degradation efficiency, and the degradation efficiency is 39.9% after analysis and calculation.
[0043] Example 5
[0044] The other steps were the same as in Example 4 to obtain 5% CIS / BWO brown powder.
[0045] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 min in dark conditions to reach adsorption-desorption equilibrium, degrade under ultrasonic vibration for 15 min, take samples every 5 min, measure the absorbance, calculate the degradation efficiency, and the degradation efficiency is 23.6% after analysis and calculation.
[0046] Example 6
[0047] The other steps were the same as in Example 4 to obtain 5% CIS / BWO brown powder.
[0048] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 minutes in dark conditions to reach adsorption-desorption equilibrium, and degrade under sunlight and ultrasonic vibration for 15 minutes. Take samples every 5 minutes, measure the absorbance, and calculate the degradation efficiency. The degradation efficiency is 87% after analysis and calculation.
[0049] Example 7
[0050] Weigh 1 g of BWO and 0.1 g of CdIn2S4, and other ingredients are the same as in Example 4 to obtain a 10% CIS / BWO brown powder.
[0051] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 min in dark conditions to reach adsorption-desorption equilibrium, degrade under sunlight for 15 min, take samples every 5 min, measure the absorbance, calculate the degradation efficiency, and the degradation efficiency is 57.6% after analysis and calculation.
[0052] Example 8
[0053] The other steps were the same as in Example 7 to obtain 10% CIS / BWO brown powder.
[0054] Weigh 10 mg of catalyst and 30 ml of 10 mol / L rhodamine B, stir for 30 min in dark conditions to reach adsorption-desorption equilibrium, degrade under ultrasonic vibration for 15 min, take samples every 5 min, measure the absorbance, calculate the degradation efficiency, and the degradation efficiency is 32.4% after analysis and calculation.
[0055] Figure 7 10%CIS / BWO catalyst and BWO hysteresis loop diagram; it can be seen that the addition of CIS changes the piezoelectricity of the composite.
[0056] Example 9
[0057] The other steps were the same as in Example 7 to obtain 10% CIS / BWO brown powder.
[0058] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 minutes in dark conditions to reach adsorption-desorption equilibrium, and degrade under sunlight and ultrasonic vibration for 15 minutes. Take samples every 5 minutes, measure the absorbance, and calculate the degradation efficiency. The degradation efficiency is 99.9% after analysis and calculation, which basically achieves complete degradation.
[0059] Stability experiment: After repeating the stability experiment four times, the degradation effect in piezoelectric photocatalysis still reached 99% in 15 minutes, and the stability was excellent.
[0060] Example 10
[0061] Weigh 1 g Bi2WO6 and 0.15 g CdIn2S4, and other ingredients are the same as in Example 4 to obtain 15% CIS / BWO brown powder.
[0062] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 min in dark conditions to reach adsorption-desorption equilibrium, degrade under sunlight for 15 min, take samples every 5 min, measure the absorbance, calculate the degradation efficiency, and the degradation efficiency is 35.2% after analysis and calculation.
[0063] Embodiment 11
[0064] The rest was the same as in Example 10 to obtain 15% CIS / BWO brown powder.
[0065] Weigh 10 mg of catalyst and 30 ml of 10 mol / L rhodamine B, stir for 30 min in dark conditions to reach adsorption-desorption equilibrium, degrade under ultrasonic vibration for 15 min, take samples every 5 min, measure the absorbance, calculate the degradation efficiency, and the degradation efficiency is 22.5% after analysis and calculation.
[0066] Example 12
[0067] The rest was the same as in Example 10 to obtain 15% CIS / BWO brown powder.
[0068] Weigh 10 mg of catalyst and 30 ml of 10 mol / L Rhodamine B, stir for 30 minutes in dark conditions to reach adsorption-desorption equilibrium, and degrade under sunlight and ultrasonic vibration for 15 minutes. Take samples every 5 minutes, measure the absorbance, and calculate the degradation efficiency. The degradation efficiency is calculated to be 81.1%.
[0069] The best ratio obtained from the degradation efficiency is 10% CIS / BWO.
Claims
1. Application of a typical type II heterojunction CdIn2S4 / Bi2WO6 piezoelectric-photocomposite catalyst in piezoelectric photodegradation of organic matter, characterized in that: Bi2WO6 and CdIn2S4 were prepared respectively, CdIn2S4 and Bi2WO6 were dissolved in anhydrous ethanol, stirred, mixed evenly, filtered, washed, dried and ground at room temperature to obtain CdIn2S4 / Bi2WO6 composite catalyst; the mass of CdIn2S4 was 10% of the mass of Bi2WO6; the catalyst was weighed and added to organic pollution, stirred in dark conditions to reach adsorption-desorption equilibrium, and degraded under sunlight irradiation and ultrasonic vibration; Preparation of Bi2WO6: Bismuth source and tungsten source are added to deionized water, stirred and dissolved at room temperature, and the mixture is transferred to a reactor lined with polytetrafluoroethylene, and a hydrothermal reaction is carried out in an oven; after cooling to room temperature, it is filtered, washed, dried, and ground to finally obtain a white powder, which is the Bi2WO6 catalyst BWO; Bi(NO3)3 . 5H2O as bismuth source; Na2WO4 . 2H2O as tungsten source; Bi(NO3)3 . 5H2O and Na2WO4 . The mass ratio of 2H2O is 2.9:1, the hydrothermal reaction temperature is 190°C, and the reaction time is 2h; Preparation of CdIn2S4: Add thiourea, cadmium chloride and indium III chloride tetrahydrate into deionized water, sonicate for 0.5 h to completely dissolve them, transfer the resulting transparent solution into a reactor lined with polytetrafluoroethylene, and carry out hydrothermal reaction in an oven; after cooling to room temperature, filter, wash, dry and grind to finally obtain a yellow powder, which is the CdIn2S4 catalyst; the molar ratio of thiourea, cadmium chloride and indium III chloride tetrahydrate is 4:1:2; the hydrothermal reaction temperature is 150℃-220℃, and the reaction time is 48h.