Front film materials and photovoltaic modules
By using the front film material of fluoroplastic transparent film and water-blocking film in the double-glass components, combined with the weather-resistant adhesive layer and the hydrophobic transmissive layer, the problems of high weight, low light transmittance and dust accumulation of the double-glass components are solved. It achieves high light transmission, high barrier and weather resistance, replaces glass packaging and is suitable for lightweight flexible photovoltaic modules.
Patent Information
- Application Number
- CN202210966366.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-08-12
AI Technical Summary
Due to the large weight, high cell fragmentation rate, difficulty in installation and glass burst, the double-glass components are not light transmittance, which cannot replace glass packaging, and dust accumulates after long-term outdoor use and affects the light transmittance effect.
A front film material is used, including a weather-resistant adhesive layer between the fluoroplastic transparent film and the water-blocking film. A hydrophobic and permeable layer is added to the surface of the fluoroplastic transparent film, and a magnesium fluoride, titanium dioxide and polydimethylsilic oxygen are used. Materials such as alkyl form a hydrophobic and transmissive layer, and the weather resistance and light transmittance of the material are improved by composite ultraviolet absorbers and antioxidants.
Improve the light transmittance of fluorine-containing plastic transparent film to more than 94%, realizes self-cleaning effect, extends the service life of photovoltaic modules, solves the problems of weight and installation difficulty, and provides a high light transmittance and high barrier , a new packaging material with strong weather resistance.
Smart Images

Figure CN115401969B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar photovoltaic manufacturing, and in particular to a front film material and a photovoltaic module. Background Art
[0002] With the continuous development of the solar photovoltaic industry, double-glass modules have broad application prospects in high-efficiency batteries, photovoltaic building integration, etc. However, due to the double-sided glass packaging, double-glass modules have problems such as heavy weight, high battery cell fragmentation rate, difficult installation, and glass bursting, and are subject to the load-bearing requirements of some industrial and commercial roofs and civil roofs.
[0003] Due to its crystal structure, PVDF has a low light transmittance of about 90%, which is not as high as glass (94%), so it cannot be used in large quantities. In addition, although the surface of PVDF itself has a certain degree of hydrophobicity, dust easily accumulates on its surface after being placed outdoors for a long time, thus affecting the overall light transmission effect. Summary of the invention
[0004] In order to solve the above problems, the present invention aims to provide a front film material and a photovoltaic module. The front film material is light, highly transparent, highly barrier, and highly weather-resistant, and can be used in the manufacture of lightweight and flexible photovoltaic modules.
[0005] In order to achieve the above-mentioned object, the present invention provides a front film material, which includes a fluorine-containing plastic transparent film and a water-blocking film, wherein a weather-resistant adhesive layer connecting the fluorine-containing plastic transparent film and the water-blocking film is provided between the two, and a hydrophobic permeability-enhancing layer is provided on the surface of the fluorine-containing plastic transparent film away from the water-blocking film; wherein the raw materials of the hydrophobic permeability-enhancing layer include magnesium fluoride, titanium dioxide and polydimethylsiloxane in a mass ratio of 1:1:10-10:1:1; in parts by mass, the raw materials of the fluorine-containing plastic transparent film include 85-100 parts of fluorine-containing plastics, 1-5 parts of antioxidants, 1-5 parts of composite ultraviolet absorbers and 1-5 parts of light stabilizers, wherein the composite ultraviolet absorber comprises an organic ultraviolet absorber and an inorganic ultraviolet absorber, and the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber is greater than 1:1 and less than 5:1; the inorganic ultraviolet absorber comprises inorganic nanoparticles with a particle size of 5nm-50nm, and the organic ultraviolet absorber comprises a benzotriazole ultraviolet absorber and / or a triazine ultraviolet absorber.
[0006] In a specific embodiment of the present invention, the light transmittance of fluorine-containing plastics such as PVDF is about 90%, which is lower than the light transmittance of glass; and although fluorine-containing plastics have a certain degree of hydrophobicity, after long-term outdoor use, dust will accumulate on the surface of fluorine-containing plastics, affecting the overall light transmittance effect. The present invention can increase the light transmittance of the fluorine-containing plastic transparent film to more than 94%, reaching a level equivalent to the light transmittance of glass, by adding a hydrophobic anti-transmission layer on the surface of the fluorine-containing plastic transparent film; and the hydrophobic anti-transmission layer can give the surface of the fluorine-containing plastic transparent film a self-cleaning effect, ensuring that the photovoltaic module containing the front film material generates electricity with high efficiency for a long time.
[0007] The raw material composition of the hydrophobic permeability-enhancing layer provided by the present invention is simple, and a good permeability-enhancing and hydrophobic effect is achieved through the synergistic effect between titanium dioxide and magnesium fluoride.
[0008] In the above hydrophobic anti-reflection layer, the particle size of the magnesium fluoride is generally 1nm-1000nm, and the particle size of the titanium dioxide is generally 1nm-1000nm. By controlling the particle sizes of magnesium fluoride and titanium dioxide within a specific range, it is beneficial to obtain lower surface energy and higher light transmittance, thereby obtaining an excellent hydrophobic anti-reflection effect.
[0009] In the above hydrophobic anti-reflection layer, the particle size of the polydimethylsiloxane may be 1 μm-1000 μm.
[0010] According to a specific embodiment of the present invention, the thickness of the hydrophobic anti-permeability layer can be controlled to be 1 μm-5 μm, and the contact angle between the hydrophobic anti-permeability layer and water can be 120°-150°, for example, can reach 137°.
[0011] According to a specific embodiment of the present invention, compared with adding an organic ultraviolet absorber alone or adding an inorganic ultraviolet absorber alone, by adding a certain proportion of organic ultraviolet absorbers and inorganic ultraviolet absorbers to form a composite ultraviolet absorber in a fluorine-containing plastic, not only can the weather resistance, ultraviolet isolation degree (especially the absorption of ultraviolet rays in the 300-400nm band) and long-term ultraviolet isolation of the fluorine-containing plastic transparent film formed by the fluorine-containing plastic be improved, so as to effectively protect the water-blocking film located at the lower layer of the fluorine-containing plastic transparent film from being destroyed; it can also improve the compatibility between the components of the fluorine-containing plastic transparent film, and avoid the precipitation of the fluorine-containing plastic transparent film under the wet and hot aging conditions. Through the synergistic effect of the composite ultraviolet absorber and the hydrophobic transmittance-enhancing layer, the fluorine-containing plastic transparent film can maintain a long-term high light transmittance.
[0012] According to a specific embodiment of the present invention, the raw material of the fluorine-containing plastic transparent film may further include 0-50 parts by mass of modified polymethyl methacrylate. The modified polymethyl methacrylate can improve the transverse toughness of the fluorine-containing plastic transparent film and enhance the processability of the fluorine-containing plastic, especially enhance the processability of the fluorine-containing plastic in the blow molding process.
[0013] In the above-mentioned fluorine-containing plastic transparent film, the fluorine-containing plastic may include PVDF or the like.
[0014] In the above-mentioned fluorine-containing plastic transparent film, the inorganic ultraviolet absorber comprises zinc oxide, or a combination of zinc oxide and titanium dioxide. By adding zinc oxide, diffuse reflection can be reduced, the overall transparency of the fluorine-containing plastic transparent film can be improved, and the light transmittance increase can make the photovoltaic module cell sheet where the front film material is located receive more light, so as to improve the overall power generation of the photovoltaic module. In addition, zinc oxide can also improve the absorption effect of the ultraviolet rays of the fluorine-containing plastic transparent film at 350nm-400nm (UVA band), and improve the weather resistance of the front film material as a whole. By adding a small amount of titanium dioxide, the self-cleaning performance of the fluorine-containing plastic transparent film can be further improved, and the hydrophobic anti-transmission layer can be kept super-hydrophobic in the long-term outdoor use process.
[0015] In the above-mentioned fluorine-containing plastic transparent film, when the inorganic ultraviolet absorber comprises a combination of zinc oxide and titanium dioxide, the mass ratio of zinc oxide to titanium dioxide is generally controlled to be 1:10-10:1, for example, it can be 2:1.
[0016] The present invention has found that by adjusting the particle size of inorganic nanoparticles in the inorganic ultraviolet absorber, better stability and structural uniformity can be obtained in the production process of fluorine-containing plastic transparent film. When the particle size of the inorganic nanoparticles is too large, the fluorine-containing plastic transparent film will have larger crystal points, and the product has higher haze and poor transparency; when the particle size of the inorganic nanoparticles is too small, obvious nanoparticle agglomeration will appear in the fluorine-containing plastic transparent film, causing adverse effects on the appearance of the product. The present invention can control the product haze within a suitable range by controlling the particle size of the inorganic nanoparticles within the range of 5-50nm, while effectively improving the production stability of the product and avoiding the problem of crystal points.
[0017] In some specific embodiments, the inorganic ultraviolet absorber can be zinc oxide with a particle size of 5nm-50nm, titanium dioxide with a particle size of 5nm-50nm, etc.
[0018] In the above-mentioned fluorine-containing plastic transparent film, the organic ultraviolet absorber is generally selected from long-term absorbers such as benzotriazole ultraviolet absorbers and triazine ultraviolet absorbers, which have strong absorption in the 300-350nm UVB band. Compared with benzotriazole ultraviolet absorbers, triazine ultraviolet absorbers have better durability. Specifically, the benzotriazole ultraviolet absorber can include 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol ultraviolet absorber (UV234 ultraviolet absorber).
[0019] According to a specific embodiment of the present invention, UVB has a greater impact on the aging process of the water-blocking film than UVA, and according to international standards, the proportion of UVB in the current laboratory UV aging box also needs to reach 3%-10%. Therefore, the amount of the organic UV absorber is generally controlled to be greater than the amount of the inorganic UV absorber to obtain better UVB blocking and anti-aging performance.
[0020] The present invention has found that in the composite ultraviolet absorber, the organic ultraviolet absorber is a consumable material. Once the organic ultraviolet absorber fails due to consumption, failure will expand from local to overall, affecting the overall weather resistance of the fluorine-containing plastic transparent film and the protective effect on the water-blocking film. In addition, if the organic ultraviolet absorber is not added in sufficient amount, it will also cause the overall weather resistance of the transparent film to be low, especially after UV200KWh, the fluorine-containing plastic transparent film will become brittle as a whole, lose toughness, and cannot protect the water-blocking film covered by it. If the amount of organic ultraviolet absorber added is too much, it is easy to cause the fluorine-containing plastic transparent film to have precipitation problems under dry heat and wet heat conditions: in some specific embodiments, the organic ultraviolet absorber will precipitate after being placed under dry heat conditions (such as room temperature) for 2 months, and will also precipitate under wet heat conditions such as PCT96h. The precipitation will seriously affect the overall light transmittance of the fluorine-containing plastic transparent film, thereby affecting the power generation efficiency of the component. Too high an inorganic ultraviolet absorber content will cause the surface of the fluorine-containing plastic transparent film to be rough, and because the inorganic ultraviolet absorbers such as nano zinc oxide and nano titanium oxide have large specific surface areas and surface energies, they are easy to agglomerate, thereby causing agglomeration during the processing process, resulting in obvious protruding crystal points and other defects in the appearance of the fluorine-containing plastic transparent film, affecting the appearance and reliability of the photovoltaic module; if the inorganic ultraviolet absorber content is too low, the composite ultraviolet absorber cannot effectively block the ultraviolet rays in the UVA band, thereby causing the fluorine-containing plastic transparent film as a whole to fail in the UVA band. Therefore, the present invention, by compounding the organic ultraviolet absorber and the inorganic ultraviolet absorber in a specific ratio, can not only effectively exert the ultraviolet absorption capacity of the two, but also greatly improve the structural stability and performance stability of the system, so that the front film material can still maintain a high ultraviolet isolation performance and light transmittance after long-term placement or aging conditions, and avoid precipitation. In a specific embodiment of the present invention, the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber is generally controlled to be greater than 1:1 and less than 5:1, preferably 2:1-4:1, for example, 2:1, 3:1 and 4:1.
[0021] In the above-mentioned fluorine-containing plastic transparent film, the antioxidant generally includes one or a combination of two or more of a hindered phenol antioxidant, a phosphite antioxidant, etc. In some specific embodiments, the antioxidant may also be a composite antioxidant, specifically a composite antioxidant comprising a hindered phenol antioxidant and a phosphite antioxidant. For example, the present invention may use a composite antioxidant in which the primary antioxidant is hindered phenol 1010 and the secondary antioxidant is phosphite 168.
[0022] In the above-mentioned fluorine-containing plastic transparent film, the light stabilizer generally includes one or a combination of two or more of a polymeric high molecular weight hindered amine light stabilizer, a low molecular weight hindered amine light stabilizer (HALS), and a non-polymeric high molecular weight hindered amine light stabilizer. Among them, the molecular weight of the polymeric high molecular weight hindered amine light stabilizer used in the present invention can be 2000-4000, for example, it can be Tinuvin 622; the molecular weight of the low molecular weight hindered amine light stabilizer used in the present invention can be 100-1000; the molecular weight of the non-polymeric high molecular weight hindered amine light stabilizer used in the present invention can be 100-200.
[0023] According to a specific embodiment of the present invention, the thickness of the fluorine-containing plastic transparent film is generally controlled to be 10μm-50μm, and the light transmittance of the fluorine-containing plastic transparent film at 400nm-1100nm can reach ≥91%; the blocking rate of the fluorine-containing plastic transparent film for ultraviolet rays at 280nm-380nm can reach ≥98%.
[0024] According to a specific embodiment of the present invention, the raw materials of the weather-resistant adhesive layer may include a pressure-sensitive adhesive, a liquid ultraviolet absorber combination, and a solid ultraviolet absorber combination.
[0025] According to a specific embodiment of the present invention, the mass ratio of the liquid ultraviolet absorber combination to the solid ultraviolet absorber combination can be controlled to be 3:97-5:95, and the total mass of the liquid ultraviolet absorber combination and the solid ultraviolet absorber combination accounts for 1%-10% of the total mass of the raw materials of the weather-resistant adhesive layer. The present invention has found that when the mass ratio of the liquid ultraviolet absorber combination to the solid ultraviolet absorber combination is 3:97-5:95, the weather-resistant adhesive layer has a higher ultraviolet blocking ability, and after aging treatment, the ultraviolet blocking ability of the weather-resistant adhesive layer remains at a higher level. In some specific embodiments, the ultraviolet blocking ability is better when the mass ratio of the liquid ultraviolet absorber combination to the solid ultraviolet absorber combination is 4:96.
[0026] In the weather-resistant adhesive layer, the pressure-sensitive adhesive may include one or a combination of two or more of acrylate pressure-sensitive adhesive, polyester pressure-sensitive adhesive, and polyurethane pressure-sensitive adhesive, etc. In some specific embodiments, the pressure-sensitive adhesive is preferably an acrylate pressure-sensitive adhesive, which has better long-term effectiveness than polyester pressure-sensitive adhesive and polyurethane pressure-sensitive adhesive, requires less solvent, and is more environmentally friendly.
[0027] In the above-mentioned weather-resistant adhesive layer, the acrylic pressure-sensitive adhesive generally adopts a one-component solvent-type pressure-sensitive adhesive, for example, a one-component solvent-type pressure-sensitive adhesive whose main component is a polyisocyanate resin can be adopted. In some specific embodiments, the solid content of the one-component solvent-type pressure-sensitive adhesive can be 30%-50%, and the viscosity of the one-component solvent-type pressure-sensitive adhesive at room temperature of 25°C is 3500-5500mPa·s. In a specific embodiment, when a solvent-type acrylic pressure-sensitive adhesive is adopted, the total mass of the raw materials of the weather-resistant adhesive layer is calculated by taking the mass of the solution of the solvent-type acrylic pressure-sensitive adhesive as the mass of the pressure-sensitive adhesive.
[0028] In the above-mentioned weather-resistant adhesive layer, by adding a liquid ultraviolet absorber combination and a solid ultraviolet absorber combination into the pressure-sensitive adhesive, the weather resistance of the pressure-sensitive adhesive can be improved, and the weather resistance and service life of the entire weather-resistant adhesive layer can be extended.
[0029] In the weather-resistant adhesive layer, the liquid ultraviolet absorber combination may include a liquid ultraviolet absorber, a liquid light stabilizer and a liquid antioxidant.
[0030] In the above liquid ultraviolet absorber combination, the liquid ultraviolet absorber may include liquid benzotriazole ultraviolet absorber UV-571 and / or liquid triazine ultraviolet absorber UV-400MPA, etc.
[0031] In the above liquid ultraviolet absorber combination, the liquid antioxidant includes liquid hindered phenol antioxidant AO-1135 and the like.
[0032] In the above liquid UV absorber combination, the liquid light stabilizer is generally a liquid composite light stabilizer. The composite light stabilizer includes a synergistic mixture of IRGANOX 1135, TINUVIN 571 and TINUVIN 765. In some specific embodiments, the composite light stabilizer can be composite light stabilizer B75 produced by BASF.
[0033] In the above liquid ultraviolet absorber combination, the mass ratio of the liquid ultraviolet absorber, the liquid light stabilizer and the liquid antioxidant is preferably 1:1:1-10:1:1.
[0034] In the weather-resistant adhesive layer, the solid ultraviolet absorber combination may include a solid ultraviolet absorber and a solid light stabilizer.
[0035] In the above solid ultraviolet absorber combination, the solid ultraviolet absorber may include one or a combination of two or more of powdered benzotriazole ultraviolet absorber UV-234, powdered triazine ultraviolet absorber UV-1577, powdered BETTERSOL UV-1697, etc.
[0036] In the above solid ultraviolet absorber combination, the solid light stabilizer is preferably a neutral solid light stabilizer, for example, a hindered amine light stabilizer (HALS) can be used. The hindered amine light stabilizer (HALS) includes HALS-292, HALS-123 and the like.
[0037] In the above solid ultraviolet absorber combination, the mass ratio of the solid ultraviolet absorber to the solid light stabilizer is preferably 1:5-5:1.
[0038] According to a specific embodiment of the present invention, the thickness of the weather-resistant adhesive layer can be controlled to be 20 μm-100 μm, the light transmittance of the weather-resistant adhesive layer at 400 nm-1100 nm can reach ≥90%, and the UV blocking rate at 280 nm-380 nm can reach ≥97%.
[0039] In the above-mentioned front film material, the water-blocking film may include a material with water-blocking performance or a material without water-blocking performance. For example, the material of the water-blocking film may specifically include film materials such as PET, polyester (such as polycarbonate), etc.
[0040] According to a specific embodiment of the present invention, the transmittance of the front film material at 400nm-1100nm can reach more than 93%; the blocking rate of the front film material for ultraviolet rays at 280-380nm can reach more than 98%, and the overall thickness of the front film material is 50μm-300μm.
[0041] According to a specific embodiment of the present invention, the method for preparing the front film material may include:
[0042] S1. Mix a liquid ultraviolet absorber, a liquid light stabilizer, a liquid antioxidant, a solid ultraviolet absorber, a solid light stabilizer and a solid antioxidant in proportion and mix them evenly, then mix the obtained mixture with a pressure-sensitive adhesive to obtain a raw material for a weather-resistant adhesive layer, preferably stirring and dissolving at a temperature of about 50°C to facilitate rapid dissolution of the solid ultraviolet absorber, the solid light stabilizer and the solid antioxidant; after complete dissolution, apply the raw material for the weather-resistant adhesive layer to the surface of the water-blocking film, control the thickness of the weather-resistant adhesive layer to 20 μm-100 μm (preferably 50 μm), let it stand at room temperature for 24 hours, and ripen at 60°C for 24 hours to form a weather-resistant adhesive layer;
[0043] S2, mixing fluorine-containing plastic, composite ultraviolet absorber, light stabilizer, antioxidant and modified polymethyl methacrylate, and obtaining a fluorine-containing plastic transparent film by double-layer extrusion film blowing;
[0044] S3, mixing magnesium fluoride, titanium dioxide and a solution of polydimethylsiloxane (generally using ethyl acetate as a solvent) at room temperature, stirring to form a raw material for a hydrophobic anti-reflection layer, and placing the raw material in a spraying device for standby use;
[0045] S4, compounding the surface of the fluorine-containing plastic transparent film and the weather-resistant adhesive layer; then spraying the raw material of the hydrophobic permeability-enhancing layer on the surface of the fluorine-containing plastic transparent film away from the water-blocking film, standing at room temperature for 24 hours, and ripening at 55° C. for 48 hours to obtain the front film material.
[0046] The present invention also provides a photovoltaic module, which includes the front film material. The front film material can be used as a transparent back plate for packaging of a double-sided module, and plays an excellent packaging and protection role.
[0047] The beneficial effects of the present invention are as follows: the front film material provided by the present invention is a new type of packaging material with high light transmittance, high barrier, strong weather resistance and light weight, which can replace the existing front cover glass, effectively solve the problems faced by glass packaging materials such as bulkiness, difficulty in installation, easy to burst, high fragmentation rate, etc., and can meet the outdoor use of solar photovoltaic modules. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a schematic structural diagram of the front film material of Example 1.
[0049] Figure 2 This is the water contact angle test diagram of sample 2 in test example 1.
[0050] Figure 3 This is a water contact angle test diagram of sample 3 in test example 1.
[0051] Figure 4 This is the SEM image of the crystal point area in sample 7 of test example 2.
[0052] Figure 5 This is the EDS analysis result of the crystal point area in sample 7 of test example 2.
[0053] Figure 6 This is a micrograph of the precipitation area on the surface of the sample in Test Example 3, in which the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber is 6:1.
[0054] Figure 7 This is a micrograph of the surface area of the sample in Test Example 3 in which the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber is 4:1.
[0055] Figure 8 These are the experimental results of long-term room temperature placement of the PVDF transparent film in Test Example 3 with a mass ratio of organic ultraviolet absorber to inorganic ultraviolet absorber of 4:1 and 6:1.
[0056] Explanation of symbols
[0057] Hydrophobic and permeability-enhancing layer 1, PVDF transparent film 2, weather-resistant adhesive layer 3, water-blocking film 4. DETAILED DESCRIPTION
[0058] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0059] Example 1
[0060] This embodiment provides a front film material, the structure of which is as follows Figure 1 As shown. The front film material includes a hydrophobic anti-reflection layer 1, a PVDF transparent film 2, a weather-resistant adhesive layer 3 and a water-blocking film 4 which are stacked in sequence. The weather-resistant adhesive layer 3 is used to connect the PVDF transparent film 2 and the water-blocking film 4. The weather-resistant adhesive layer 3 can avoid aging of the water-blocking film 4 by isolating most of the ultraviolet rays, thereby extending the service life of the front film material; the hydrophobic anti-reflection layer 1 is arranged on the surface of the PVDF transparent film 2 to provide self-cleaning and anti-reflection effects, so that the PVDF transparent film 2 can maintain a high light transmittance for a long time. The thickness of the hydrophobic anti-reflection layer 1 is 5μm, the thickness of the PVDF transparent film 2 is 25μm, and the thickness of the weather-resistant adhesive layer 3 is 50μm.
[0061] The preparation method of the front film material comprises:
[0062] 1. Weigh 2 g of magnesium fluoride, 1 g of titanium dioxide, 9 g of polydimethylsiloxane and 100 mL of ethyl acetate, dissolve the polydimethylsiloxane in ethyl acetate, stir at room temperature until dissolved, then add magnesium fluoride and titanium dioxide, stir and dissolve to form the raw materials of the hydrophobic anti-transmission layer 1;
[0063] The particle size of magnesium fluoride is 200 nm, the particle size of titanium dioxide is 50 nm, and the particle size of polydimethylsiloxane is 500 μm.
[0064] 2. In parts by mass, 100 parts of polyvinylidene fluoride, 30 parts of modified polymethyl methacrylate, 5 parts of a composite UV absorber, 5 parts of an antioxidant, and 5 parts of a light stabilizer are stirred to form a raw material for a PVDF transparent film; wherein the composite UV absorber is composed of an organic UV absorber and an inorganic UV absorber in a mass ratio of 4:1, the organic UV absorber is 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol UV absorber, the inorganic UV absorber is composed of zinc oxide and titanium dioxide in a mass ratio of 2:1, the particle sizes of zinc oxide and titanium dioxide are both 50 nm, the antioxidant is a composite antioxidant, the main antioxidant of the composite antioxidant is hindered phenol 1010, and the auxiliary antioxidant is phosphite 168; the light stabilizer is Tinuvin 622.
[0065] 3. Weigh 2g of liquid UV absorber, 1g of liquid light stabilizer, and 1g of liquid antioxidant as a liquid UV absorber combination, weigh 64g of solid UV absorber and 32g of solid light stabilizer as a solid UV absorber combination, and weigh 3400g of solvent-based acrylate pressure-sensitive adhesive. Mix the liquid UV absorber combination with the solid UV absorber combination, and then mix with the solvent-based acrylate pressure-sensitive adhesive, stir and dissolve evenly at 50°C to form the raw material for the weather-resistant adhesive layer;
[0066] Among them, the liquid UV absorber is the liquid triazine UV absorber UV-400MPA, the liquid light stabilizer is the liquid composite light stabilizer B75, the liquid antioxidant is the liquid hindered phenol antioxidant AO-1135, the solid UV absorber is the benzotriazole UV absorber UV-234, the solid light stabilizer is the hindered amine light stabilizer HALS-292, and the manufacturer of the solvent-based acrylate pressure-sensitive adhesive is Shanghai Weike Optoelectronic New Materials Co., Ltd., model XA640.
[0067] 4. Use a doctor blade coating device to coat the raw material of the weather-resistant adhesive layer on the surface of the water-blocking PET film, let it stand at room temperature for 24 hours, and mature it at 60°C in a drying tunnel for 24 hours. Then, compound the surface of the PVDF transparent film and the weather-resistant adhesive layer, and then spray the raw material of the hydrophobic and transmittance-enhancing layer on the surface of the PVDF transparent film (away from the water-blocking PET film), let it stand for 24 hours, and mature it at 55°C for 48 hours to obtain the front film material.
[0068] Example 2
[0069] This embodiment provides a front film material, the structure of which is as follows Figure 1 As shown. The front film material includes a hydrophobic anti-reflection layer 1, a PVDF transparent film 2, a weather-resistant adhesive layer 3 and a water-blocking film 4 which are stacked in sequence. The weather-resistant adhesive layer 3 is used to connect the PVDF transparent film 2 and the water-blocking film 4, and to avoid aging of the water-blocking film 4 by isolating most of the ultraviolet rays, thereby extending the service life of the front film material; the hydrophobic anti-reflection layer 1 is arranged on the surface of the PVDF transparent film 2, and is used to provide self-cleaning and anti-reflection effects, so that the PVDF transparent film can maintain a high light transmittance for a long time. The thickness of the hydrophobic anti-reflection layer 1 is 2μm, the thickness of the PVDF transparent film 2 is 25μm, and the thickness of the weather-resistant adhesive layer 3 is 50μm.
[0070] The preparation method of the front film material of this embodiment includes:
[0071] 1. The composition and proportion of the raw materials of the hydrophobic permeability-enhancing layer are the same as those in Example 1; wherein the particle size of magnesium fluoride is 50 nm, the particle size of titanium dioxide is 50 nm, and the particle size of polydimethylsiloxane is 100 μm.
[0072] 2. In parts by mass, 100 parts of polyvinylidene fluoride, 15 parts of modified polymethyl methacrylate, 3 parts of a composite UV absorber, 1 part of an antioxidant, and 1 part of a light stabilizer are stirred to form a raw material for a PVDF transparent film; wherein the composite UV absorber is composed of an organic UV absorber and an inorganic UV absorber in a mass ratio of 3:1, the organic UV absorber is a 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol UV absorber, the inorganic UV absorber is composed of zinc oxide and titanium dioxide in a mass ratio of 1:2, the particle sizes of zinc oxide and titanium dioxide are both 50 nm, the antioxidant is a composite antioxidant, the main antioxidant of the composite antioxidant is hindered phenol 1010, and the auxiliary antioxidant is phosphite 168; the light stabilizer is Tinuvin 622.
[0073] 3. Weigh 2g of liquid UV absorber, 1g of liquid light stabilizer, and 1g of liquid antioxidant as a liquid UV absorber combination, weigh 64g of solid UV absorber and 32g of solid light stabilizer as a solid UV absorber combination, and weigh 3400g of solvent-based acrylate pressure-sensitive adhesive. Mix the liquid UV absorber combination with the solid UV absorber combination, and then mix with the solvent-based acrylate pressure-sensitive adhesive, stir and dissolve evenly at 50°C to form the raw material for the weather-resistant adhesive layer;
[0074] Among them, the liquid UV absorber is the liquid triazine UV absorber UV-400MPA, the liquid light stabilizer is the liquid composite light stabilizer B75, the liquid antioxidant is the liquid hindered phenol antioxidant AO-1135, the solid UV absorber is the benzotriazole UV absorber UV-234, the solid light stabilizer is the hindered amine light stabilizer HALS-292, and the manufacturer of the solvent-based acrylate pressure-sensitive adhesive is Shanghai Weike Optoelectronic New Materials Co., Ltd., model XA640.
[0075] 4. Use a doctor blade coating device to coat the raw material of the weather-resistant adhesive layer on the surface of the water-blocking PET film, let it stand at room temperature for 24 hours, and mature it at 60°C in a drying tunnel for 24 hours. Then, compound the surface of the PVDF transparent film and the weather-resistant adhesive layer, and then spray the raw material of the hydrophobic and transmittance-enhancing layer on the surface of the PVDF transparent film (away from the water-blocking PET film), let it stand for 24 hours, and mature it at 55°C for 48 hours to obtain the front film material.
[0076] Example 3
[0077] This embodiment provides a front film material, the structure of which is as follows Figure 1As shown. The front film material includes a hydrophobic anti-reflection layer 1, a PVDF transparent film 2, a weather-resistant adhesive layer 3 and a water-blocking film 4 which are stacked in sequence. The weather-resistant adhesive layer 3 is used to connect the PVDF transparent film 2 and the water-blocking film 4, and to avoid aging of the water-blocking film 4 by isolating most of the ultraviolet rays, thereby extending the service life of the front film material; the hydrophobic anti-reflection layer 1 is arranged on the surface of the PVDF transparent film 2, and is used to provide self-cleaning and anti-reflection effects, so that the PVDF transparent film can maintain a high light transmittance for a long time. The thickness of the hydrophobic anti-reflection layer 1 is 5μm, the thickness of the PVDF transparent film 2 is 15μm, and the thickness of the weather-resistant adhesive layer 3 is 50μm.
[0078] The preparation method of the front film material comprises:
[0079] 1. The composition and proportion of the raw materials of the hydrophobic permeability-enhancing layer are the same as those in Example 1; wherein the particle size of magnesium fluoride is 70 nm, the particle size of titanium dioxide is 50 nm, and the particle size of polydimethylsiloxane is 200 μm.
[0080] 2. In parts by mass, 100 parts of polyvinylidene fluoride, 10 parts of modified polymethyl methacrylate, 3 parts of a composite UV absorber, 1 part of an antioxidant, and 1 part of a light stabilizer are stirred to form a raw material for a PVDF transparent film; wherein the composite UV absorber is composed of an organic UV absorber and an inorganic UV absorber in a mass ratio of 3:1, the organic UV absorber is a 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol UV absorber, the inorganic UV absorber is composed of zinc oxide and titanium dioxide in a mass ratio of 1:2, the particle sizes of zinc oxide and titanium dioxide are both 50 nm, the antioxidant is a composite antioxidant, the main antioxidant of the composite antioxidant is hindered phenol 1010, and the auxiliary antioxidant is phosphite 168; the light stabilizer is Tinuvin 622.
[0081] 3. Weigh 2g of liquid UV absorber, 1g of liquid light stabilizer, and 1g of liquid antioxidant as a liquid UV absorber combination, weigh 64g of solid UV absorber and 32g of solid light stabilizer as a solid UV absorber combination, and weigh 3400g of solvent-based acrylate pressure-sensitive adhesive. Mix the liquid UV absorber combination with the solid UV absorber combination, and then mix with the solvent-based acrylate pressure-sensitive adhesive, stir and dissolve evenly at 50°C to form the raw material for the weather-resistant adhesive layer;
[0082] Among them, the liquid UV absorber is the liquid triazine UV absorber UV-400MPA, the liquid light stabilizer is the liquid composite light stabilizer B75, the liquid antioxidant is the liquid hindered phenol antioxidant AO-1135, the solid UV absorber is the benzotriazole UV absorber UV-234, the solid light stabilizer is the hindered amine light stabilizer HALS-292, and the manufacturer of the solvent-based acrylate pressure-sensitive adhesive is Shanghai Weike Optoelectronic New Materials Co., Ltd., model XA640.
[0083] 4. Use a doctor blade coating device to coat the raw material of the weather-resistant adhesive layer on the surface of the water-blocking PET film, let it stand at room temperature for 24 hours, and mature it at 60°C in a drying tunnel for 24 hours. Then, compound the surface of the PVDF transparent film and the weather-resistant adhesive layer, and then spray the raw material of the hydrophobic and transmittance-enhancing layer on the surface of the PVDF transparent film (away from the water-blocking PET film), let it stand for 24 hours, and mature it at 55°C for 48 hours to obtain the front film material.
[0084] Test Example 1
[0085] This test example provides a test experiment of the overall UV blocking effect, light transmission effect and hydrophobic effect of the front film before and after the hydrophobic anti-reflection layer is coated on the surface of the PVDF transparent film.
[0086] Sample 1 is a front film material, and its preparation method is similar to that of Example 1, except that: Sample 1 does not contain a hydrophobic transmittance-enhancing layer, and the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber in the PVDF transparent film of Sample 1 is 3:1.
[0087] Sample 2 is a front film material, and its preparation method is similar to that of Example 1, except that the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber in the PVDF transparent film of Sample 2 is 3:1.
[0088] The test results are summarized in Table 1. The test band of light transmittance is 400nm-1100nm, and the test band of UV blocking rate is 280nm-380nm.
[0089] Table 1
[0090] UV blocking rate % Transmittance % Water contact angle (°) Sample 1 98.65% 90.94% 122 Sample 2 98.76% 93.27% 137
[0091] As can be seen from Table 1, the overall transmittance (400-1100nm) of the front film material without surface anti-reflection treatment is less than 91%, which is still a certain distance compared with photovoltaic glass (about 94%). After the PVDF transparent film is subjected to anti-reflection treatment (adding a hydrophobic anti-reflection film), the transmittance of the front film material with a hydrophobic anti-reflection layer is increased to 93%, which is close to that of glass, and the ultraviolet blocking ability is not affected. The above results show that the use of the method of the present invention to add a hydrophobic anti-reflection layer on the surface of the PVDF transparent film can greatly improve the overall transmittance of the PVDF transparent film and the front film material.
[0092] Figure 2 , Figure 3 The water contact angle test diagrams of sample 1 and sample 2 are respectively measured to be about 122° and 137° for sample 1 and sample 2. It can be seen from Table 1 that the hydrophobic anti-reflection layer can effectively improve the hydrophobicity of the surface of the front film material.
[0093] Test Example 2
[0094] This test example provides a product stability test for a PVDF transparent film containing inorganic UV absorbers of different particle sizes.
[0095] PVDF transparent films were prepared using inorganic nanoparticles with a particle size greater than 50 nm, a particle size of 5-50 nm, and a particle size less than 5 nm as inorganic ultraviolet absorbers, respectively, and were recorded as Sample 3, Sample 4, and Sample 5. The other component parameters and preparation methods of the PVDF transparent film raw materials of Sample 3, Sample 4, and Sample 5 were the same as those of Example 1. The haze test results and production stability results of each PVDF transparent film sample are summarized in Table 2.
[0096] Table 2
[0097] Haze % Production stability Sample 3 (particle size > 50 nm) 19.7 Large crystal point problem Sample 4 (particle size 5-50nm) 8.42 Amorphous point problem Sample 5 (particle size < 5 nm) 6.32 Large crystal point problem caused by agglomeration
[0098] Note: Large crystal spots refer to black spots with a diameter of ≥1.3mm on the PVDF transparent film under backlight; large crystal spot problems refer to the presence of large crystal spots on the film surface, and the number is >2 / m2;
[0099] The defect inspection machine was used to check the number of crystal points on the film surface during the production process of Sample 4 and Sample 5. The inspection results were as follows: during the production process of Sample 4, no black spots or transparent spots with a diameter ≥1.3mm were produced, and most of the black spots or transparent spots had a diameter between 0.5mm-1.3mm (excluding 1.3mm), with an average of 1-2 per square meter, and the PVDF transparent film had excellent appearance. During the mass production process of Sample 5, the large crystal points (diameter ≥1.3mm) on the surface were relatively dense, with an average of 8-10 per square meter, which seriously affected the appearance of the PVDF transparent film surface, caused poor overall material of the front film, and reduced the service life of the photovoltaic modules.
[0100] Figure 4 This is the SEM image of the crystal point area in sample 5. Figure 5 This is the EDS analysis result of the crystal point area in sample 5.
[0101] As can be seen from Table 2, when the particle size of the inorganic ultraviolet absorber is too large or too small, the PVDF transparent film will have a crystal point problem, affecting the structural uniformity of the film. In addition, if the particle size of the inorganic ultraviolet absorber is too large, it will increase the haze of the film material, thereby affecting the light transmittance of the PVDF transparent film (400nm-1100nm). Figure 4 and Figure 5 It can be seen that if the particle size of the inorganic UV absorber is too small, it will lead to the agglomeration of inorganic particles, mainly zinc oxide, and then form a crystal point area.
[0102] Test Example 3
[0103] This test example provides a test of the light transmittance, ultraviolet isolation and stability of a PVDF transparent film containing different proportions of inorganic ultraviolet absorbers and organic ultraviolet absorbers. Except for the mass ratio of the inorganic ultraviolet absorber and the organic ultraviolet absorber, the other component parameters and preparation methods of the PVDF transparent film in this test example are the same as those in Example 1. See Table 3 for the test results. In Table 3, 280nm-380nm is the test band for testing the ultraviolet blocking rate of the PVDF transparent film, and the test result is the blocking rate; 400nm-1100nm is the band for testing the light transmittance of the PVDF transparent film, and the test result is the light transmittance. The aging conditions of UV300KWh are in accordance with the ultraviolet aging test requirements specified in Section 6.26 of the T / CPIA 0031-2021 standard "Transparent protective film for double-sided battery module encapsulation", and the aging conditions of DH2000h are: continuous aging for 2000h at a temperature of 85°C and a relative humidity of 85RH%.
[0104] Table 3
[0105]
[0106] As can be seen from Table 3, the initial UV blocking ability (280nm-380nm) of the PVDF transparent film containing only a single inorganic UV absorber is only 56%, which cannot block ultraviolet rays for a long time. As the overall material of the front film, the single inorganic UV absorber cannot effectively protect the water-blocking film after aging under ultraviolet (UV) and damp heat (DH) conditions, thereby causing the overall front film to become brittle and fail; and the PVDF transparent film containing only a single organic UV absorber precipitated after being placed at room temperature for 2 months, and the transmittance of the transparent PVDF film in the wavelength range of 400nm-1100nm decreased by 2% compared with the initial value. In contrast, the PVDF transparent film provided by the present invention to which both inorganic ultraviolet absorbers and organic ultraviolet absorbers are added has good ultraviolet blocking ability and high transparency. Furthermore, when the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber is controlled to be 1:1-4:1, the structure of the prepared PVDF transparent film remains stable after aging under ultraviolet (UV) and wet heat (DH) conditions, no precipitation occurs, and a high ultraviolet blocking ability and transparency can be maintained.
[0107] When the mass ratio of organic UV absorber to inorganic UV absorber is 4:1, the UV blocking ability of the prepared PVDF transparent film is the best, and it will not cause precipitation problems under various aging conditions and long-term storage for more than 1 year, and the product has high stability.
[0108] Figure 6 This is a micrograph of the surface precipitation area of a sample with a mass ratio of organic UV absorber to inorganic UV absorber of 6:1 after DH2000h aging. Figure 7This is a micrograph of the surface area of a sample with a mass ratio of organic UV absorber to inorganic UV absorber of 4:1 after DH2000h aging. Figure 6 , Figure 7 All images were collected using a Keyence confocal microscope.
[0109] Figure 8 These are the experimental results of long-term storage at room temperature for samples with a mass ratio of organic UV absorber to inorganic UV absorber of 4:1 and 6:1.
[0110] From Table 3, Figure 6 , Figure 7 , Figure 8 It can be seen that when the organic UV absorber is excessive relative to the inorganic UV absorber, the PVDF transparent film will precipitate after being placed at room temperature for a long time, or precipitate after aging. When the inorganic UV absorber is excessive, the UV blocking ability decreases significantly, indicating that only when the mass ratio of the two UV absorbers is controlled within an appropriate range can high light transmittance, high UV isolation performance and long-term stability be achieved. Further comparison shows that adding two UV absorbers at the same time can ensure that the UV blocking ability of the transparent PVDF film under various aging conditions is maintained at more than 90%, thereby better protecting the water-blocking film and extending the service life of the overall material of the front film; on the other hand, it can ensure that the PVDF transparent film does not precipitate when placed indoors and outdoors for a long time, and continuously ensures a transmittance of 90% (400-1100nm), which is a technical effect that neither the addition of organic UV absorbers alone nor the addition of inorganic UV absorbers alone has.
[0111] Test Example 4
[0112] This test example provides a test experiment of the UV blocking effect, light transmittance and weather resistance of a weather-resistant adhesive layer with different UV absorbers added.
[0113] Among them, the aging conditions of UV300KWh are in accordance with the ultraviolet aging test requirements specified in Section 6.26 of the T / CPIA 0031-2021 standard "Transparent protective film for bifacial battery module encapsulation".
[0114] The experimental conditions of DH1000h are: continuous aging for 1000h at 85℃ and 85RH%.
[0115] TC200 test conditions: in an environmental test chamber that cycles between (-40℃)±2℃ and +85℃±2℃, the rate of temperature change between the highest and lowest temperatures does not exceed 100℃ / h, and at each extreme temperature, it should remain stable for at least 10 minutes, and the cycle time should not exceed 6 hours, for a total of 200 cycles. Two aging tests are conducted in accordance with IEC61215 standards.
[0116] The test band for light transmittance is 400-1100nm, and the test band for UV blocking rate is 280nm-380nm.
[0117] Samples 8 to 10 are front film materials, and the preparation methods are similar or the same as those of Example 1. The difference between the preparation methods of Sample 8 and Example 1 is that only a liquid UV absorber combination and an acrylate pressure-sensitive adhesive are added to the weather-resistant adhesive layer of Sample 8, and no solid UV absorber combination is added; the difference between the preparation methods of Sample 9 and Example 1 is that only a solid UV absorber combination and an acrylate pressure-sensitive adhesive are added to the weather-resistant adhesive layer of Sample 9, and no liquid UV absorber combination is added; the preparation method of Sample 10 is exactly the same as that of Example 1, that is, a solid UV absorber combination and a liquid UV absorber combination are added to the weather-resistant adhesive layer of Sample 10. The test results are summarized in Table 4.
[0118] Table 4
[0119]
[0120] From the results in Table 4, it can be seen that the UV blocking rate of the weather-resistant adhesive layer with a single liquid UV absorber as the UV absorbing component decreased significantly after UV300KWh, DH1000h and TC200 aging, indicating that the protective ability of the weather-resistant adhesive layer on the water-blocking film was weakened; the UV blocking ability and light transmittance of the weather-resistant adhesive layer with a single solid UV absorber as the UV absorbing component decreased significantly after DH1000h aging, which was due to the precipitation of the solid UV absorber at this time. The weather-resistant adhesive layer prepared by compounding a liquid UV absorber combination with a solid UV absorber combination can, on the one hand, ensure that the UV blocking ability of the material remains at an excellent level under various aging conditions, and on the other hand, it can also avoid the precipitation problem under humid and hot conditions, ensuring the overall long-term effectiveness and durability of the front film material.
Claims
1. A front film material, which comprises a hydrophobic anti-reflection layer, a fluorine-containing plastic transparent film, a weather-resistant adhesive layer and a water-blocking film stacked in sequence; in, The raw material of the hydrophobic anti-transmission layer is formed by dissolving polydimethylsiloxane in ethyl acetate, stirring at room temperature until dissolved, then adding magnesium fluoride and titanium dioxide, stirring and dissolving to form the raw material of the hydrophobic anti-transmission layer, wherein the mass ratio of magnesium fluoride, titanium dioxide and polydimethylsiloxane is 1:1:10-10:1:1; The raw materials of the fluorine-containing plastic transparent film are 85-100 parts of fluorine-containing plastic, 1-5 parts of antioxidant, 1-5 parts of composite ultraviolet absorber, and 1-5 parts of light stabilizer in parts by mass, wherein the composite ultraviolet absorber includes an organic ultraviolet absorber and an inorganic ultraviolet absorber, and the mass ratio of the organic ultraviolet absorber to the inorganic ultraviolet absorber is 2:1-4:1; The inorganic ultraviolet absorber is an inorganic nanoparticle with a particle size of 5nm-50nm, the organic ultraviolet absorber includes a benzotriazole ultraviolet absorber and / or a triazine ultraviolet absorber, and the inorganic ultraviolet absorber includes zinc oxide, or a combination of zinc oxide and titanium dioxide; In the raw materials of the hydrophobic anti-reflection layer, the particle size of the polydimethylsiloxane is 1 μm-1000 μm; the particle size of the magnesium fluoride is 1 nm-1000 nm, and the particle size of the titanium dioxide is 1 nm-1000 nm; The raw materials of the weather-resistant adhesive layer include a pressure-sensitive adhesive, a liquid ultraviolet absorber combination and a solid ultraviolet absorber combination; the liquid ultraviolet absorber combination includes a liquid ultraviolet absorber, a liquid light stabilizer and a liquid antioxidant; The solid ultraviolet absorber combination comprises a solid ultraviolet absorber and a solid light stabilizer; The mass ratio of the liquid ultraviolet absorber combination to the solid ultraviolet absorber combination is 3:97-5:95, and the total mass of the liquid ultraviolet absorber combination and the solid ultraviolet absorber combination accounts for 1%-10% of the total mass of the weather-resistant adhesive layer raw material; The thickness of the hydrophobic anti-reflection layer is 1 μm-5 μm, the thickness of the fluorine-containing plastic transparent film is 10 μm-50 μm, the thickness of the weather-resistant adhesive layer is 20 μm-100 μm, and the overall thickness of the front film material is 50 μm-300 μm.
2. The front film material according to claim 1, wherein: The fluorine-containing plastic includes PVDF.
3. The front film material according to claim 1, wherein: The mass ratio of the zinc oxide to the titanium dioxide is 1:10-10:
1.
4. The front film material according to claim 1, wherein: The organic ultraviolet absorber includes 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol.
5. The front film material according to claim 1, wherein: In the raw material of the fluorine-containing plastic transparent film, the antioxidant includes one or a combination of two or more of a hindered phenol antioxidant and a phosphite antioxidant; The light stabilizer includes one or a combination of two or more of a polymeric high molecular weight hindered amine light stabilizer, a low molecular weight hindered amine light stabilizer, and a non-polymeric high molecular weight hindered amine light stabilizer; wherein the molecular weight of the polymeric high molecular weight hindered amine light stabilizer is 2000-4000, the molecular weight of the low molecular weight hindered amine light stabilizer is 100-1000, and the molecular weight of the non-polymeric high molecular weight hindered amine light stabilizer is 100-200.
6. The front film material according to claim 1, wherein: The pressure-sensitive adhesive includes one or a combination of two or more of acrylate pressure-sensitive adhesive, polyester pressure-sensitive adhesive and polyurethane pressure-sensitive adhesive.
7. The front film material according to claim 1, wherein: The liquid ultraviolet absorber includes liquid benzotriazole ultraviolet absorber UV-571 and / or liquid triazine ultraviolet absorber UV-400MPA; The liquid antioxidant includes liquid hindered phenol antioxidant AO-1135; The liquid light stabilizer includes a liquid composite light stabilizer, and the composite light stabilizer includes a mixture of IRGANOX1135, TINUVIN 571 and TINUVIN 765; The solid ultraviolet absorber includes one or a combination of two or more of powdered benzotriazole ultraviolet absorber UV-234, triazine ultraviolet absorber UV-1577, and BETTERSOL UV-1697; The solid light stabilizer includes a hindered amine light stabilizer, and the hindered amine light stabilizer includes HALS-292 and / or HALS-123.
8. The front film material according to claim 1, wherein: In the liquid ultraviolet absorber combination, the mass ratio of the liquid ultraviolet absorber, the liquid light stabilizer and the liquid antioxidant is 1:1:1-10:1:1; In the solid ultraviolet absorber combination, the mass ratio of the solid ultraviolet absorber to the solid light stabilizer is 1:5-5:
1.
9. A photovoltaic module comprising the front film material according to any one of claims 1 to 8.
Citation Information
Cited By
Photovoltaic module non-glass front plate and preparation method and application thereof
CN121262894A