Polyethylene powder and moldings

By controlling the characteristic parameters and process conditions of polyethylene powder, the problem of degradation and contamination of ultra-high molecular weight polyethylene powder during processing is solved, and the high purity and strength of the molded body are achieved, making it suitable for high-demand industrial applications.

CN115403688BActive Publication Date: 2024-10-29ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202210549232.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-20
Publication Date
2024-10-29
Estimated Expiration
2042-05-20

AI Technical Summary

Technical Problem

Existing ultra-high molecular weight polyethylene powders suffer from deterioration, molecular weight reduction, gelation and contamination problems during processing, resulting in insufficient cleanliness and stability of molded bodies, especially in applications with high purity and high strength requirements.

Method used

By controlling the intrinsic viscosity of polyethylene powder, heat flow measured by oxidation induction time, metal component content and particle size distribution, polyethylene powder with excellent molecular weight stability and cleanability characteristics is prepared, using continuous polymerization and uniform catalyst introduction. and high-activity polymerization processes to reduce catalyst residues and abnormal reactions, and improve the mechanical strength and wear resistance of the molded body.

Benefits of technology

It achieves the molecular weight stability of polyethylene powder and excellent whiteness and cleanliness of the molded body. It is suitable for applications with high purity and high strength requirements, such as microporous membranes, fibers and high-strength fibers, and improves industrial practicality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003653904540000341
    Figure BDA0003653904540000341
  • Figure BDA0003653904540000351
    Figure BDA0003653904540000351
Patent Text Reader

Abstract

The present invention relates to polyethylene powder and a molded body. The present invention provides a polyethylene powder and a molded body thereof having excellent molecular weight stability and capable of obtaining a molded body having excellent whiteness and cleanliness. A polyethylene powder, wherein the intrinsic viscosity of the polyethylene powder is greater than or equal to 3.0 dl / g and less than 30.0 dl / g, and in the oxidation induction time measurement according to ISO11357-6 (2018) (150°C, oxygen, sample mass 5 mg), the heat flow of the polyethylene powder after switching to oxygen for 60 minutes is greater than or equal to 0.03 mW and less than 0.25 mW.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polyethylene powder and shaped bodies. Background Art

[0002] Polyethylene has been used in various applications such as films, sheets, microporous films, fibers, foams, and sintered bodies because it is easy to melt-process and a molded body obtained using polyethylene has high mechanical strength, excellent chemical resistance, and rigidity.

[0003] In particular, ultra-high molecular weight polyethylene has high practicality due to its higher mechanical strength, excellent sliding properties and wear resistance.

[0004] However, even if ultra-high molecular weight polyethylene melts at a temperature above the melting point, its fluidity is low, so it is difficult to make into pellets and is used in powder form. As methods for molding the ultra-high molecular weight polyethylene powder, there are known compression molding methods in which the ultra-high molecular weight polyethylene powder is pressurized under heating and then cut into a shape to be used; and molding methods in which the ultra-high molecular weight polyethylene powder is dissolved in a solvent such as liquid paraffin, then stretched and the solvent is removed to form a sheet or filament (for example, see Patent Documents 1 and 2).

[0005] On the other hand, in recent years, there has been an increasing demand for cleanliness of chemical solutions, cleaning water, and the like used in the manufacturing processes of displays, electronic components, various media devices, and the like.

[0006] For example, when ultra-high molecular weight polyethylene containing additives, impurities, and oligomers produced by deterioration is used as a container for storing high-purity chemicals, ultrapure water, etc. (hereinafter also referred to as the contact object) or as a filter for filtration, there is a problem that these substances may dissolve and contaminate the contact object or cause it to deteriorate.

[0007] In view of the above-mentioned problems, regarding high-purity polyethylene resin materials, for example, the following technology has been disclosed: a resin composition of ultra-high molecular weight polyethylene having an inherent viscosity of greater than 10 dl / g and less than 80 dl / g and polyethylene having a molecular weight distribution (Mw / Mn) of less than 4 is a polyethylene resin material having a small content of low molecular weight components and excellent cleanliness (for example, see Patent Document 3).

[0008] In addition, for example, the following technology is disclosed: ultra-high molecular weight polyethylene with an intrinsic viscosity of 10 dl / g or more and 60 dl / g or less has a low chlorine content, which inhibits corrosion of the molding machine and does not require the addition of metal soap as a neutralizing agent, so it has excellent cleaning properties (for example, see Patent Document 4).

[0009] Prior art literature

[0010] Patent Literature

[0011] [Patent Document 1] Japanese Patent No. 6195403

[0012] [Patent Document 2] Japanese Patent Application Publication No. 2020-16007

[0013] [Patent Document 3] Japanese Patent Application Publication No. 2017-165938

[0014] [Patent Document 4] Japanese Patent Application Publication No. 2018-145412 Summary of the invention

[0015] Problems to be solved by the invention

[0016] Regarding the compression molded body of ultra-high molecular weight polyethylene powder, in order to make it show excellent physical properties, it is necessary to make the powders completely fused to each other, and it is necessary to perform compression processing at high temperature for a long time. In addition, regarding the above-mentioned compression molded body, in recent years, the use of compression molded bodies with higher strength and excellent high dimensional accuracy has increased, and the necessity of compression molding for a longer time and a higher temperature than before, and annealing for a long time at a temperature below the melting point in order to relax the residual strain after molding has also increased. In addition, in the case of using ultra-high molecular weight polyethylene powder for diaphragms and high-strength fibers, the management of undissolved powder is also strictly carried out, so in order to make the ultra-high molecular weight polyethylene powder completely dissolved in the solvent, mixing is carried out at a longer time and a higher temperature than before. Ultra-high molecular weight polyethylene with excellent cleanliness and excellent whiteness is required in the above-mentioned various uses.

[0017] However, the technology disclosed in Patent Documents 1 and 2 has the following problem: in order to suppress the deterioration of ultra-high molecular weight polyethylene powder, a large amount of antioxidants, neutralizing agents such as calcium stearate are added, and then heat processing is performed to produce a molded body and high-strength fiber. When the molded body is used, the additives are dissolved, so the cleanliness is poor.

[0018] In addition, Patent Document 3 records that the discoloration (yellowing) and oxidative degradation caused by titanium are suppressed, and that the product is clean due to the small amount of low molecular weight components. However, there is no record of degradation caused by other metal components or the polymer structure of the ultra-high molecular weight polyethylene powder, and there are problems such as molecular weight reduction and gelation during the compression molding process with long-term heating.

[0019] Patent Document 4 describes reducing the chlorine content in ultrahigh molecular weight polyethylene powder, but contains a large amount of impurities such as catalyst residues, and does not describe suppressing degradation, which has the problem of limiting its use for applications requiring extremely strict cleanliness.

[0020] Therefore, in view of the above-mentioned problems of the prior art, an object of the present invention is to provide a polyethylene powder and a molded product thereof which are excellent in molecular weight stability and can provide a molded product having excellent whiteness and cleanability.

[0021] Means used to solve problems

[0022] The present inventors have conducted intensive studies to solve the above problems and have found that a polyethylene powder having a predetermined intrinsic viscosity and a predetermined heat flow in an oxidation induction time measurement can solve the above problems, thereby completing the present invention.

[0023] That is, the present invention is as follows. [1]

[0025] A polyethylene powder, wherein the intrinsic viscosity of the polyethylene powder is greater than or equal to 3.0 dl / g and less than 30.0 dl / g, and

[0026] In the oxidation induction time measurement according to ISO11357-6 (2018) (150°C, oxygen, sample mass 5 mg), the heat flow of the polyethylene powder 60 minutes after switching to oxygen is greater than or equal to 0.03 mW and less than 0.25 mW. [2]

[0028] The polyethylene powder according to the above-mentioned [1], wherein the content of Mg in the polyethylene powder is less than 10.0 ppm. [3]

[0030] The polyethylene powder according to the above [1] or [2], wherein the Ti content in the polyethylene powder is less than 3.0 ppm. [4]

[0032] The polyethylene powder according to any one of [1] to [3] above, wherein the content of Al in the polyethylene powder is less than 8.0 ppm. [5]

[0034] The polyethylene powder as described in any one of [1] to [4] above, wherein the content of α-olefin in the polyethylene powder is less than 0.10 mol %. [6]

[0036] The polyethylene powder according to any one of the above-mentioned [1] to [5], wherein the maximum rate of increase in weight of the polyethylene powder when heated at 200° C. in air for 1 hour is less than 2.0%. [7]

[0038] The polyethylene powder as described in any one of [1] to [6] above, wherein the total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm in the polyethylene powder is 50 mass % or more and less than 75 mass %. [8]

[0040] The polyethylene powder as described in any one of [1] to [7] above, wherein the close packing density of the polyethylene powder is greater than or equal to 0.50 g / cm 3 And less than 0.65g / cm 3 ,and

[0041] The polyethylene powder has a value obtained by dividing the compact bulk density by the loose bulk density (compact bulk density / loose bulk density) of greater than or equal to 1.05 and less than 1.30. [9]

[0043] The polyethylene powder according to any one of [1] to [8] above, wherein the content of Ca in the polyethylene powder is less than 10 ppm.

[10]

[0045] A molded product, wherein the molded product is a molded product of the polyethylene powder according to any one of [1] to [9] above.

[0046] Effects of the Invention

[0047] According to the present invention, there can be provided a polyethylene powder which is excellent in molecular weight stability and can give a molded product having excellent whiteness and cleanability, and a molded product thereof. DETAILED DESCRIPTION

[0048] Hereinafter, a mode for carrying out the present invention (hereinafter also referred to as “the present embodiment”) will be described in detail.

[0049] It should be noted that the following embodiments are examples for explaining the present invention, and are not intended to limit the present invention to the following contents. The present invention can be implemented with various modifications within the scope of the gist of the invention.

[0050] [Polyethylene powder]

[0051] The intrinsic viscosity of the polyethylene powder of this embodiment is greater than or equal to 3.0 dl / g and less than 30.0 dl / g, and in the oxidation induction time measurement (150°C, oxygen, sample mass 5 mg), the heat flow 60 minutes after switching to oxygen is greater than or equal to 0.03 mW and less than 0.25 mW.

[0052] With the above-mentioned configuration, the polyethylene powder of the present embodiment has excellent stability in molecular weight and can obtain a molded product having excellent whiteness and cleanability.

[0053] The polyethylene powder of the present embodiment is a so-called ultra-high molecular weight polyethylene powder having an intrinsic viscosity of 3.0 dl / g or more.

[0054] As the polyethylene constituting the polyethylene powder of the present embodiment, for example, an ethylene homopolymer or a copolymer of ethylene and other comonomers may be appropriately mentioned, but the present invention is not limited thereto.

[0055] There are no particular limitations on other comonomers, and examples thereof include α-olefins and vinyl compounds.

[0056] Examples of the α-olefins include, but are not limited to, α-olefins having 3 to 20 carbon atoms, and specifically include propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, and the like.

[0057] Examples of the vinyl compound include vinylcyclohexane, styrene, and derivatives thereof, but are not limited thereto.

[0058] Furthermore, non-conjugated polyenes such as 1,5-hexadiene and 1,7-octadiene may be used as other comonomers as necessary.

[0059] When the polyethylene powder of the present embodiment is a copolymer, the copolymer may be a ternary random polymer.

[0060] The other comonomers may be used alone or in combination of two or more.

[0061] When the ethylene copolymer is set to 100 mol%, the amount of other comonomers is preferably 0.1 mol% or less, more preferably 0.08 mol% or less, and further preferably 0.06 mol% or less. By adjusting the amount of other comonomers to 0.1 mol% or less, there is a tendency to reduce the generation of tertiary carbons that are easily degraded and to suppress the generation of oligomers. In addition, the catalyst activity in the polymerization reaction tends to increase, and the amount of metal components in the catalyst residue tends to be easily suppressed.

[0062] In addition, the comonomer amount of polyethylene can be confirmed by infrared analysis, NMR method, or the like.

[0063] (Intrinsic viscosity [η])

[0064] The intrinsic viscosity [η] of the polyethylene powder of the present embodiment is 3.0 dl / g or more and less than 30.0 dl / g, preferably 3.5 dl / g or more and less than 28.0 dl / g, and more preferably 4.0 dl / g or more and less than 26.0 dl / g.

[0065] In addition, the intrinsic viscosity can be measured in decalin at 135°C.

[0066] When the intrinsic viscosity [η] is 3.0 dl / g or more, the amount of low molecular weight components with poor oxidation resistance is small, the molecular chain breakage or crosslinking caused by degradation during molding is suppressed, and the degradation durability of the molded body is excellent. In addition, the molded body obtained from the polyethylene powder of this embodiment tends to be a molded body with sufficient mechanical strength and wear resistance.

[0067] On the other hand, when the intrinsic viscosity [η] is less than 30.0 dl / g, the catalyst activity in the polymerization reaction tends to be increased, and the amount of metal components in the catalyst residue tends to be easily suppressed. In addition, due to the excellent molding processability, the fusion force between the polyethylene powders is improved, thereby excellent mechanical strength, and the solubility of the polyethylene powder tends to be increased.

[0068] The intrinsic viscosity [η] of the polyethylene powder can be controlled within the above numerical range by appropriately adjusting the polymerization conditions described below, etc. Specifically, the intrinsic viscosity [η] can be controlled by allowing hydrogen as a chain transfer agent to exist in the polymerization system or by changing the polymerization temperature, etc.

[0069] The intrinsic viscosity [η] of the polyethylene powder of the present embodiment can be obtained by preparing solutions obtained by dissolving polyethylene powder in decalin at different concentrations, measuring the solution viscosity of the solution at 135° C., and extrapolating the reduced viscosity calculated from the measured solution viscosity to a concentration of 0. Specifically, it can be obtained by the method described in the Examples described later.

[0070] (Heat flow 60 minutes after switching to oxygen in the oxidation induction time measurement)

[0071] For the polyethylene powder of this embodiment, the heat flux 60 minutes after switching to oxygen in the oxidation induction time measurement according to ISO11357-6 (2018) (150°C, under oxygen, sample mass 5 mg) is greater than or equal to 0.03 mW and less than 0.25 mW, preferably greater than or equal to 0.04 mW and less than 0.24 mW, and more preferably greater than or equal to 0.05 mW and less than 0.23 mW.

[0072] The heat flow 60 minutes after switching to oxygen in the above-mentioned oxidation induction time measurement was 0.03 mW or more, which tends to indicate that a high-purity molded product can be obtained.

[0073] On the other hand, the heat flow after 60 minutes after switching to oxygen in the above-mentioned oxidation induction time measurement is less than 0.25 mW, which means that the polyethylene powder is not easily oxidatively degraded, and the breakage or cross-linking of the molecular chains caused by degradation during the molding process is suppressed. When a molded body is made, it becomes a molded body with excellent degradation durability, and a molded body with high whiteness tends to be obtained.

[0074] The heat flow in the oxidation induction time measurement is measured according to ISO11357-6 (2018), and the heat release caused by the oxidation reaction of polyethylene can be measured using a differential scanning calorimeter (DSC) or the like. As a measurement method, the test sample is heated in a nitrogen atmosphere, and then switched to an oxygen atmosphere when it reaches 150°C, and the heat flow after 60 minutes at a constant temperature of 150°C is measured. It should be noted that the details of the heat flow after 60 minutes after switching to oxygen in the oxidation induction time measurement at 150°C are described in the examples described later.

[0075] As a method for controlling the heat flux 60 minutes after switching to oxygen in the measurement of oxidation induction time to be within the range of 0.03 mW or more and less than 0.25 mW, there can be cited a method of producing polyethylene having a structure with less impurities that promote degradation as a polyethylene structure that is not easy to degrade without adding additives such as antioxidants. Specifically, there can be cited: reducing the generation of tertiary carbon that is easy to degrade to below a specified amount; reducing the double bonds at the ends of the polymer chains generated by abnormal reactions during polymerization and thermal degradation to below a specified amount; reducing metal components such as catalyst residues that promote oxidation degradation and oligomer components generated by abnormal reactions to below a specified amount; etc.

[0076] As a more specific method, the following methods can be cited: conducting a continuous polymerization uniformly in the system, wherein ethylene gas, solvent, catalyst, etc. are continuously supplied to the polymerization system, and unreacted ethylene gas and solvent are continuously discharged together with the generated polyethylene powder; a main catalyst and a co-catalyst are alternately introduced from the same pipeline to suppress local rapid polymerization; a polymerization reaction is adjusted to be highly active to suppress the amount of metal components in the catalyst residue; during the cooling of the polymerization reaction, a condenser is used for cooling with a jacket and cooling the vaporized solvent, etc., so that the polyethylene powder that has undergone an abnormal reaction along with the vaporized solvent is not fed into the polymerization reactor again; ethanol is introduced into a buffer tank before separating the polyethylene powder and the solvent so that the ethanol reaches 10% by mass of the solvent amount, thereby removing metal components and oligomer components as much as possible; while spraying water and isopropyl alcohol (70% by mass / 30% by mass) vapor to the polyethylene powder after polymerization and blowing nitrogen at a temperature of 100° C. to 110° C., the volatilized solvent and hydrochloric acid gas generated by the catalyst are removed; etc.

[0077] Generally, in the production process of polyethylene powder, polyethylene powder is easily oxidatively degraded due to local abnormal reactions during polymerization, insufficient purification, degradation during drying, etc. However, a major feature of the polyethylene powder of this embodiment is that it is not easily oxidatively degraded.

[0078] (Mg content)

[0079] The Mg content in the polyethylene powder of the present embodiment is preferably less than 10.0 ppm, more preferably less than 8.0 ppm, and even more preferably less than 6.0 ppm.

[0080] When the Mg content is less than 10.0 ppm, the oxidative degradation of polyethylene can be effectively suppressed, and the molecular weight reduction and gelation caused by the crosslinking reaction can be more effectively suppressed. In addition, when a molded body is made, the molded body has excellent degradation durability and has a tendency to suppress the coloration and embrittlement of the molded body.

[0081] The Mg content can be controlled within the above numerical range by increasing the productivity of polyethylene per unit catalyst.

[0082] The productivity of polyethylene per unit catalyst can be controlled by adjusting the polymerization temperature, polymerization pressure, and slurry concentration of the reactor when manufacturing polyethylene. That is, in order to improve the productivity of polyethylene per unit catalyst of the polyethylene constituting the polyethylene powder of the present embodiment, increasing the polymerization temperature, increasing the polymerization pressure, and / or increasing the slurry concentration can be cited.

[0083] The catalyst used is not particularly limited, and preferred catalysts include common Ziegler-Natta catalysts and metallocene catalysts.

[0084] As a method for improving the productivity of polyethylene per unit catalyst, the following methods can also be cited: alternately introducing the main catalyst and the co-catalyst from the same pipeline to suppress local rapid polymerization; using a jacket to cool the condenser and the vaporized solvent during the cooling of the polymerization reaction so that the polyethylene powder that has undergone abnormal reaction with the vaporized solvent is not put into the polymerization reactor again; introducing ethanol into the buffer tank before separating the polyethylene powder and the solvent so that the ethanol reaches 10% by mass of the solvent, thereby removing metal components and oligomer components as much as possible; separating the polyethylene powder and the solvent by centrifugal separation, and adjusting the solvent content contained in the polyethylene powder before drying to 70% by mass or less relative to the mass of the polyethylene powder; etc. It should be noted that the Mg content in the polyethylene powder can be measured by the method described in the examples described later.

[0085] (Ti content)

[0086] The Ti content in the polyethylene powder of the present embodiment is preferably less than 3.0 ppm, more preferably less than 2.5 ppm, and even more preferably less than 2.0 ppm.

[0087] When the Ti content is less than 3.0 ppm, the oxidative degradation of polyethylene can be effectively suppressed, and the molecular weight reduction and gelation caused by the crosslinking reaction can be more effectively suppressed. In addition, when a molded body is made, the molded body has excellent degradation durability and has a tendency to suppress coloration and embrittlement of the molded body.

[0088] As a method for adjusting the Ti content to less than 3.0 ppm, the same method as the above-mentioned method for controlling the Mg content can be applied.

[0089] (Al content)

[0090] The Al content in the polyethylene powder of the present embodiment is preferably less than 8.0 ppm, more preferably less than 7.0 ppm, and even more preferably less than 6.0 ppm.

[0091] When the Al content is less than 8.0 ppm, the oxidative degradation of polyethylene can be effectively suppressed, and the molecular weight reduction and gelation caused by the crosslinking reaction can be more effectively suppressed. In addition, when a molded body is made, the molded body has excellent degradation durability and has a tendency to suppress coloration and embrittlement of the molded body.

[0092] As a method for adjusting the Al content to less than 8.0 ppm, the same method as the above-mentioned method for controlling the Mg content can be applied.

[0093] (α-olefin content)

[0094] When the ethylene copolymer is taken as 100 mol %, the content of α-olefin in the polyethylene powder of the present embodiment is preferably less than 0.10 mol %, more preferably 0.08 mol % or less, and further preferably 0.06 mol % or less.

[0095] By adjusting the content of α-olefin to less than 0.10 mol%, the generation of tertiary carbons that are easily degraded can be reduced and the generation of oligomers can be suppressed. In addition, the catalyst activity in the polymerization reaction tends to increase, and the amount of metal components in the catalyst residue tends to be easily suppressed.

[0096] The α-olefin content in the polyethylene powder can be measured by infrared analysis or NMR.

[0097] The content of α-olefin in the polyethylene powder of the present embodiment can be controlled within the above-mentioned numerical range by adjusting the amount of α-olefin added to the polymerization reactor relative to ethylene.

[0098] (Maximum rate of oxidation weight increase)

[0099] The maximum oxidation weight increase rate of the polyethylene powder of this embodiment when heated at 200° C. in air is preferably less than 2.0%, more preferably less than 1.9%, and even more preferably less than 1.8%.

[0100] When the maximum oxidation weight increase rate of the polyethylene powder when heated at 200°C in air is less than 2.0%, the initial oxidation of polyethylene tends to be suppressed, and subsequent chain reaction decomposition tends to be less likely to occur. In addition, the storage stability of the polyethylene powder tends to be improved.

[0101] When polyethylene is heated in air, weight increase occurs due to oxidation, which is an initial reaction of degradation. The smaller the weight increase rate, the more likely it is to suppress subsequent molecular weight reduction caused by molecular chain breakage and gelation caused by cross-linking reaction. In addition, when polyethylene powder is stored for a long time in summer, polyethylene powder that is slightly degraded during storage but is not prone to initial oxidation reaction tends to have improved storage stability, so the smaller the maximum oxidation weight increase rate, the more preferred.

[0102] As a method for controlling the maximum rate of increase in oxidation weight of polyethylene powder when heated at 200°C in air to be less than 2.0%, the following method can be cited: conducting a continuous polymerization uniformly in the system, wherein ethylene gas, solvent, catalyst, etc. are continuously supplied to the polymerization system, and unreacted ethylene gas and solvent are continuously discharged together with the generated polyethylene powder; a main catalyst and a co-catalyst are alternately introduced from the same pipeline to suppress local rapid polymerization; a polymerization reaction is adjusted to be highly active to suppress the amount of metal components in the catalyst residue; and a catalyst is used in the cooling of the polymerization reaction. A jacket-cooled condenser is used to cool the vaporized solvent, etc., so that the polyethylene powder that has undergone abnormal reaction along with the vaporized solvent will not be fed back into the polymerization reactor; ethanol is introduced into the buffer tank before separating the polyethylene powder and the solvent so that the ethanol reaches 10% by mass of the solvent, thereby removing metal components and oligomer components as much as possible; while spraying water and isopropanol (70% by mass / 30% by mass) vapor to the polyethylene powder after polymerization and blowing nitrogen at a temperature above 100°C and below 110°C, the volatilized solvent and hydrochloric acid gas generated by the catalyst are completely removed; etc.

[0103] (Total mass ratio of particles with a particle size of 106 μm or more and less than 212 μm)

[0104] The preferred total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm in the polyethylene powder of this embodiment is 50 mass % or more and less than 75 mass %, more preferably 52 mass % or more and less than 73 mass %, and further preferably 54 mass % or more and less than 71 mass %.

[0105] The total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm is 50 mass % or more, and the amount of fine powder and coarse powder is small, so that the polyethylene powder has excellent powder fluidity. In addition, when the polyethylene powder is kneaded with a solvent such as liquid paraffin, the generation of lumps caused by fine powder and the generation of dissolved residues caused by coarse powder that is difficult to dissolve can be suppressed.

[0106] On the other hand, since the total mass proportion of particles having a particle size greater than or equal to 106 μm and less than 212 μm is less than 75 mass%, when compression molding is performed using a press or a plunger extruder, it is easy to fill the mold as densely as possible, and there is a tendency that molding strain is not easily retained in the molded body.

[0107] As a method for controlling the total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm in the polyethylene powder of the present embodiment within a range of 50% by mass or more and less than 75% by mass, a method of using a catalyst having a small particle size distribution as a catalyst used in the polymerization of polyethylene can be cited. In addition, by adjusting the conditions when the polyethylene is obtained by polymerization, the mass ratio of the above particle size of the polyethylene powder can be controlled. For example, by reducing the polymerization pressure or shortening the residence time in the reactor, the total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm can be controlled.

[0108] The total mass ratio of particles with a particle size greater than or equal to 106 μm and less than 212 μm can be calculated as follows: when classification is performed by sieving using sieves with mesh sizes of 300 μm, 212 μm, 150 μm, 106 μm, 75 μm, and 53 μm, the total mass of powder on the 106 μm and 150 μm sieves is divided by the total mass of the powder.

[0109] (Average particle size)

[0110] In addition, from the viewpoint of processability and handleability, the polyethylene powder of this embodiment preferably has an average particle size of 500 μm or less, more preferably 400 μm or less, and still more preferably 300 μm or less. The particle size at which the mass of the polyethylene powder remaining on each sieve obtained above is 50% by mass in the cumulative curve obtained by accumulating the mass of the polyethylene powder remaining on each sieve from the side with the smaller sieve hole size is the average particle size.

[0111] (Close packing density)

[0112] The close packing density of the polyethylene powder of this embodiment is preferably greater than or equal to 0.50 g / cm 3 And less than 0.65g / cm 3 , more preferably greater than or equal to 0.52 g / cm 3 And less than 0.63g / cm 3 , more preferably greater than or equal to 0.54 g / cm 3 And less than 0.61g / cm 3 .

[0113] The close packing density is 0.50g / cm 3 As described above, the polyethylene powder has few aggregates and irregular shapes and is close to a spherical shape, so the powder has excellent fluidity and is easy to fill into the mold most densely when compression molding is performed using a press or a plunger extruder, and molding strain is not likely to remain in the molded body.

[0114] On the other hand, the close packing density is less than 0.65 g / cm 3 , the powder solubility is excellent, it can be processed at a lower temperature and in a short time, and there is a tendency to obtain polyethylene powder with higher purity.

[0115] The dense packing density of the polyethylene powder of this embodiment is controlled to be equal to or greater than 0.50 g / cm 3 And less than 0.65g / cm 3 The method for synthesizing the polyol within the range of 1 to 400 Å can include a method of synthesizing using a general Ziegler-Natta catalyst or a metallocene catalyst, and a method of synthesizing using a catalyst described later is particularly preferred.

[0116] Furthermore, by suppressing the heat generation due to the rapid polymerization reaction occurring when the polyethylene powder is produced, the dense packing density of the polyethylene powder of the present embodiment can also be controlled within the above range.

[0117] As specific methods, the following methods can be listed: carrying out uniform continuous polymerization in the system, wherein ethylene gas, solvent, catalyst, etc. are continuously supplied to the polymerization system, and unreacted ethylene gas and solvent are continuously discharged together with the generated polyethylene powder; a main catalyst and a co-catalyst are alternately introduced from the same pipeline to suppress local rapid polymerization; during the cooling of the polymerization reaction, a condenser for cooling the vaporized solvent and the like is used to prevent the polyethylene powder that has undergone an abnormal reaction along with the vaporized solvent from being put into the polymerization reactor again; etc.

[0118] (tight packing density / loose packing density)

[0119] The value obtained by dividing the close packing density by the loose packing density (close packing density / loose packing density) of the polyethylene powder of this embodiment is preferably 1.05 or more and less than 1.30, more preferably 1.07 or more and 1.27 or less, and further preferably 1.09 or more and 1.24 or less.

[0120] When the value obtained by dividing the close packing density by the loose packing density is within the range of 1.05 or more and less than 1.30, the polyethylene powder has excellent fluidity, the generation of voids during compression molding can be further suppressed, and the mechanical properties of the molded body can be further improved.

[0121] The loose bulk density is the density measured in a state where the powder is loosely filled in a container of a predetermined volume (without tapping).

[0122] The tight packing density is the density measured by repeatedly dropping (vibrating) a container of a specified volume filled with powder from a certain height at a certain speed and tightly filling the container until the packing density of the powder in the container becomes substantially constant. Specifically, the tight packing density and the loose packing density can be measured by the method described in the examples described below.

[0123] The polyethylene powder having a value obtained by dividing the tight bulk density by the loose bulk density within the above range can be obtained by controlling the particle size distribution, particle shape, and the like.

[0124] (Ca content)

[0125] The Ca content in the polyethylene powder of the present embodiment is preferably less than 10.0 ppm, more preferably less than 8.0 ppm, and even more preferably less than 6.0 ppm.

[0126] When the Ca content is less than 10.0 ppm, less Ca is eluted and the polyethylene powder has a higher purity, and can be suitably used in a container or the like that prevents elution of impurities.

[0127] Examples of methods for controlling the Ca content in the polyethylene powder of the present embodiment to be less than 10.0 ppm include a method of using a catalyst not containing Ca, a method of not adding a neutralizing agent such as calcium stearate, and a method of not adding an additive containing Ca.

[0128] In addition, the Ca content in the polyethylene powder can be measured by the method described in the examples mentioned later.

[0129] [Method for producing polyethylene powder]

[0130] The polyethylene powder of the present embodiment can be produced by a conventionally known polymerization method.

[0131] As the polymerization method, for example, a method of polymerizing (copolymerizing) ethylene or a monomer containing ethylene by a slurry polymerization method, a gas phase polymerization method, or a solution polymerization method can be cited, but it is not limited thereto. A slurry polymerization method that can effectively remove the polymerization heat is particularly preferred. In the slurry polymerization method, an inert hydrocarbon medium can be used as the medium.

[0132] There are no particular restrictions on the inert hydrocarbon medium, and examples thereof include: aliphatic hydrocarbons such as propane, butane, isobutane, pentane, isopentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethyl chloride, chlorobenzene, and dichloromethane; and mixtures thereof.

[0133] In the polymerization process of polyethylene powder, it is preferred to use an inert hydrocarbon medium having a carbon number of 6 or more and 10 or less. If the carbon number is 6 or more, low molecular weight components generated by side reactions during ethylene polymerization and deterioration of polyethylene are relatively easy to dissolve and can be easily removed in the process of separating polyethylene from the polymerization medium. On the other hand, if the carbon number is 10 or less, there is a tendency to suppress the adhesion of polyethylene powder to the reaction tank, thereby enabling industrially stable operation.

[0134] The polymerization temperature in the production process of the polyethylene powder of the present embodiment is preferably 30°C or more and 100°C or less, more preferably 35°C or more and 95°C or less, and further preferably 40°C or more and 90°C or less. If the polymerization temperature is 30°C or more, the activity of the catalyst tends to be improved, the metal component as the catalyst residue remaining in the polyethylene can be reduced, and there is a tendency that industrially efficient production can be performed. On the other hand, if the polymerization temperature is 100°C or less, the attachment on the reaction tank can be suppressed, and the generation of polyethylene powder that has undergone abnormal reaction with the vaporized solvent can be suppressed, and there is a tendency that stable operation can be performed.

[0135] The polymerization pressure in the production step of the polyethylene powder is preferably normal pressure or higher and 2.0 MPa or lower, more preferably 0.1 MPa or higher and 1.5 MPa or lower, and even more preferably 0.1 MPa or higher and 1.0 MPa or lower.

[0136] The polymerization reaction can be carried out by any of the batch, semi-continuous and continuous methods, and the continuous method is particularly preferred. By continuously supplying ethylene gas, solvent, catalyst and the like into the polymerization system and continuously discharging the ethylene gas, solvent, catalyst and the like together with the generated polyethylene powder, it is possible to suppress the local high temperature state caused by the rapid reaction of ethylene, and it is possible to suppress the deactivation of the catalyst and side reactions, which tends to make the polymerization system more stable.

[0137] Alternatively, the polymerization may be performed in two or more steps with different reaction conditions.

[0138] In the production process of the polyethylene powder of the present embodiment, polyethylene is produced by using a catalyst component. Examples of the catalyst component include, but are not limited to, Ziegler-Natta catalysts, metallocene catalysts, and Phillips catalysts.

[0139] As the Ziegler-Natta catalyst, for example, the Ziegler-Natta catalyst described in Japanese Patent No. 5767202 can be appropriately used, and as the metallocene catalyst, for example, the metallocene catalyst described in Japanese Patent Publication No. 2006-273977 and Japanese Patent No. 4868853 can be appropriately used, but it is not limited thereto. In addition, the catalyst component used in the production process of the polyethylene powder of the present embodiment can contain a cocatalyst such as triisobutylaluminum and Tebbe reagent.

[0140] The average particle size of the above-mentioned catalyst is preferably 0.1 μm or more and 20 μm or less, more preferably 0.2 μm or more and 16 μm or less, and further preferably 0.5 μm or more and 12 μm or less. If the average particle size of the catalyst is 0.1 μm or more, there is a tendency to prevent the problems of scattering and adhesion of the obtained polyethylene powder. In addition, when the average particle size of the catalyst is 20 μm or less, there is a tendency to prevent the polyethylene powder from becoming too large and settling in the polymerization system or causing problems such as clogging of the pipeline in the post-processing process of the polyethylene powder. The particle size distribution of the catalyst is preferably narrow, and fine powder and coarse powder can also be removed by sieving, centrifugal separation, and cyclone separator.

[0141] In the manufacturing process of the polyethylene powder of the present embodiment, the introduction of the main catalyst and the co-catalyst is preferably added alternately from the bottom of the polymerization reactor using the same introduction line. As the adding method, there is no restriction, and it is preferred to repeat the following operation: continuously add the solid catalyst component as the main catalyst for 1 minute, then stop for 1 minute, then continuously add the co-catalyst such as triisobutylaluminum for 1 minute, and then stop for 1 minute. The catalyst reaction starts the reaction by contacting the main catalyst with the co-catalyst. By alternately adding from the same introduction line, the contact between the high concentration of the main catalyst and the co-catalyst just after addition can be reduced, and polyethylene can be generated without rapid reaction. Therefore, as a method for generating the polyethylene of the present embodiment with excellent resistance to oxidative degradation, it is the most preferred.

[0142] In the manufacturing process of the polyethylene powder of the present embodiment, ethylene gas is preferably introduced from the bottom of the polymerization reactor. In addition, for example, as described in the specification of German Patent Application Publication No. 3127133, the intrinsic viscosity of the obtained polyethylene powder can be controlled by allowing hydrogen to exist in the polymerization system or changing the polymerization temperature. In addition, by adding hydrogen as a chain transfer agent into the polymerization system, the intrinsic viscosity can be controlled within an appropriate range. When hydrogen is added into the polymerization system, the molar fraction of hydrogen is preferably 0 mol% or more and 30 mol% or less, more preferably 0 mol% or more and 25 mol% or less, and further preferably 0 mol% or more and 20 mol% or less.

[0143] In addition, in the present embodiment, in addition to the above-mentioned components, other known components useful for the production of polyethylene may be contained.

[0144] In the production process of the polyethylene powder of the present embodiment, the deactivation of the catalyst system after use is not particularly limited, and is preferably carried out in a buffer tank before centrifugal separation of the polyethylene powder and the solvent. Chemical agents for deactivating the catalyst system include, but are not limited to, oxygen, water, alcohols, glycols, phenols, carbon monoxide, carbon dioxide, ethers, carbonyl compounds, and alkynes.

[0145] The deactivation of the catalyst system is preferably carried out by introducing alcohol into the buffer tank so that the alcohol accounts for 5% to 20% by mass of the solvent. By adding a predetermined amount of alcohol to an inert hydrocarbon medium having 6 to 10 carbon atoms and stirring, metal components as catalyst residues, oligomer components generated by side reactions, etc. can be effectively extracted.

[0146] In the production process of the polyethylene powder of the present embodiment, the solvent and the polyethylene powder are separated after the polymerization reaction.

[0147] Examples of the solvent separation method include decantation, centrifugal separation, and filter filtration. Centrifugal separation is preferred from the viewpoint of high separation efficiency between the polyethylene powder and the solvent.

[0148] The amount of the solvent contained in the polyethylene powder after the solvent is separated is not particularly limited, but is preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less relative to the total mass of the polyethylene powder. By adjusting the amount of the solvent contained in the polyethylene powder to 70% by mass or less, there is a tendency that metal components, oligomer components, etc. contained in the solvent are less likely to remain in the polyethylene powder.

[0149] In the production process of the polyethylene powder of the present embodiment, after the solvent is separated, it is preferable to perform a drying treatment.

[0150] The drying temperature is preferably 80°C or higher and 150°C or lower, more preferably 90°C or higher and 140°C or lower, and further preferably 100°C or higher and 130°C or lower.

[0151] If the drying temperature is 80°C or higher, effective drying can be performed. On the other hand, if the drying temperature is 150°C or lower, the polyethylene powder can be dried while thermal degradation is suppressed. In the drying step, it is preferred that a mixed solution of water and alcohol (20 / 80% to 80 / 20% by mass) is sprayed onto the polyethylene powder after polymerization and the mixture is heated to 10 m / s. 3 The drying is performed while the inert gas is sprayed at a flow rate of more than 1 / hour to remove the volatile solvent. The drying is performed while the volatile matter is effectively removed by spraying an aqueous solution containing a more volatile alcohol, because low molecular weight components generated by side reactions and hydrochloric acid generated by catalyst deactivation can be reduced, and therefore it is preferred.

[0152] (additive)

[0153] The polyethylene powder of the present embodiment may contain, in addition to the above-mentioned components, other known components useful for the production of polyethylene powder.

[0154] The polyethylene powder of the present embodiment may further contain additives such as a neutralizing agent.

[0155] The neutralizing agent is used as a scavenger of chlorine contained in the polyethylene powder or a molding processing aid. There is no particular limitation on the neutralizing agent, and examples thereof include stearates of alkaline earth metals such as calcium, magnesium, and barium. There is no particular limitation on the content of the neutralizing agent, but it is preferably 1000 ppm or less, more preferably 600 ppm or less, and further preferably 200 ppm or less relative to the total amount of the polyethylene powder. In the polyethylene powder of this embodiment, since the additive may be eluted when the polyethylene powder and the molded body containing the polyethylene powder are used, it is preferred not to use the additive.

[0156] The content of the additive contained in the polyethylene of the present embodiment can be determined by extracting the additive in the polyethylene powder by Soxhlet extraction using tetrahydrofuran (THF) for 6 hours, and separating and quantifying the extract by liquid chromatography.

[0157] The polyethylene powder of the present embodiment may be blended with polyethylenes having different intrinsic viscosities, molecular weight distributions, etc., and may also be blended with other resins such as low-density polyethylene, linear low-density polyethylene, polypropylene, and polystyrene.

[0158] [Molding body]

[0159] The polyethylene powder of the present embodiment can be used for various purposes by various processing methods.

[0160] The molded product of the present embodiment can be produced by molding the polyethylene powder of the present embodiment. Since the molded product has high purity and excellent heat resistance, it can be suitably used as a microporous film, fiber, sheet, or bulk molded product.

[0161] Examples of such a molded article include separators for secondary batteries, particularly lithium ion secondary batteries, separators for lead acid batteries, and high-strength fibers.

[0162] In addition, by utilizing the excellent characteristics of wear resistance, high sliding properties, high strength, and high impact resistance that are the characteristics of ultra-high molecular weight polyethylene, it can be used for gears or rollers, curtain rails, pinball rails, lining sheets for storage silos for grain, etc., slip coatings for rubber products, etc., ski board materials and ski boot soles, lining materials for heavy machinery such as trucks and forklifts, etc. through solid state molding such as extrusion molding, press molding, and cutting.

[0163] Furthermore, the molded body obtained by sintering the polyethylene powder of the present embodiment can be used for, for example, a filter, a dust collecting material, a suction transport sheet, and the like.

[0164] Furthermore, the present invention can be suitably used in applications requiring cleanliness, such as containers for storing high-purity chemicals, ultrapure water, etc. (hereinafter, also referred to as contact objects) and filters for filtration.

[0165] [Example]

[0166] Hereinafter, the present embodiment will be described in detail with reference to specific examples and comparative examples, but the present embodiment is not limited to the following examples and comparative examples.

[0167] The measuring methods of various physical properties and characteristics are as follows.

[0168] [Measurement and evaluation methods of various physical properties and characteristics]

[0169] ((1) Determination of intrinsic viscosity [η])

[0170] 10 mg of polyethylene powder was added to 20 mL of decalin (containing 1 g / L of 2,6-di-tert-butyl-4-methylphenol) and stirred at 150°C for 2 hours to dissolve the polymer. The solution was placed in a constant temperature tank at 135°C using a Cannon-Fenske viscometer to measure the falling time (ts) between the markings. Similarly, the mass of the polyethylene powder was changed to prepare solutions at 3 points, and the falling time was measured.

[0171] The falling time (tb) of decalin alone without polyethylene powder added as a blank was measured. The reduced viscosity (ηsp / C) of the polymer obtained according to the following formula was plotted, and a linear equation of the concentration (C) (unit: g / dl) and the reduced viscosity (ηsp / C) of the polymer was derived, and the intrinsic viscosity [η] extrapolated to a concentration of 0 was obtained.

[0172] (ηsp / C)=(ts / tb-1) / C

[0173] ((2) Heat flow 60 minutes after switching to oxygen in the oxidation induction time measurement)

[0174] The heat flow 60 minutes after switching to oxygen in the oxidation induction time measurement was measured by an oxidation induction time test according to ISO11357-6 (2018).

[0175] The measurement was performed using a differential scanning calorimeter (manufactured by Shimadzu Corporation, trade name: DSC-60Plus).

[0176] First, put 5 mg of aluminum oxide in an aluminum pan for DSC measurement as a reference. Set it on the left side of the DSC-60Plus furnace, and set an aluminum pan with 5 mg (accurately weighed) polyethylene powder on the right side of the furnace. While nitrogen is flowing in the furnace at 25 mL / min, the temperature is raised from 40°C to 150°C at a heating rate of 25°C / min, and the temperature is left to stand for 5 minutes in this state, then the nitrogen is switched to oxygen and the measurement is started.

[0177] The sampling interval during measurement was set to 0.5 seconds.

[0178] The value obtained by subtracting the heat flow when switching the nitrogen gas to the oxygen gas from the heat flow after 60 minutes was defined as the heat flow after 60 minutes in the oxidation induction time measurement.

[0179] ((3) Mg, Ti, Al, Ca content)

[0180] The polyethylene powder was decomposed under pressure using a microwave decomposition device (model ETHOS TC, manufactured by Milestone General), and the elemental concentrations of magnesium, titanium, aluminum, and calcium were determined as the metal content in the polyethylene powder using an internal standard method using ICP-MS (inductively coupled plasma mass spectrometer, model X series X7, manufactured by Thermo Fisher Scientific).

[0181] ((4) α-olefin content)

[0182] The α-olefin content in the polyethylene powder was determined according to the method disclosed in Macromolecules, 10, 773 (1977) by GJ Ray et al.13 The α-olefin content was calculated from the area intensity of the methylene carbon signal observed in the C-NMR spectrum.

[0183] Measuring device: ECS-500 manufactured by JEOL Ltd.

[0184] Observation core: 13 C

[0185] Observation frequency: 100.53MHz

[0186] Pulse width: 45° (7.5 microseconds)

[0187] Pulse program: single pulse dec

[0188] PD: 5 seconds

[0189] Measuring temperature: 130℃

[0190] Cumulative times: more than 30,000 times

[0191] Benchmark: PE(-eee-) signal, 29.9ppm

[0192] Solvent: o-dichlorobenzene-d4

[0193] Sample concentration: 5 wt% to 10 wt%

[0194] Dissolving temperature: 130℃~140℃

[0195] ((5) Maximum rate of increase in oxidation weight)

[0196] Using a thermogravimetric analyzer (manufactured by PerkinElmer, trade name "Pyris1 TGA"), the temperature was raised from room temperature to 200°C under the conditions of sample weight: 5 mg, oxygen flow rate: 10 mL / min, and heating rate: 30°C / min, and the temperature was maintained for 1 hour, and then the weight increase rate was measured. It was confirmed that the weight of the polyethylene powder increased the most due to oxidation within about 30 minutes from the start of the measurement, and then the weight gradually decreased. The ratio of the maximum weight increase was taken as the maximum oxidation weight increase rate.

[0197] ((6) Total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm, and average particle size)

[0198] The total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm is measured as follows.

[0199] 100 g of polyethylene powder was weighed in a 200 mL plastic cup, 1 g of carbon black was added, and the mixture was stirred thoroughly with a spoon. The stirred polyethylene powder was classified by passing through sieves with mesh sizes of 300 μm, 212 μm, 150 μm, 106 μm, 75 μm, and 53 μm according to the JIS Z 8801 standard. The total mass of the powder on the 106 μm and 150 μm sieves was divided by the total mass of the powder as the total mass ratio (mass %) of particles with a particle size of 106 μm or more and less than 212 μm.

[0200] In addition, in the cumulative curve obtained by accumulating the mass of the polyethylene powder remaining on each sieve from the side with the smaller mesh size, the particle size when it reached 50% by mass was taken as the average particle size.

[0201] ((7) Tight packing density / loose packing density)

[0202] The compact bulk density and loose bulk density were measured using a powder tester PT-X model (manufactured by Hosokawa Micron Co., Ltd.).

[0203] The sample supply device was vibrated to allow the polyethylene powder to flow down a 100 cm stainless steel 3 The polyethylene powder was placed in a cylindrical container until it was full. The excess polyethylene powder on the container was scraped off with a blade and the measured density was taken as the loose bulk density (g / cm 3 ).

[0204] In addition, in stainless steel 100cm 3 The cylindrical container was covered with a lid, and the polyethylene powder was made to flow down by vibrating the sample supply device. The vibration was carried out under the conditions of a stroke length (vibration height) of 18 mm, a vibration speed of 60 times / min, and a vibration number of 180 times. Then, the excess polyethylene powder on the container was scraped off with a blade, and the measured density was taken as the compacted bulk density (g / cm 3 ).

[0205] The value of the close packing density / the loose packing density is determined by dividing the measured value of the close packing density measured in the above manner by the measured value of the loose packing density measured in the above manner.

[0206] ((8) Whiteness of the molded body)

[0207] According to ISO11542-2, the molded body was produced by preheating at 220°C and 5 MPa for 5 minutes, and then heating and compressing at 220°C and 10 MPa for 45 minutes. Then, annealing was performed at 100°C for 24 hours.

[0208] The whiteness of the molded article was measured and evaluated using a colorimeter CR-20 (manufactured by Konica Minolta, Inc.) in accordance with the measurement standard CIE / ASTM E313-96.

[0209] The evaluation criteria are as follows.

[0210] 〇…The whiteness of the molded body is 95 or more.

[0211] △…The whiteness of the molded body is 90 or more and less than 95.

[0212] ×…The whiteness of the molded product is less than 90.

[0213] The following results were obtained: the polyethylene powder of the examples had high whiteness, was excellent in resistance to oxidative degradation, did not discolor, and had excellent whiteness even when heated and compressed for a long period of time.

[0214] ((9) Molecular weight reduction rate during kneading)

[0215] When the total amount of the polyethylene powder and the liquid paraffin was 100 parts by mass, 30 parts by mass of the polyethylene powder and 70 parts by mass of the liquid paraffin were mixed to prepare a slurry-like liquid.

[0216] The obtained slurry-like liquid was fed into a twin-screw extruder through a feeder and kneaded at 230°C for 30 minutes to obtain a polyethylene gel. The polyethylene gel was extruded from a T-die set at the front end of the extruder, and then immediately cooled and solidified using a casting roll cooled to 25°C to form a gel sheet. The gel sheet was stretched to 7×7 times at 120°C using a synchronous biaxial stretching machine to obtain a stretched film. The stretched film was then immersed in hexane to completely extract and remove the liquid paraffin, and then vacuum dried at 50°C for 12 hours.

[0217] The molecular weight reduction rate was calculated by the following formula: the value obtained by subtracting the intrinsic viscosity of the stretched film from the intrinsic viscosity of the raw polyethylene powder was divided by the intrinsic viscosity of the raw polyethylene powder and the obtained value was multiplied by 100.

[0218] {[(intrinsic viscosity of polyethylene powder) - (intrinsic viscosity of stretched film)] / (intrinsic viscosity of polyethylene powder)} × 100 (%)

[0219] The molecular weight reduction rate was evaluated based on the following criteria.

[0220] The evaluation criteria are as follows.

[0221] 〇 ... The molecular weight reduction rate is 10% or less.

[0222] △ ... The molecular weight reduction rate is greater than 10% and less than or equal to 15%.

[0223] ×…The molecular weight reduction rate is greater than 15%.

[0224] ((10) Cleanliness)

[0225] 500 mL of ultrapure water (purified using TrePure LV-10T (manufactured by Toray Industries, Inc.) (registered trademark)) was placed in a 1 L round glass container, the container was capped, and the container was shaken and washed for 30 seconds, and then drained. This shaking and washing was repeated 5 times.

[0226] The container was again filled with 500 mL of ultrapure water, and a molded body with a width of 2 cm, a length of 15 cm, and a thickness of 4 mm produced according to ISO11542-2 was introduced therein, and the container was covered with a lid and shaken for 30 seconds, and then drained. This shaking and washing was repeated 5 times.

[0227] Next, 500 mL of ultrapure water was added to the 1 L round glass container containing the molded body, and the mixture was shaken for 4 weeks at 70° C. After 4 weeks, 5 mL of the filled water was collected, and the number of particles of 0.1 μm or more leached therein was measured using a particle counter (KL-22 (manufactured by RION Corporation)).

[0228] The number of particles contained in water was calculated using the following formula and this was taken as the cleanliness.

[0229] The calculation formula and evaluation criteria are as follows.

[0230] Cleanliness: Number of particles in water (pieces / mL) = {(number of counts (pieces)) × (volume of ultrapure water 100 (mL))} / {sample volume 5 (mL) × container capacity 200 (mL)}

[0231] 〇…less than 40 / mL.

[0232] △…≥40 / mL and less than 70.

[0233] ×…70 cells / mL or more.

[0234] [(Production Example) Synthesis of Catalyst]

[0235] (Preparation of solid catalyst component [A])

[0236] 1600 mL of hexane was added to an 8 L stainless steel autoclave that had been fully purged with nitrogen. 800 mL of a 1 mol / L titanium tetrachloride hexane solution and 800 mL of a 1 mol / L AlMg5(C4H9) solution having the composition formula were added simultaneously over 4 hours at 10°C while stirring. 11 A hexane solution of an organomagnesium compound represented by (OSiH) 2 was added. After the addition, the temperature was slowly raised and the reaction was continued at 10°C for 1 hour.

[0237] After the reaction was completed, 1600 mL of the supernatant was removed and washed five times with 1600 mL of hexane to prepare a solid catalyst component [A].

[0238] The amount of titanium contained in 1 g of the solid catalyst component [A] was 3.05 mmol.

[0239] (Preparation of solid catalyst component [B])

[0240] <(1) Synthesis of raw material (b-1)>

[0241] 2000 mL of 1 mol / L Mg6(C4H9) was added to an 8 L stainless steel autoclave that had been fully purged with nitrogen. 12 Al(C2H5)3 hexane solution (equivalent to 2000 mmol in terms of magnesium and aluminum) was added dropwise with 146 mL of 5.47 mol / L n-butanol hexane solution for 3 hours while stirring at 50°C, and the pipeline was cleaned with 300 mL of hexane after the reaction. Then, stirring was continued at 50°C for 2 hours. After the reaction was completed, the solution cooled to room temperature was used as raw material (b-1). The raw material (b-1) had a total concentration of 0.704 mol / L of magnesium and aluminum.

[0242] <(2) Synthesis of raw material (b-2)>

[0243] 2000 mL of 1 mol / L Mg6(C4H9) was added to an 8 L stainless steel autoclave that had been fully purged with nitrogen. 12 A hexane solution of Al(C2H5)3 (equivalent to 2000 mmol in terms of magnesium and aluminum) was added dropwise with 240 mL of a hexane solution of 8.33 mol / L methylhydrogenpolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd.) for 3 hours while stirring at 80°C, and the pipeline was cleaned with 300 mL of hexane after the reaction. Then, stirring was continued at 80°C for 2 hours. After the reaction was completed, the solution cooled to room temperature was used as raw material (b-2). The raw material (b-2) had a total concentration of 0.786 mol / L of magnesium and aluminum.

[0244] <(3) (B-1) Synthesis of carrier>

[0245] 1000 mL of a 1 mol / L hexane solution of hydroxytrichlorosilane was added to an 8 L stainless steel autoclave after full nitrogen substitution, and 1340 mL of a hexane solution of an organic magnesium compound of the raw material (b-1) (equivalent to 943 mmol of magnesium) was added dropwise at 65° C. for 3 hours, and then the reaction was continued while stirring at 65° C. for 1 hour. After the reaction was completed, the supernatant was removed and washed 4 times with 1800 mL of hexane to obtain a carrier (B-1). The carrier was analyzed, and the magnesium contained in 1 g of solid was 7.5 mmol.

[0246] <(4) Preparation of solid catalyst component [B]>

[0247] To 1970 mL of hexane slurry containing 110 g of the carrier (B-1), 103 mL of a 1 mol / L hexane solution of titanium tetrachloride and 131 mL of the raw material (b-2) were added simultaneously over 3 hours while stirring at 10°C.

[0248] After the addition, the reaction was continued for 1 hour at 10° C. After the reaction was completed, the supernatant was removed and washed four times with hexane to remove unreacted raw material components, thereby preparing a solid catalyst component [B].

[0249] [Example 1]

[0250] (Manufacture of polyethylene)

[0251] Hexane, ethylene, 1-butene, hydrogen, and a catalyst were continuously supplied to a 300 L container-type polymerization reactor equipped with a stirring device.

[0252] Hexane was supplied from the bottom of the polymerization reactor at 80 L / hour.

[0253] Ethylene gas was supplied from the bottom of the polymerization reactor to maintain the polymerization pressure at 0.3 MPa.

[0254] 1-Butene and hydrogen were supplied to the upper gas phase portion of the polymerization reactor so that the gas phase concentration of 1-butene relative to ethylene was 0.25 mol% and the gas phase concentration of hydrogen relative to ethylene and 1-butene was 11.2 mol%.

[0255] A solid catalyst component [A] and triisobutylaluminum as a co-catalyst were used as catalysts. The solid catalyst component [A] was added at a rate of 0.2 g / hour and triisobutylaluminum was added at a rate of 10 mmol / hour alternately from the bottom of the polymerization reactor using the same introduction line. As an addition method, the following operation was repeated: the solid catalyst component [A] was added continuously for 1 minute, then stopped for 1 minute, and then triisobutylaluminum was added continuously for 1 minute, then stopped for 1 minute.

[0256] The polymerization temperature was maintained at 78° C. by a condenser that was cooled by a jacket and cooled the vaporized solvent, etc. It should be noted that a filter with a mesh size of 75 μm was set in the pipeline for returning the solvent cooled by the condenser to the polymerization reactor so that the polyethylene powder mixed in the solvent would not be put into the polymerization reactor again.

[0257] The catalyst activity was 12000 g-PE / g-solid catalyst component [A], and the slurry concentration was 27%.

[0258] The obtained polymerization slurry is continuously withdrawn into a flash tank equipped with a stirring device so that the liquid level of the polymerization reactor is kept constant, and unreacted ethylene and hydrogen are separated.

[0259] Next, the polymerized slurry was continuously pumped out into a buffer tank equipped with a stirring device so that the liquid level of the flash tank was kept constant. Ethanol was introduced into the buffer tank so that the ethanol content reached 10% by mass of the solvent, and stirred for 1.5 hours.

[0260] Next, the polymerized slurry was continuously sent to a centrifuge to keep the liquid level of the buffer tank constant, and polyethylene was separated from the solvent and the like other than polyethylene to obtain polyethylene powder. The content of the solvent and the like relative to polyethylene at this time was 55%.

[0261] The separated polyethylene powder was dried at 105° C. for 2 hours. It should be noted that the polyethylene powder after polymerization was sprayed with steam of water and isopropyl alcohol (70% by mass / 30% by mass) and heated at 15 m / s. 3 The drying step was performed while blowing nitrogen at a flow rate of 1000 rpm to remove the volatilized solvent. The polyethylene powder obtained was sieved with a mesh size of 425 μm to remove the powder that did not pass through the sieve, thereby obtaining the polyethylene powder of Example 1. The physical properties of the obtained polyethylene powder are shown in Table 1.

[0262] [Example 2]

[0263] In the polymerization step, 1-butene was not introduced, hydrogen was introduced in such a manner that the gas phase concentration relative to ethylene was 10.6 mol%, and solid catalyst component [B] was used instead of solid catalyst component [A]. The polyethylene powder of Example 2 was obtained by the same operation as in Example 1. The catalyst activity was 12000 g-PE / g-solid catalyst component [B], and the slurry concentration was 29%.

[0264] [Example 3]

[0265] In the polymerization step, the polymerization temperature was set to 76° C., 1-butene was not introduced, and hydrogen was introduced in such a manner that the gas phase concentration relative to ethylene was 0.18 mol %, and the polyethylene powder of Example 3 was obtained by the same operation as in Example 1. It should be noted that the catalyst activity was 16000 g-PE / g-solid catalyst component [A], and the slurry concentration was 28%.

[0266] [Example 4]

[0267] In the polymerization step, the polymerization temperature was set to 71° C., the polymerization pressure was set to 0.35 MPa, hydrogen was introduced in such a manner that the gas phase concentration relative to ethylene was 0.20 mol %, and the solid catalyst component [B] was used instead of the solid catalyst component [A]. The polyethylene powder of Example 4 was obtained by the same operation as in Example 1. It should be noted that the catalyst activity was 20,000 g-PE / g-solid catalyst component [B], and the slurry concentration was 25%.

[0268] [Example 5]

[0269] In the polymerization step, 150 ppm of calcium stearate was introduced relative to the polyethylene powder, and the polyethylene powder of Example 5 was obtained by the same operation as in Example 4. The catalyst activity was 20000 g-PE / g-solid catalyst component [B], and the slurry concentration was 25%.

[0270] [Example 6]

[0271] In the polymerization step, the polymerization temperature was set to 65° C., the polymerization pressure was set to 0.35 MPa, 1-butene was introduced in a gas phase concentration of 0.35 mol % relative to ethylene, hydrogen was introduced in a gas phase concentration of 0.01 mol % relative to ethylene and 1-butene, solid catalyst component [B] was used instead of solid catalyst component [A], and ethanol was not introduced into the buffer tank. The polyethylene powder of Example 6 was obtained by the same operation as in Example 1. It should be noted that the catalyst activity was 10000 g-PE / g-solid catalyst component [B], and the slurry concentration was 25%.

[0272] [Example 7]

[0273] In the polymerization step, the polymerization temperature was set to 57° C., the polymerization pressure was set to 0.36 MPa, 1-butene and hydrogen were not introduced, and the solid catalyst component [B] was used instead of the solid catalyst component [A]. The polyethylene powder of Example 7 was obtained by the same operation as in Example 1. It should be noted that the catalyst activity was 8000 g-PE / g-solid catalyst component [B], and the slurry concentration was 20%.

[0274] [Comparative Example 1]

[0275] In the polymerization step, the polymerization temperature was set to 85° C., the polymerization pressure was set to 0.90 MPa, 1-butene was introduced in a manner of 3.7 mol% relative to ethylene, and hydrogen was introduced in a manner of 24.2 mol% relative to ethylene and 1-butene. The polyethylene powder of Comparative Example 1 was obtained by the same operation as in Example 1. It should be noted that the catalyst activity was 50,000 g-PE / g-solid catalyst component [A], and the slurry concentration was 27%.

[0276] [Comparative Example 2]

[0277] In the polymerization step, the polymerization temperature was set to 85° C., the polymerization pressure was set to 0.85 MPa, 1-butene was not introduced, and hydrogen was introduced in such a manner that the gas phase concentration relative to ethylene was 33.2 mol %, and the polyethylene powder of Comparative Example 2 was obtained by the same operation as Comparative Example 1. It should be noted that the catalyst activity was 51000 g-PE / g-solid catalyst component [A], and the slurry concentration was 26%.

[0278] [Comparative Example 3]

[0279] In the polymerization step, the polymerization temperature was set to 61° C., the polymerization pressure was set to 0.32 MPa, 1-butene was introduced in a gas phase concentration of 6.5 mol% relative to ethylene, hydrogen was not introduced, and the solid catalyst component [B] was used instead of the solid catalyst component [A]. The polyethylene powder of Comparative Example 3 was obtained by the same operation as in Example 1. It should be noted that the catalyst activity was 10000 g-PE / g-solid catalyst component [B], and the slurry concentration was 25%.

[0280] [Comparative Example 4]

[0281] A polyethylene powder of Comparative Example 4 was obtained by the same operation as in Example 1 except that 150 ppm of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] was added as an antioxidant.

[0282] [Comparative Example 5]

[0283] In the polymerization step, the polymerization temperature was set to 45° C., the polymerization pressure was set to 0.28 MPa, 1-butene was introduced in a gas phase concentration of 0.35 mol % relative to ethylene, hydrogen was introduced in a gas phase concentration of 0.23 mol % relative to ethylene and 1-butene, solid catalyst component [B] was used instead of solid catalyst component [A], solid catalyst component [B] was introduced at a rate of 0.3 g / hour, triisobutylaluminum was introduced at a rate of 15 mmol / hour, and ethanol was not introduced into the buffer tank, the polyethylene powder of Comparative Example 5 was obtained by the same operation as in Example 1. It should be noted that the catalyst activity was 4500 g-PE / g-solid catalyst component [B], and the slurry concentration was 35%.

[0284] [Comparative Example 6]

[0285] In the polymerization step, the solid catalyst component [B] and triisobutylaluminum as a co-catalyst were continuously added from separate introduction lines, and ethanol was not introduced into the buffer tank. The polyethylene powder of Comparative Example 6 was obtained by the same operation as in Example 6. The catalyst activity was 10000 g-PE / g-solid catalyst component [B], and the slurry concentration was 25%.

[0286] [Comparative Example 7]

[0287] In the polymerization step, the solid catalyst component [A] and triisobutylaluminum as a co-catalyst were continuously added from separate introduction lines, the temperature was adjusted only by jacket cooling without using a condenser, ethanol was not introduced into the buffer tank, only water was sprayed, and the temperature was adjusted by 3 m 3 A polyethylene powder of Comparative Example 7 was obtained by the same operation as in Example 3 except that nitrogen was blown at 1:1 / hour. The catalyst activity was 14500 g-PE / g-solid catalyst component [B], and the slurry concentration was 28%.

[0288]

[0289]

[0290] Industrial Applicability

[0291] The polyethylene powder of the present invention has excellent molecular weight stability even under processing conditions under more severe conditions, and a molded product containing the polyethylene powder is a molded product with excellent whiteness and cleanliness, and therefore has high industrial applicability as a material for various films, sheets, microporous films, fibers, foams, tubes, etc. requiring high purity.

Claims

1. A polyethylene powder, in, The intrinsic viscosity of the polyethylene powder is greater than or equal to 3.0 dl / g and less than 30.0 dl / g, and In the oxidation induction time measurement carried out according to ISO11357-6 (2018) at 150°C, oxygen and a sample mass of 5 mg, the heat flow of the polyethylene powder 60 minutes after switching to oxygen was greater than or equal to 0.03 mW and less than 0.25 mW.

2. The polyethylene powder according to claim 1, in, The intrinsic viscosity of the polyethylene powder is greater than or equal to 3.5 dl / g and less than 28.0 dl / g.

3. The polyethylene powder according to claim 1 or 2, in, The intrinsic viscosity of the polyethylene powder is greater than or equal to 4.0 dl / g and less than 26.0 dl / g.

4. The polyethylene powder according to claim 1 or 2, in, The heat flow of the polyethylene powder is greater than or equal to 0.04 mW and less than 0.24 mW.

5. The polyethylene powder according to claim 1 or 2, in, The heat flux of the polyethylene powder is greater than or equal to 0.05 mW and less than 0.23 mW.

6. The polyethylene powder according to claim 1 or 2, in, The content of Mg in the polyethylene powder is less than 10.0 ppm.

7. The polyethylene powder according to claim 6, in, The content of Mg in the polyethylene powder is less than 8.0 ppm.

8. The polyethylene powder according to claim 6, in, The content of Mg in the polyethylene powder is less than 6.0 ppm.

9. The polyethylene powder according to claim 1 or 2, in, The Ti content in the polyethylene powder is less than 3.0 ppm.

10. The polyethylene powder according to claim 9, in, The Ti content in the polyethylene powder is less than 2.5 ppm.

11. The polyethylene powder according to claim 9, in, The Ti content in the polyethylene powder is less than 2.0 ppm.

12. The polyethylene powder according to claim 1 or 2, in, The Al content in the polyethylene powder is less than 8.0 ppm.

13. The polyethylene powder according to claim 12, in, The content of Al in the polyethylene powder is less than 7.0 ppm.

14. The polyethylene powder according to claim 12, in, The Al content in the polyethylene powder is less than 6.0 ppm.

15. The polyethylene powder according to claim 1 or 2, in, The polyethylene constituting the polyethylene powder is an ethylene homopolymer or a copolymer of ethylene and other comonomers.

16. The polyethylene powder according to claim 15, in, The other comonomers are one or more selected from α-olefins and vinyl compounds.

17. The polyethylene powder according to claim 16, in, The α-olefin is an α-olefin having 3 to 20 carbon atoms.

18. The polyethylene powder according to claim 16 or 17, in, The α-olefin is one or more selected from propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, and 1-tetradecene.

19. The polyethylene powder according to claim 16, in, The vinyl compound is one or more selected from vinylcyclohexane, styrene and derivatives thereof.

20. The polyethylene powder according to claim 1 or 2, in, The content of α-olefin in the polyethylene powder is less than 0.10 mol %.

21. The polyethylene powder according to claim 20, in, The content of α-olefin in the polyethylene powder is 0.08 mol % or less.

22. The polyethylene powder according to claim 20, in, The content of α-olefin in the polyethylene powder is 0.06 mol % or less.

23. The polyethylene powder according to claim 1 or 2, in, The maximum weight increase rate of the polyethylene powder when heated at 200° C. in air for 1 hour is less than 2.0%.

24. The polyethylene powder according to claim 23, in, The maximum weight increase rate of the polyethylene powder is less than 1.9%.

25. The polyethylene powder according to claim 23, in, The maximum weight increase rate of the polyethylene powder is less than 1.8%.

26. The polyethylene powder according to claim 1 or 2, in, The total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm in the polyethylene powder is 50 mass % or more and less than 75 mass %.

27. The polyethylene powder according to claim 26, in, The total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm in the polyethylene powder is 52 mass % or more and less than 73 mass %.

28. The polyethylene powder according to claim 26, in, The total mass ratio of particles having a particle size of 106 μm or more and less than 212 μm in the polyethylene powder is 54 mass % or more and less than 71 mass %.

29. The polyethylene powder according to claim 1 or 2, in, The dense packing density of the polyethylene powder is greater than or equal to 0.50 g / cm 3 And less than 0.65g / cm 3 ,and The polyethylene powder has a value obtained by dividing the compact bulk density by the loose bulk density (compact bulk density / loose bulk density) of greater than or equal to 1.05 and less than 1.

30.

30. The polyethylene powder of claim 29, in, The dense packing density of the polyethylene powder is greater than or equal to 0.52 g / cm 3 And less than 0.63g / cm 3 .

31. The polyethylene powder of claim 29, in, The dense packing density of the polyethylene powder is greater than or equal to 0.54 g / cm 3 And less than 0.61g / cm 3 .

32. The polyethylene powder of claim 29, in, The polyethylene powder has a value obtained by dividing the close packing density by the loose packing density (close packing density / loose packing density) of 1.07 or more and 1.27 or less.

33. The polyethylene powder of claim 29, in, The polyethylene powder has a value obtained by dividing the close packing density by the loose packing density (close packing density / loose packing density) of 1.09 or more and 1.24 or less.

34. The polyethylene powder according to claim 1 or 2, in, The average particle size of the polyethylene powder is 500 μm or less.

35. The polyethylene powder of claim 34, in, The average particle size of the polyethylene powder is 400 μm or less.

36. The polyethylene powder of claim 34, in, The average particle size of the polyethylene powder is 300 μm or less.

37. The polyethylene powder according to claim 1 or 2, in, The content of Ca in the polyethylene powder is less than 10 ppm.

38. The polyethylene powder of claim 37, in, The content of Ca in the polyethylene powder is less than 8.0 ppm.

39. The polyethylene powder of claim 37, in, The content of Ca in the polyethylene powder is less than 6.0 ppm.

40. The polyethylene powder according to claim 1 or 2, in, The whiteness of a molded body obtained by using the polyethylene powder is greater than or equal to 90.

41. The polyethylene powder according to claim 1 or 2, in, The molecular weight reduction rate of the polyethylene powder during kneading calculated by the following formula is less than or equal to 15%, {[(intrinsic viscosity of polyethylene powder)-(intrinsic viscosity of stretched film obtained using polyethylene powder)] / (intrinsic viscosity of polyethylene powder)}×100(%).

42. A shaped body, in, The molded body is a molded body of the polyethylene powder according to any one of claims 1 to 41.

43. The shaped body according to claim 42, in, The shaped body is a microporous membrane, fiber, sheet, container or filter.

Citation Information

Patent Citations

  • PROCESS FOR THE PRODUCTION OF POLYOLEFINS AND THEIR COPOLYMERISATS

    DE3127133A1

  • Ultrahigh molecular weight polyethylene composition-made separator

    JP2017165938A

  • Ultra-high-molecular-weight polyethylene particle and molded body consisting of the same

    JP2018145412A

  • Polyethylene fiber

    JP2020016007A

  • Powder of ultrahigh-molecular-weight ethylene copolymer, and molded object obtained from powder of ultrahigh-molecular-weight ethylene copolymer

    CN107438631A