Packaging material and preparation method thereof, photovoltaic module

By using a high reflectivity substrate layer and a packaging material that selects a transmissive colored layer in photovoltaic modules, the problems of appearance and power attenuation of photovoltaic modules are solved, aesthetics and power improvement are achieved, and the service life is extended.

CN115418018BActive Publication Date: 2024-11-26FOSTER (JIAXING) NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211209634.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-26
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The existing photovoltaic module packaging materials have shortcomings in appearance adaptability and power attenuation, which are difficult to meet the dual requirements of aesthetic needs and extended service life.

Method used

The encapsulation material consisting of a substrate layer and a colored layer is adopted. The substrate layer has high reflectivity in each ultraviolet-visible-infrared band, and the colored layer has selective transmissibility in the ultraviolet-visible-infrared band, through reasonable reflectivity and thickness. Design to increase the power generation power of photovoltaic modules and extend the service life.

Benefits of technology

It realizes the aesthetics and power gain of photovoltaic modules, reduces the power attenuation speed, is suitable for optoelectronic building applications, and extends the service life of the modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115418018B_ABST
    Figure CN115418018B_ABST
Patent Text Reader

Abstract

The present invention provides a packaging material for packaging of photovoltaic modules, the packaging material includes a substrate layer and a colored layer at least arranged on the surface of one side of the substrate layer; the substrate layer meets the following conditions: the average reflectivity of any section of the substrate layer parallel to the surface of the substrate layer in the thickness direction in the wavelength range of 200nm-700nm is higher than 5%, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 30%, and the reflectivity of light at 1400nm is more than 50%; the packaging material meets the following conditions: the surface test of the packaging material on one side of the colored layer shows that the average reflectivity of the packaging material in the wavelength range of 200nm-700nm is higher than 4%, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 20%, and the reflectivity of light at 1400nm is more than 40%. The packaging material provided by the present invention, used for the packaging of photovoltaic modules, has the functional gain of extending weather resistance and reducing power attenuation of photovoltaic modules, and is applied to photovoltaic modules for photovoltaic buildings, and has good chromaticity matching and aesthetics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cell packaging, and in particular to a photovoltaic packaging material and a preparation method thereof, and a photovoltaic module. Background Art

[0002] With the continuous changes in energy structure, the development of new energy has become a global proposition. In terms of application scenarios, solar cells have a clear trend of both centralized and distributed applications, and the prospects for diversified application areas and smart photovoltaics are broad. Industrial and commercial roofs, residential roofs, curtain walls, color steel plate factory roofs and other locations have received more and more attention because they can be used for both power generation and partial building materials.

[0003] The biggest difference between photovoltaic modules used in buildings and conventional ground power stations is the different requirements for customized appearance. Traditional photovoltaic modules, especially crystalline silicon photovoltaic modules, are relatively simple black and white, which is far from the pursuit of diverse aesthetics in architecture. For example, photovoltaic modules made of white backplane materials are white between the cell gaps, the frame and the cell, and the entire module will present alternating tones of white and blue. This color tone is applied to the roof or curtain wall, and the overall appearance is less beautiful and the client is less accepting. Therefore, it is a difficult problem for the photovoltaic industry to meet both the module function and aesthetic requirements at the same time.

[0004] In addition, as the use of photovoltaic modules increases, the power of photovoltaic modules will gradually decay. In order to solve the problem of photovoltaic module power decay, in addition to improving the performance of the battery itself, it is also crucial to improve the packaging materials of photovoltaic modules. At present, the main solutions for improving the power decay of modules with packaging materials focus on improving the water vapor barrier and reducing the migration of free metal ions to reduce the PID effect (Potential Induced Degradation) of photovoltaic modules, thereby reducing the power decay of photovoltaic modules. The light reflectivity of each band of the packaging material is also crucial to the power decay of photovoltaic modules. Specifically, the absorption of light in the ultraviolet band will accelerate the aging of photovoltaic packaging materials, and the ultraviolet band light itself has little gain on the power of photovoltaic modules. As the photovoltaic packaging materials age, the power attenuation of photovoltaic modules will be further aggravated. The visible light band and near-infrared band are the main response bands of photovoltaic modules. In theory, the higher the reflectivity of the visible light band and near-infrared band, the greater the gain in the power generation of photovoltaic modules. However, as the reflectivity of light in the visible light band and near-infrared band increases, it will be difficult to meet the appearance performance of photovoltaic modules on the other hand, and it will also accelerate the aging of photovoltaic modules, resulting in increased power attenuation of photovoltaic modules, making it difficult to meet their service life. The reflectivity of infrared light exceeding the 1400nm band increases, and there is basically no gain in the power generation of photovoltaic modules, but the absorption of light in this infrared band will cause the aging of photovoltaic modules to accelerate, and also negatively affect the long-term power generation of photovoltaic modules. Therefore, controlling the reflectivity of light in each band of photovoltaic packaging materials within a reasonable range so that the packaging materials can not only increase the power generation power of the battery cells, but also reduce the aging of photovoltaic modules and extend the service life of photovoltaic modules is an effective solution to reduce the power attenuation rate of the modules.

[0005] Therefore, there is an urgent need for a new packaging material to solve the above problems. When used in photovoltaic modules, it is not only required to have excellent appearance and overall beauty, but also to generate power gain for the photovoltaic modules and reduce the power attenuation of the photovoltaic modules. Summary of the invention

[0006] The main purpose of the present invention is to provide a packaging material to solve the problems in the prior art that the packaging material used in photovoltaic modules has low appearance adaptability and serious power attenuation of the photovoltaic modules.

[0007] In order to achieve the above object, according to one aspect of the present invention, there is provided a packaging material for packaging a photovoltaic module, the packaging material comprising a substrate layer and a colored layer at least arranged on one side surface of the substrate layer;

[0008] The substrate layer satisfies the following conditions: the average reflectivity of any cross section of the substrate layer parallel to the surface of the substrate layer in the thickness direction is higher than 5% in the wavelength range of 200nm-700nm, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 30%, and the reflectivity of light at 1400nm is higher than 50%;

[0009] The packaging material meets the following conditions: the average reflectivity of the surface of one side of the colored layer of the packaging material in the wavelength range of 200nm-700nm is higher than 4%, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 20%, and the reflectivity of light at 1400nm is above 40%.

[0010] Furthermore, the glossiness of the surface of the colored layer away from the substrate layer is 25-85 GU.

[0011] Furthermore, the color layer has a thickness of 3-50 μm.

[0012] Furthermore, the thickness of the substrate layer is 12-300 μm.

[0013] Furthermore, the colored layer is obtained by coating a coating on the surface of the substrate layer and then drying it, and the coating contains a resin, a pigment, an additive and a solvent.

[0014] Furthermore, the mass ratio of the total mass of the resin and the additives to the mass of the pigment in the coating is no higher than 20:1.

[0015] Furthermore, the resin in the coating is selected from one or more of fluorocarbon resin, acrylic resin, alkyd resin, polyester resin, epoxy resin, phenolic resin, and terpene resin;

[0016] The auxiliary agent is selected from one or more of a curing agent, a stabilizing agent, a catalyst, and a diluent;

[0017] The pigment is selected from one or more of azo, phthalocyanine, aniline, naphthalene, phenanthroline, pyrrole, pyrazole, imidazole, oxazole, pyridine, pyridazine, pyrimidine, pyrazine, acridine, quinoline, purine, carbazole, oxazine, thiophene, indole, phenoxazine, porphyrin, and porphine colored pigments.

[0018] Furthermore, the substrate is selected from any one of polyethylene terephthalate film, polyethylene naphthalate film, polyolefin film, polycarbonate film, polyethylene-acrylate film, polyethylene-methacrylate film, polyester film, polyurethane film, styrene-methyl methacrylate copolymer film, methyl methacrylate-butadiene-styrene copolymer film, preferably any one of polyethylene terephthalate film, polyethylene naphthalate film, and polyolefin film.

[0019] A method for preparing a packaging material, wherein the packaging material is applied to a packaging backplane, resin, additives, pigments and solvents are uniformly mixed into a coating, which is then coated onto at least one side of a substrate layer using a coating process, and then dried at 60°C-200°C to obtain the packaging material.

[0020] A photovoltaic module comprises a packaging front plate, a front layer adhesive film, a battery layer, a back layer adhesive film and a packaging back plate, wherein the packaging back plate comprises the above-mentioned packaging material.

[0021] By applying the technical solution of the present invention, the encapsulation material of the present invention is completed by selecting the substrate layer of the encapsulation material, selecting the substrate layer with different reflectivity for the ultraviolet-visible-infrared band light, and matching the colored layer that selectively transmits the light of different bands. The encapsulation material provided by the present invention is used for the encapsulation of photovoltaic modules, has the functional gain of extending weather resistance and reducing the power attenuation of photovoltaic modules, and is especially used in photovoltaic modules for photovoltaic buildings, and also has good chromaticity matching and aesthetics. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0023] Figure 1 A structure of a packaging material is shown;

[0024] Figure 2 The structure of a photovoltaic module is shown.

[0025] The above drawings include the following reference numerals:

[0026] 1. Encapsulation backplane; 11. Colored layer; 12. Base material layer; 2. Back layer adhesive film; 3. Cell layer; 4. Front layer adhesive film; 5. Encapsulation front plate; A-A', cross section along the thickness direction of the base material layer. DETAILED DESCRIPTION

[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0028] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0029] A packaging material for packaging a photovoltaic module, the packaging material comprising a substrate layer and a colored layer at least arranged on one side of the substrate layer;

[0030] The substrate layer satisfies the following conditions: the average reflectivity of any cross section of the substrate layer parallel to the surface of the substrate layer in the thickness direction is higher than 5% in the wavelength range of 200nm-700nm, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 30%, and the reflectivity of light at 1400nm is higher than 50%;

[0031] The packaging material meets the following conditions: the average reflectivity of the surface of one side of the colored layer of the packaging material in the wavelength range of 200nm-700nm is higher than 4%, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 20%, and the reflectivity of light at 1400nm is above 40%.

[0032] Specifically, the present application provides a packaging material, which is used for packaging of photovoltaic modules, especially for packaging backplanes in photovoltaic modules, such as Figure 1 As shown, the packaging material includes a substrate layer and a colored layer, and the colored layer is at least arranged on the surface of one side of the substrate layer.

[0033] Photovoltaic modules include cells and packaging materials, wherein the cells are dark in color. In order to achieve a consistent overall appearance of the photovoltaic module and to make it aesthetically pleasing, the packaging materials, especially the back layer adhesive film and the packaging backboard, preferably use packaging materials with a dark appearance. In order to achieve a good gain effect of the packaging material in the photovoltaic module, the substrate layer of the packaging material needs to have a certain reflectivity in the infrared-visible-ultraviolet bands. For photovoltaic modules, the absorption of infrared band light in the module can easily cause the internal environment of the photovoltaic module to deteriorate, thereby affecting the power generation efficiency of the photovoltaic module. At the same time, the long-term high temperature inside the photovoltaic module will further aggravate the aging of the photovoltaic module, thereby reducing the power generation power of the photovoltaic module and increasing the power attenuation. Therefore, the packaging material is required to have a relatively high reflectivity in the infrared band. The reflectivity of the packaging material in the ultraviolet-visible light band is relatively low. In addition to the packaging material with a dark appearance, the photovoltaic module also includes transparent packaging materials. Different types of packaging materials are used in combination to realize photovoltaic module packaging. The reflectivity of the dark appearance packaging material in the ultraviolet-visible light band needs to be lower than that in the infrared band. The reflectivity in the visible light band is low, which can ensure that the appearance of the components is basically consistent, all dark in color, and more beautiful. The reflectivity of light in the ultraviolet band is low, which can reduce the aging rate and yellowing rate of other packaging materials in the photovoltaic module, thereby extending the service life of the photovoltaic module.

[0034] Therefore, the packaging material needs to select a substrate layer with an average reflectivity higher than 5% in the wavelength range of 200nm-700nm, an average reflectivity higher than 30% in the wavelength range of 1200nm-2500nm, and a reflectivity of more than 50% at 1400nm as the substrate of the packaging material. In the present application, the substrate layer provides support for the reflective performance of the packaging material. Selecting a substrate layer with an average reflectivity of higher than 4% in the wavelength range of 200nm-700nm as the substrate of the packaging material can provide a certain gain for the photovoltaic module and improve the light utilization rate of the photovoltaic module. The average reflectivity in the wavelength range of 1200nm-2500nm is higher than 30%. The substrate layer has a high reflectivity for light in the infrared band, which not only reflects more infrared band light to the battery cell to improve the power generation power of the battery cell, but also reduces the absorption of infrared band light in the packaging material, slows down the aging rate of the photovoltaic module, extends the service life of the photovoltaic module, and reduces the power attenuation of the photovoltaic module. Preferably, the reflectivity of the substrate layer for 1400nm light is more than 50%, and 1400nm is the end of the infrared range with better infrared response of the crystalline silicon cell, belonging to the near-infrared range. The light reflectivity here exceeds 50%, which can ensure that the infrared light maintains the power gain of the photovoltaic module.

[0035] It should be noted that the reflectivity of the substrate layer can be obtained by measuring the surface of any one side of the substrate layer, or by cutting the substrate layer in parallel to the two side surfaces along the thickness direction, such as Figure 1 The section shown by A-A' in the figure is used to test the reflectivity of each band of the section in the thickness direction of the substrate layer. Considering the stability of the substrate layer in use, it is preferred that the packaging film selects a substrate as the substrate layer whose average reflectivity in the wavelength range of 200nm-700nm is higher than 4%, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 30%, and the reflectivity of light at 1400nm is higher than 50%. In order to facilitate actual operation, the substrate layer is cut parallel to the surface of the substrate layer at half the thickness to measure the reflectivity of the section of the substrate layer.

[0036] The colored layer is a light-transmitting coating, which has a certain degree of selective permeability to light in the ultraviolet-visible-infrared bands. The packaging material is tested from the surface of the colored layer away from the substrate layer, and it is necessary to satisfy that the overall reflection of the packaging film for light in the ultraviolet-visible-infrared bands is lower than the reflectivity of the substrate layer. According to the actual use of photovoltaic modules, the colored layer can be a light-transmitting coating of various colors. Preferably, the colored layer is a dark light-transmitting coating, and the packaging material has a dark appearance. Specifically, the Lab value of the colored layer side of the packaging material is L: 10 ~ 55, a: -20 ~ 50, b: -40 ~ 50.

[0037] The packaging material satisfies that the surface of the colored layer away from the substrate layer has an average reflectivity higher than 4% in the wavelength range of 200nm-700nm, an average reflectivity higher than 20% in the wavelength range of 1200nm-2500nm, and a reflectivity of light at 1400nm of more than 50%.

[0038] It should be noted that the surface of the colored layer away from the substrate layer does not refer to the reflectivity test of the colored layer itself, but the reflectivity test of the packaging material as a whole. It can be seen that the structure of the packaging material with the substrate layer superimposed on the colored layer not only effectively ensures the effect of the substrate layer on light reflection and improving the power of the photovoltaic module, but also achieves a good appearance effect through the colored layer and reduces the problem of reducing the service life of the photovoltaic module caused by the secondary absorption of ultraviolet light in the module.

[0039] Compared with the existing technical solution of directly adding dark pigments and ultraviolet additives to the substrate layer, it can effectively solve the problem that too much additives are added to the substrate layer itself, resulting in mechanical performance degradation, cracking, powdering, embrittlement, etc., leading to the failure of the encapsulation effect. The encapsulation material is adapted to the photovoltaic module as a whole, more beautiful, and can be adjusted according to customer customization needs to match the style of household photovoltaic buildings.

[0040] Further preferably, the colored layer can be a dark layer or a light layer. When the colored layer is a light layer, the average reflectivity of the surface of the colored layer of the packaging material away from the substrate layer in the wavelength range of 200nm-700nm is less than 70%; when the colored layer is a dark layer, the average reflectivity of the surface of the colored layer of the packaging material away from the substrate layer in the wavelength range of 200nm-700nm is less than 10%.

[0041] Furthermore, the glossiness of the surface of the colored layer away from the substrate layer is 25-85 GU.

[0042] Specifically, there is a certain difference between the surface hardness of the colored layer and the surface hardness of the substrate layer. Compared with the technical solution of using a colored layer plus a substrate layer, due to the relatively low mechanical hardness of the surface of the colored layer, scratches, creases and other marks are very likely to appear on one side of the colored layer after the packaging material is rolled up and then unfolded. The defects in appearance are very likely to affect product sales. Therefore, in order to solve the problem of product appearance, it is necessary to control the glossiness of one side of the colored layer of the packaging material to be less than 85GU. When the surface glossiness of one side of the colored layer of the packaging material is less than 85GU, when scratches and creases appear on the surface of the colored layer, it does not affect the appearance of the packaging material. Preferably, the glossiness of the surface of one side of the colored layer of the packaging material is 25-85GU. At this time, the packaging material presents a certain matte effect, excellent appearance, and will not lose too much light, thereby increasing the power of the photovoltaic module.

[0043] Furthermore, the color layer has a thickness of 3-50 μm.

[0044] Specifically, from the perspective of light transmittance, the thickness of the colored layer is 3-50um. When the thickness of the colored layer is less than 3μm, its ultraviolet light transmittance will exceed 1%, and its ultraviolet barrier property is poor. In addition, the visible light transmittance will also increase, and the covering effect will be significantly reduced. When the thickness of the colored layer is greater than 50μm, the infrared light transmittance will decrease, which has a great impact on the utilization rate of infrared rays. At the same time, the colored layer absorbs more infrared band light, resulting in the deterioration of the internal environment of the photovoltaic module. It is difficult to dissipate heat quickly during the operation of the module, which further aggravates the power attenuation of the photovoltaic module.

[0045] From the perspective of manufacturing process, the thickness of the substrate layer is 12-300um. If the thickness of the substrate layer is less than 12μm, the processing technology is relatively high, the uniformity of mechanical properties is difficult to control, and the manufacturing cost is relatively high. If the thickness of the substrate layer is greater than 300μm, conventional double-drawing equipment is difficult to produce, the thickness uniformity is difficult to control, and the uniformity of mechanical properties is difficult to control.

[0046] Furthermore, the colored layer is obtained by coating a coating on the surface of the substrate layer and then drying it, the coating comprising resin, pigment, additives and solvent, and the ratio of the total mass of the resin and additives to the mass of the pigment in the coating is not higher than 20:1.

[0047] Specifically, the colored layer is obtained by coating the coating on one side of the substrate layer and then drying it. The colored layer is a composition comprising a mixture of resin, pigment, additive and solvent. The mass ratio of the resin: additive: pigment is preferably 10-19.5:0.5-5:1. If the pigment mass ratio is too low, the color coverage is poor, and the ultraviolet and visible light transmittance is high; if the pigment mass ratio is too high, the dispersion uniformity is poor, and the occurrence of agglomeration will reduce the transmittance in the infrared range. From the perspective of appearance and transmittance and reflectivity of each band, the ratio of the total mass of the resin and additives in the coating to the mass of the pigment is not higher than 20:1.

[0048] Furthermore, the resin in the coating is selected from one or more of fluorocarbon resin, acrylic resin, alkyd resin, polyester resin, epoxy resin, phenolic resin, and terpene resin;

[0049] The auxiliary agent is selected from one or more of a curing agent, a stabilizing agent, a catalyst, and a diluent;

[0050] The pigment is selected from one or more of azo, phthalocyanine, aniline, naphthalene, phenanthroline, pyrrole, pyrazole, imidazole, oxazole, pyridine, pyridazine, pyrimidine, pyrazine, acridine, quinoline, purine, carbazole, oxazine, thiophene, indole, phenoxazine, porphyrin, and porphine colored pigments.

[0051] Specifically, the pigment can be selected from benzimidazolone, copper phthalocyanine, aluminum phthalocyanine, zinc phthalocyanine, tetrafluoroisoindolinone, 3,4,9,10-tetracarboxamide diimide, quinacridone, 2,9-dimethyl-anthraquino[2,1,9-DEF:6,5,10-D'E'F']diisoquinoline-1,3,8,10(2H,9H)-tetraone, 5,12-dihydro-quinolino[2,3-B]acridine-7,14-dione, N-[4-(aminocarbonyl)phenyl]-4-[[1-[[(2,3-dihydro-2-oxygen)-1,3,8,10(2H,9H)-tetraone] [substituted-1H-benzimidazol-5-yl)-amino]carbonyl]-2-oxopropyl]azo]aniline, N,N-bis(4-methoxybenzyl)perylene-3,4,9,10-dicarboximide, 8,18-dichloro-5,15-diethyl-5,15-dihydrocarbazo[3',2':5,6][1,4]oxazine[2,3-b]indol[2,3-i]phenoxazine, 3,6-bis(4-chlorophenyl)-2,5-dihydro-pyrrolo[3,4-c]pyrrole-1,4-dione, etc.

[0052] Further, the curing agent is selected from one or more of hexamethylene diisocyanate trimer, hexamethylene diisocyanate prepolymer, isophorone diisocyanate trimer, isophorone diisocyanate prepolymer, hydrogenated xylylene isocyanate trimer, hydrogenated xylylene isocyanate prepolymer, toluene diisocyanate trimer, toluene diisocyanate prepolymer, methylated polymethylol melamine resin, butylated polymethylol melamine resin, mixed etherified polymethylol melamine resin, polyamide, polymethylene diamine, diethylene triamine, pentamethyl diethylene triamine, triethylene tetramine, diethylene triamine, triethylene tetramine, (2,3-dimethyl) dibutylene triamine;

[0053] The stabilizing agent is selected from one or more of acrylic block copolymers, silicon-containing copolymers, acidic group-containing copolymers, polyether siloxane copolymers, acrylate copolymers, calcium carbonate, silicon dioxide, and zinc oxide;

[0054] The catalyst is selected from one or more of pentamethyldiethylenetriamine, bis(dimethylaminoethyl)ether, stannous octoate, dioctyltin dilaurate, monobutyltin oxide, monobutyltin triisooctoate, dibutyltin dilaurate, acetic acid, p-toluenesulfonic acid, phthalic acid, lauric acid, and isooctanoic acid; the diluent is selected from one or more of alcohols, benzenes, esters, and ketones.

[0055] Furthermore, from the perspective of convenient coating, the coating has a viscosity of less than 20,000 cps at 25°C.

[0056] Furthermore, the average ultraviolet light transmittance of the colored layer in the range of 200nm-400nm is lower than 1.0%, the average visible light transmittance in the range of 400nm-750nm is lower than 50%, and the average infrared light transmittance in the range of 750nm-2500nm is higher than 50%.

[0057] Specifically, the colored layer has the effect of beautifying the appearance and selectively transmitting light of each wavelength band. The average value of the ultraviolet light transmittance of the colored layer in the range of 200nm-400nm is less than 1.0%, which is conducive to reducing the aging of other layers of the packaging material by ultraviolet rays, and specifically, it can reduce the ultraviolet aging of the substrate layer. The substrate layer mainly plays a supporting and blocking role. After ultraviolet aging, mechanical properties will decline, crack, powder, embrittlement and other phenomena will occur, resulting in the failure of the packaging function.

[0058] The average visible light transmittance of the colored layer in the range of 400nm-750nm is less than 50%. At this time, the colored layer appears dark in appearance. The packaging material formed after compounding with the substrate layer is adapted to the photovoltaic module as a whole, is more beautiful, and can be adjusted according to customer customization needs to match the household photovoltaic architectural style.

[0059] The average infrared light transmittance of the colored layer in the range of 750nm-2500nm is higher than 50%. At this time, the colored layer has a high transmittance for infrared light, which reduces the absorption of infrared light in the component and has a certain effect on reducing the power attenuation of the component. On the other hand, infrared rays that pass through the front glass, battery cells, etc. can pass through the colored layer to the substrate layer, and are reflected by the substrate layer to the back of the battery cell, thereby obtaining some power generation gain.

[0060] Furthermore, the substrate layer is selected from any one of polyethylene terephthalate film, polyethylene naphthalate film, polyolefin film, polycarbonate film, polyethylene-acrylate film, polyethylene-methacrylate film, polyester film, polyurethane film, styrene-methyl methacrylate copolymer film, methyl methacrylate-butadiene-styrene copolymer film, preferably any one of polyethylene terephthalate film, polyethylene naphthalate film, and polyolefin film.

[0061] Specifically, the substrate layer is preferably one of a polyethylene terephthalate film, a polyethylene naphthalate film, and a polyolefin film.

[0062] Furthermore, the packaging material is applied to a packaging backplane, and the colored layer is obtained by uniformly mixing resin, additives, and pigments, coating the mixture on a substrate layer using a coating process, and then drying the mixture at 60° C.-200° C. and rolling the mixture up.

[0063] A photovoltaic module, such as Figure 2As shown, the photovoltaic module includes a packaging front plate, a front layer of adhesive film, a battery layer, a back layer of adhesive film and a packaging back plate, and the packaging back plate is the packaging material.

[0064] Furthermore, the packaging material is applied to a packaging backplane, and the side of the packaging material substrate layer away from the colored layer may be a polyester film, a fluorine film, or other coatings.

[0065] The packaging material provided by the present invention has a good gain effect in photovoltaic modules. The base material layer of the packaging material needs to have a certain reflectivity in each of the infrared-visible-ultraviolet bands, and is matched with a colored layer. The reflectivity of the dark-appearance packaging material in the ultraviolet-visible light band needs to be lower than the reflectivity in the infrared band. The reflectivity in the visible light band is low, which can ensure that the appearance of the module is basically consistent, all dark in color, and more beautiful. The reflectivity of light in the ultraviolet band is low, which can reduce the aging speed and yellowing speed of other packaging materials in the photovoltaic module, thereby extending the service life of the photovoltaic module.

[0066] By matching the components in the colored layer system, the encapsulation material prepared can not only meet the color diversity needs of photovoltaic buildings, but also has excellent color stability and long-term weather resistance.

[0067] The beneficial effects of the present application are further illustrated below in combination with embodiments and comparative examples.

[0068] Preparation of coating composition: The colored layer is prepared by coating the coating on the surface of the substrate layer and then drying it. The components and addition amounts of the coating composition are shown in Table 1.

[0069] Table 1

[0070]

[0071] The specific components in Table 1 are as follows:

[0072] Resin:

[0073] A1: Fluorocarbon resin ETERFLON-4121 (Changxing Chemical)

[0074] A2: Acrylic resin BS966 (Jiangsu Sanmu Chemical Co., Ltd.)

[0075] A3: Acrylic resin ACR6458 (Gaoming Tongde Chemical Co., Ltd.)

[0076] A5: Acrylic resin AC3265 (Nengda Chemical Co., Ltd.)

[0077] A4: Epoxy resin SM716 (Jiangsu Sanmu Chemical Co., Ltd.)

[0078] A6: Polyester resin 220# (Toyobo)

[0079] pigment:

[0080] B1: N,N-bis(4-methoxybenzyl)perylene-3,4,9,10-dicarboximide (Xin Hongli Chemical Co., Ltd.)

[0081] B2: Copper Phthalocyanine G (Longsheng Dye Chemical Co., Ltd.)

[0082] B3: Tetracarboxylic acid diimide (Handafei Biotechnology Co., Ltd.)

[0083] B4: 3,6-bis(4-chlorophenyl)-2,5-dihydro-pyrrolo[3,4-c]pyrrole-1,4-dione (Handafei Biotechnology Co., Ltd.)

[0084] B5: N-[4-(Aminocarbonyl)phenyl]-4-[[1-[[(2,3-dihydro-2-oxo-1H-benzimidazol-5-yl)-amino]carbonyl]-2-oxopropyl]azo]aniline (Nona Technology Co., Ltd.)

[0085] B6: Zinc Phthalocyanine (Wonder Chemical Co., Ltd.)

[0086] Additives:

[0087] C1: Hexamethylene diisocyanate trimer TPA-90SB (Asahi Chemical, Japan)

[0088] C2: Butylated polymethylol melamine resin XT-1 (Moore Chemical Co., Ltd.)

[0089] C3: Acrylic block copolymer A 122 (Juncai Material Technology Co., Ltd.)

[0090] C4: Bis(dimethylaminoethyl)ether BDMAEE (Guangsiyuan Polyurethane Materials Co., Ltd.)

[0091] C5: Acidic group copolymer BYK110 (BYK, Germany)

[0092] C6: p-Toluenesulfonic acid (Yinglang Chemical Co., Ltd.)

[0093] C7: Silicon-containing copolymer NXH-308 (Xuanhao New Materials Co., Ltd.)

[0094] C8: Calcium carbonate (Jiangxi Bairui Calcium Carbonate Co., Ltd.)

[0095] C9: Silicon dioxide (Rui Chuangxin Materials Technology Co., Ltd.)

[0096] C10: Zinc oxide (Haishun New Materials Co., Ltd.)

[0097] C11: Stannous octoate (Hui An Chemical Co., Ltd.)

[0098] The preparation method of the packaging material is to apply the above coating to the substrate layer by a coating process, and then dry at 60°C-200°C and roll up to obtain packaging materials S1-14 and packaging materials T1-5. The thickness setting method of the substrate layer and the colored layer of packaging materials S1-14 and packaging materials T1-5 is shown in Table 2:

[0099] Table 2

[0100]

[0101] The substrate layer is a DS11 series PET substrate customized by Dongcai Technology Group Co., Ltd. The reflectivity of the substrate layer measured at a cross section at half of the thickness direction is shown in Table 3:

[0102] Table 3

[0103] 200-700nm 1200-2500nm 1400nm Reflectivity Reflectivity Reflectivity E1 5.6 45.7 63.1 E2 66.5 57.4 78.3 E3 4 46.9 66.5 E4 13.1 66.8 79.8 E5 5.1 30.4 53.6 E6 4.2 25.1 34.2

[0104] Test items and test methods

[0105] It should be noted that the above performance indicators are measured by the following methods:

[0106] 1. Transmittance and reflectivity

[0107] The test method refers to the spectrophotometer method with an integrating sphere in the standard GB / T 29848 "Ethylene-vinyl acetate copolymer (EVA) film for photovoltaic module encapsulation".

[0108] Testing instrument: UV-visible spectrophotometer.

[0109] Test conditions: 200nm~2500nm.

[0110] 2. Surface gloss

[0111] Test method: Use a gloss meter with a measuring angle of 60°, place it on the horizontal coating surface, and read the gloss.

[0112] 3. Appearance of packaging materials

[0113] Test method: Observe with naked eyes the number of obvious scratches on the surface of a 20cm*20cm packaging material sample.

[0114] ◎: The number of scratches is less than 3, and the appearance is excellent;

[0115] ○: The number of scratches is less than 10, and the appearance is good;

[0116] △: The number of scratches is more than 10, and the appearance is not good enough.

[0117] 4. Adhesion

[0118] The test method refers to the standard GB / T 31034 "Insulating backsheet for crystalline silicon solar cell modules";

[0119] Sample size: 200mm*200mm;

[0120] Test conditions: +25℃, 50%RH.

[0121] 5. Peel strength with packaging film

[0122] The test method refers to the standard GB / T2790 "Adhesive 180° Peel Strength Test Method Flexible Materials to Rigid Materials".

[0123] Sample size: 300mm*300mm.

[0124] Stretching speed: 100mm / min.

[0125] 6. Constant resistance to moisture and heat aging

[0126] The test method refers to the standard GBT31034-2014 "Insulating backsheet for crystalline silicon solar cell modules".

[0127] Test conditions: +85°C, relative humidity 85%, 3000 hours.

[0128] 7. UV resistance

[0129] The test method refers to the standard GBT31034-2014 "Insulating backsheet for crystalline silicon solar cell modules".

[0130] Test conditions: +60℃, 320-400nm, 200kwh / m2.

[0131] 8. Photovoltaic module power attenuation

[0132] The power test method refers to the standard IEC61215 "Terrestrial crystalline silicon photovoltaic modules - Design identification and finalization".

[0133] Sample size: bifacial cells, 72 modules.

[0134] Test conditions: AM 1.5, irradiance 1000W / m2, +25℃, 50%RH.

[0135] Power attenuation rate = (initial power - power after aging) / initial power * 100%.

[0136] The reflectivity, glossiness and corresponding appearance performance of the colored layer side surface of the packaging material S1-14 and the packaging material T1-5 in each band were tested, and the test results are shown in Table 4.

[0137] Table 4

[0138]

[0139] Table 5

[0140]

[0141]

[0142] Preparation of photovoltaic modules:

[0143] The encapsulation material S1-14 and the encapsulation material T1-5 are arranged and laminated in the following manner to prepare a photovoltaic module: the module adopts a 3.2mm photovoltaic glass / 0.45mm F406PS (Foster) / 182P-per half-cell / 0.45mm F806PS (Foster) / the encapsulation material laminated structure, and is prepared after lamination at 145°C for 18 minutes. The relevant properties of the photovoltaic module are shown in Table 6:

[0144] Table 6

[0145]

[0146]

[0147] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0148] It can be seen from Table 1-6 that the performance of packaging material S1-14 is basically better than that of packaging material T1-5. Specifically, it can be intuitively seen from the performance parameters between packaging material S1-7 and T4 and T5 that the coating formula of the colored layer has a significant impact on the performance of the final packaging material. The ratio of the sum of the resin and the additive to the pigment in packaging material T5 is greater than 20, the pigment content is relatively low and there are more fillers, resulting in a significant decrease in the reflectivity of each band of the coating composition coated with the colored layer, and an increase in the power attenuation of the photovoltaic module, which is worse than S1-7. Packaging material T5 is composed of only a single-layer substrate layer and lacks a colored layer. Although the reflectivity of each band is relatively high, it has a certain gain in the power generation of the photovoltaic module in the short term, but there are serious deficiencies in adhesion and peeling strength. At the same time, the power attenuation of the photovoltaic module is serious, and the power generation of the photovoltaic module will be seriously reduced under long-term use.

[0149] The performance parameters between packaging material S8-12 and packaging material T3 can be intuitively derived. As the thickness of the colored layer increases, the overall reflectivity of the packaging material shows a decreasing trend. The increase in the thickness of the colored layer will reduce the transmittance of the colored layer to light in each band. Therefore, as the thickness of the colored layer increases, the resistance to UV yellowing is significantly improved. The thickness of the colored layer in packaging material T3 reaches 70um. At this time, the peel strength and adhesion of the packaging material are significantly reduced. Considering that the thickness of the colored layer is too large, the inside of the colored layer is difficult to withstand the stress and starts to tear from the inside of the colored layer; the thickness of the colored layer of packaging material S12 is 1um, which is relatively high in production cost and difficult in process. In addition, if the thickness of the colored layer is too low, the adhesion between the colored layer and the substrate layer and the peel strength between the packaging material and the film will both decrease. Preferably, the thickness of the colored layer is 3-50um.

[0150] The performance parameters of packaging materials S13 and packaging materials T1-2 can be intuitively seen. Usually, the performance of packaging materials changes with the type and thickness of the substrate layer. Specifically, the thickness of the substrate layer of packaging material S13 reaches 300um. Although the reflectivity of infrared band light is excellent, the heat dissipation of PET itself is poor. As the thickness of the PET substrate layer increases, the internal working environment of the component is poor, and the power attenuation of the photovoltaic component increases. For packaging material S14, the reflectivity of each band of the substrate layer is low, and the reflectivity of each band of the final packaging material also decreases. It can be seen from packaging material T1-2 that when the reflectivity of the substrate layer itself is low, the packaging material is difficult to meet the use of photovoltaic components, especially when the reflectivity of the infrared band is lower than 30%, resulting in a small power generation during the use of the photovoltaic component. At the same time, it is difficult to effectively reflect light, resulting in an increase in the power attenuation of the photovoltaic component. At the same time, the reflectivity of the ultraviolet band is low, and the ultraviolet aging performance of the packaging material itself is also insufficient, making it difficult to guarantee the service life of the photovoltaic component.

[0151] It can be seen from packaging materials S3, S5, and S7 that the inorganic filler in the colored layer coating has a great influence on the glossiness of the colored layer. The colored layer needs to maintain a certain amount of inorganic filler. As the content of inorganic filler increases, the glossiness of the colored layer side of the packaging material decreases, that is, the better the appearance performance, the less likely it is to have obvious scratches and other defects.

[0152] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A packaging material for packaging photovoltaic modules. It is characterized in that The packaging material includes a substrate layer and a colored layer at least arranged on one side surface of the substrate layer; The substrate layer meets the following conditions: the average reflectivity of any cross section of the substrate layer parallel to the surface of the substrate layer in the thickness direction is higher than 5% in the wavelength range of 200nm-700nm, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 30%, and the reflectivity of light at 1400nm is higher than 50%; the thickness of the substrate layer is 12-300μm; The packaging material meets the following conditions: the average reflectivity of the surface of the colored layer of the packaging material in the wavelength range of 200nm-700nm is higher than 4%, the average reflectivity in the wavelength range of 1200nm-2500nm is higher than 20%, and the reflectivity of light at 1400nm is more than 40%; the average reflectivity of the surface of the colored layer of the packaging material away from the substrate layer in the wavelength range of 200nm-700nm is less than 10%; The colored layer meets the following conditions: the colored layer is obtained by coating a coating on the surface of a substrate layer and then drying the coating, the coating comprising resin, pigment, additive and solvent; the ratio of the total mass of the resin and additive to the mass of the pigment in the coating is not higher than 20:1; the thickness of the colored layer is 3-50 μm.

2. The packaging material according to claim 1, It is characterized in that The glossiness of the surface of the colored layer away from the substrate layer is 25-85 GU.

3. The packaging material according to claim 1, It is characterized in that The resin in the coating is selected from one or more of fluorocarbon resin, acrylic resin, alkyd resin, polyester resin, epoxy resin, phenolic resin and terpene resin; The auxiliary agent is selected from one or more of a curing agent, a stabilizing agent, a catalyst, and a diluent; The pigment is selected from one or more of azo, phthalocyanine, aniline, naphthalene, phenanthroline, pyrrole, pyrazole, imidazole, oxazole, pyridine, pyridazine, pyrimidine, pyrazine, acridine, quinoline, purine, carbazole, oxazine, thiophene, indole, phenoxazine, porphyrin, and porphine colored pigments.

4. The packaging material according to claim 1, It is characterized in that The substrate layer is selected from any one of polyethylene terephthalate film, polyethylene naphthalate film, polyolefin film, polycarbonate film, polyethylene-acrylate film, polyethylene-methacrylate film, polyester film, polyurethane film, styrene-methyl methacrylate copolymer film, and methyl methacrylate-butadiene-styrene copolymer film.

5. The packaging material according to claim 4, It is characterized in that The substrate layer is selected from any one of polyethylene terephthalate film, polyethylene naphthalate film and polyolefin film.

6. A method for preparing a packaging material, It is characterized in that The preparation method is used to manufacture the packaging material as described in any one of claims 1 to 5, wherein the resin, additives, pigments and solvents are evenly mixed into a coating, which is then coated on at least one side of the substrate layer using a coating process and dried at 60°C-200°C to obtain the packaging material.

7. A photovoltaic module, It is characterized in that The photovoltaic module comprises a packaging front plate, a front layer adhesive film, a battery layer, a back layer adhesive film and a packaging back plate, and the packaging back plate comprises the packaging material according to any one of claims 1-5.

Citation Information

Patent Citations

  • Polyolefin photovoltaic backsheet comprising a stabilized polypropylene layer

    CN106661289A

  • Locally highly reflective photovoltaic packaging adhesive film and applications thereof

    CN110776842A

  • Weather-resistant paint, weather-resistant coating, photovoltaic backboard and preparation method thereof

    CN111440528A

  • Power gain type black photovoltaic backboard

    CN114536906A