Inorganic structure and method for producing the same

By using magnesium oxide particles, amorphous silica particles and a metal element aqueous solution to pressurize and heat in the production of inorganic structures, an amorphous compound joint is formed, which solves the energy consumption and pores caused by high-temperature heating in the sintering method. problem, achieving high density and improved mechanical strength.

CN115515901BActive Publication Date: 2024-10-29PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180032789.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-11
Publication Date
2024-10-29
Estimated Expiration
2041-05-11

AI Technical Summary

Technical Problem

The sintering method requires high-temperature heating when manufacturing inorganic structures, resulting in high energy consumption and the presence of a large number of pores in the finished product and insufficient mechanical strength.

Method used

Magnesium oxide particles are mixed with amorphous silica particles and an aqueous solution containing metal elements other than silicon, and a pressure of 10 to 600 MPa and a heating of 50 to 300°C are performed to form an amorphous solution containing silicon, metal elements, and oxygen. The bonding part of the magnesium oxide compound realizes the three-dimensional bonding of magnesium oxide particles.

Benefits of technology

It achieves high density and improved mechanical strength of the inorganic structure, reduces manufacturing costs, and improves water resistance, acid resistance, alkali resistance and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115515901B_ABST
    Figure CN115515901B_ABST
Patent Text Reader

Abstract

An inorganic structure (1, 1A) comprising: a plurality of magnesium oxide particles (2); and a bonding portion (3) covering the surface of the magnesium oxide particles (2) and bonding the magnesium oxide particles (2) to each other. The bonding portion (3) contains an amorphous compound containing silicon, a metal element other than silicon, and oxygen, and substantially does not contain alkali metals, B, V, Te, P, Bi, Pb, and Zn. A method for producing an inorganic structure (1, 1A) comprising the following steps: a step of obtaining a mixture by mixing a plurality of magnesium oxide particles (11), a plurality of amorphous silicon dioxide particles (12), and an aqueous solution (13) containing a metal element other than silicon; and a step of pressurizing and heating the mixture under conditions of a pressure of 10 to 600 MPa and a temperature of 50 to 300°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an inorganic structure and a method for producing the same. Background Art

[0002] As a method for producing an inorganic structure made of ceramics, a sintering method has been conventionally known. The sintering method is a method of obtaining a sintered body by heating an aggregate of solid powder made of an inorganic substance at a temperature lower than the melting point.

[0003] Patent Document 1 discloses a method for producing a high-density magnesia sintered body. Specifically, Patent Document 1 discloses that a magnesium compound is thermally decomposed and pre-calcined, the magnesia obtained thereby is pressurized and formed, and the formed body is calcined to obtain a magnesia sintered body. In addition, Patent Document 1 discloses that the formed body is calcined at 1250°C to 1400°C for about 20 minutes.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 54-142212 Summary of the invention

[0007] However, the sintering method requires heating the solid powder at a high temperature, so the energy consumption during manufacturing is large, which has the problem of cost. In addition, if the solid powder is simply pressed at a low temperature, the solid powder will not be fully combined with each other, so there will be a large number of pores in the obtained molded body, and there is a problem that the mechanical strength becomes insufficient.

[0008] The present invention has been made in view of the problems of the prior art. In addition, an object of the present invention is to provide an inorganic structure that can be produced by a simple method and has high density, and a method for producing the inorganic structure.

[0009] In order to solve the above problems, the inorganic structure of the first embodiment of the present invention comprises: a plurality of magnesium oxide particles; and a bonding portion that covers the surface of the magnesium oxide particles and bonds the magnesium oxide particles together. The bonding portion contains an amorphous compound containing silicon, a metal element other than silicon, and oxygen, and substantially does not contain alkali metals, B, V, Te, P, Bi, Pb, and Zn.

[0010] The method for producing an inorganic structure according to the second embodiment of the present invention comprises the following steps: a step of obtaining a mixture by mixing a plurality of magnesium oxide particles, a plurality of amorphous silicon dioxide particles and an aqueous solution containing a metal element other than silicon; and a step of pressurizing and heating the mixture under the conditions of a pressure of 10 to 600 MPa and a temperature of 50 to 300° C. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a cross-sectional view schematically showing an example of the inorganic structure according to the present embodiment.

[0012] Figure 2 It is a cross-sectional view schematically showing another example of the inorganic structure according to the present embodiment.

[0013] Figure 3 It is a schematic cross-sectional view for explaining the method for producing the inorganic structure according to the present embodiment.

[0014] Figure 4 This is a graph showing the XRD pattern of magnesia registered in ICSD and the XRD pattern of Test Sample 1 of Example 1.

[0015] Figure 5 (a) is a scanning electron microscope image of the test sample 1 of Example 1 magnified 300 times. Figure 5 (b) is a scanning electron microscope image of the magnesia powder obtained at 300 times magnification.

[0016] Figure 6 (a) is a scanning electron microscope image of the test sample 1 of Example 1 magnified 500 times. Figure 6 (b) means Figure 6 (a) is a diagram of an energy dispersive X-ray analysis spectrum in the portion marked A. Figure 6 (c) means Figure 6 (a) is a diagram of an energy dispersive X-ray analysis spectrum in the portion marked with symbol B.

[0017] Figure 7 The diagram shows a scanning electron microscope image when energy dispersive X-ray analysis was performed on the test sample 1 of Example 1, and mapping data of silicon (Si) and magnesium (Mg). Figure 7 (a) is a scanning electron microscope image of the test sample 1 magnified 500 times. Figure 7 (b) is a graph showing mapping data of silicon, Figure 7 (c) is a graph showing mapping data of magnesium.

[0018] Figure 8 (a) is a scanning electron microscope image of the bonding portion in the test sample 1 magnified 3000 times. Figure 8 (b) Figure 8 The portion marked C in (a) is a scanning electron microscope image obtained by magnifying the portion 10,000 times.

[0019] Fig. 9(a) is a diagram showing a reflected electron image of position 1 in test sample 1 of Example 1. Fig. 9 (b) is a diagram showing a reflected electron image of position 2 in test sample 1. Fig. 9 (c) is a diagram showing a reflected electron image of position 3 in test sample 1.

[0020] Fig.10 (a) is a diagram showing data obtained by binarizing the reflected electron image of position 1 in test sample 1 of Example 1. Fig.10 (b) is a diagram showing data obtained by binarizing the reflected electron image at position 2 in test sample 1. Fig.10 (c) is a diagram showing data obtained by binarizing the reflected electron image at position 3 in test sample 1. DETAILED DESCRIPTION

[0021] Hereinafter, the inorganic structure and the method for producing the inorganic structure according to the present embodiment will be described in detail using the drawings. It should be noted that the dimensional ratios in the drawings are sometimes exaggerated for convenience of description and are different from the actual ratios.

[0022] [Inorganic structures]

[0023] like Figure 1 As shown, the inorganic structure 1 of the present embodiment includes a plurality of magnesium oxide particles 2. Adjacent magnesium oxide particles 2 are bonded to each other via bonding portions 3, thereby forming the inorganic structure 1 in which the magnesium oxide particles 2 are aggregated.

[0024] The magnesium oxide particles 2 contain magnesium oxide (magnesia, MgO) as a main component. That is, the magnesium oxide particles 2 preferably contain 50 mol % or more of magnesium oxide, more preferably 80 mol % or more of magnesium oxide, and particularly preferably 90 mol % or more of magnesium oxide.

[0025] The magnesium oxide particles 2 are preferably crystalline. When the magnesium oxide particles 2 are crystalline particles, an inorganic structure 1 having higher durability can be obtained compared to the case of amorphous particles. The magnesium oxide particles 2 may be single crystal particles or polycrystalline particles.

[0026] The average particle size of the magnesium oxide particles 2 constituting the inorganic structure 1 is not particularly limited. However, the average particle size of the magnesium oxide particles 2 is preferably 300 nm to 50 μm, more preferably 300 nm to 30 μm, and particularly preferably 300 nm to 20 μm. By having the average particle size of the magnesium oxide particles 2 within this range, the magnesium oxide particles 2 are firmly bonded to each other, and the strength of the inorganic structure 1 can be improved. In addition, by having the average particle size of the magnesium oxide particles 2 within this range, as described below, the proportion of pores present inside the inorganic structure 1 becomes 20% or less, thereby improving the strength of the inorganic structure 1. It should be noted that in this specification, as the value of "average particle size", unless otherwise specified, the following value is used: a value calculated as the average value of the particle size of particles observed in several to dozens of fields of view using an observation mechanism such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM).

[0027] The shape of the magnesium oxide particles 2 is not particularly limited, and can be set to be spherical, for example. In addition, the magnesium oxide particles 2 can be whisker-shaped (needle-shaped) particles or flaky particles. Compared with spherical particles, whisker-shaped particles or flaky particles have improved contact with other particles and contact with the bonding portion 3, thereby improving the overall strength of the inorganic structure 1.

[0028] The inorganic structure 1 of this embodiment includes a bonding portion 3 bonding a plurality of magnesium oxide particles 2. Adjacent magnesium oxide particles 2 are bonded via the bonding portion 3, whereby the magnesium oxide particles 2 are three-dimensionally bonded to each other, thereby obtaining a bulk body having high mechanical strength.

[0029] Moreover, the bonding portion 3 contains an amorphous compound containing at least silicon, a metal element other than silicon, and oxygen. As described below, the inorganic structure 1 can be obtained by heating and pressurizing a mixture of magnesium oxide particles, amorphous silicon dioxide particles, and an aqueous solution containing a metal element other than silicon. At this time, the silicon dioxide particles react with the aqueous solution to form an amorphous compound containing silicon, a metal element, and oxygen. Therefore, the bonding portion 3 contains an amorphous compound containing at least silicon, a metal element other than silicon, and oxygen.

[0030] Furthermore, the bonding portion 3 preferably contains an amorphous compound as a main component. Specifically, the bonding portion 3 preferably contains 50 mol % or more of the amorphous compound, more preferably 70 mol % or more, and further preferably 90 mol % or more.

[0031] The metal element other than silicon contained in the amorphous compound of the bonding portion 3 can be set to at least one selected from alkali metals, alkaline earth metals, transition metals, base metals and semimetals. It should be noted that in this specification, alkaline earth metals include not only calcium, strontium, barium and radium, but also beryllium and magnesium. Base metals include aluminum, zinc, gallium, cadmium, indium, tin, mercury, thallium, lead, bismuth and polonium. Semimetals include boron, silicon, germanium, arsenic, antimony and tellurium.

[0032] In the amorphous compound in the bonding portion 3, the metal element other than silicon is preferably magnesium. As described below, the inorganic structure 1 can be obtained by heating and pressurizing a mixture of magnesium oxide particles, amorphous silicon dioxide particles, and an aqueous solution containing magnesium. At this time, the silicon dioxide particles react with the aqueous solution containing magnesium to form an amorphous compound containing silicon, oxygen, and magnesium. Therefore, the bonding portion 3 preferably contains an amorphous compound containing silicon, oxygen, and magnesium.

[0033] In addition, the bonding portion 3 preferably does not substantially contain alkali metals, B, V, Te, P, Bi, Pb and Zn. In addition, the bonding portion 3 preferably does not substantially contain Ca, Sr and Ba. In the present specification, "the bonding portion does not substantially contain alkali metals, B, V, Te, P, Bi, Pb and Zn" means that alkali metals, B, V, Te, P, Bi, Pb and Zn are not intentionally contained in the bonding portion 3. Therefore, when alkali metals, B, V, Te, P, Bi, Pb and Zn are mixed into the bonding portion 3 in the form of unavoidable impurities, the condition of "the bonding portion does not substantially contain alkali metals, B, V, Te, P, Bi, Pb and Zn" is satisfied. Similarly, in the present specification, "the bonding portion does not substantially contain Ca, Sr and Ba" means that Ca, Sr and Ba are not intentionally contained in the bonding portion 3. Therefore, when Ca, Sr, and Ba are mixed in the bonding portion 3 as unavoidable impurities, the condition that “the bonding portion does not substantially contain Ca, Sr, and Ba” is satisfied.

[0034] The bonding portion 3 is preferably in direct contact with the magnesium oxide particles 2. In addition, the bonding portion 3 preferably covers at least a portion of the surface of the magnesium oxide particles 2, and more preferably covers the entire surface of the magnesium oxide particles 2. As a result, the magnesium oxide particles 2 and the bonding portion 3 are firmly bonded, so that an inorganic structure 1 having excellent density and mechanical strength can be obtained.

[0035] Among them, magnesium oxide is deliquescent and may be degraded by moisture, acid, and alkali in the air. However, in the inorganic structure 1, the magnesium oxide particles 2 are covered by the bonding portion 3, so the contact between the magnesium oxide particles 2 and moisture, acid, and alkali is suppressed. Therefore, the degradation of the magnesium oxide particles 2 can be suppressed, and the water resistance, acid resistance, and alkali resistance of the inorganic structure 1 can be improved.

[0036] like Figure 2 As shown, in the inorganic structure 1A, the linking part 3 may include fine particles 4 having an average particle size of 100 nm or less. When the linking part 3 includes a plurality of fine particles 4, the linking part 3 has a denser structure, thereby improving the strength of the inorganic structure 1A.

[0037] As described above, the binding portion 3 is formed by heating and pressurizing amorphous silica particles and an aqueous solution containing metal elements other than silicon to react. Therefore, particulate matter from silica particles may be contained inside the binding portion 3. In addition, as described below, the particle size of the amorphous silica particles is preferably less than 100 nm. Therefore, the binding portion 3 may contain microparticles 4 from silica particles and having an average particle size of less than 100 nm. In addition, the particle size of the microparticles 4 contained in the binding portion 3 can be measured using a scanning electron microscope or a transmission electron microscope.

[0038] The particles 4 contained in the binding portion 3 may be particles formed of an amorphous compound containing silicon, oxygen, and a metal element other than silicon. In addition, the particles 4 may be particles formed of a crystalline compound containing silicon, oxygen, and a metal element other than silicon. The particles 4 contained in the binding portion 3 may be particles formed of an amorphous compound containing silicon, oxygen, and magnesium. In addition, the particles 4 may be particles formed of a crystalline compound containing silicon, oxygen, and magnesium. In addition, the particles 4 may also contain silicon dioxide that does not react with an aqueous solution containing a metal element other than silicon.

[0039] In the inorganic structure 1, 1A, the volume ratio of the magnesium oxide particles 2 is preferably greater than the volume ratio of the bonding portion 3. In this case, the obtained inorganic structure 1, 1A becomes a structure that easily utilizes the characteristics of the magnesium oxide particles 2. Specifically, the thermal conductivity of the magnesium oxide particles 2 is as high as about 60 W / m·K, and is a material with excellent thermal conductivity. Therefore, by making the volume ratio of the magnesium oxide particles 2 greater than the volume ratio of the bonding portion 3, the thermal conductivity of the entire inorganic structure 1, 1A can be improved.

[0040] The bonding part 3 preferably further contains a crystalline silicon-magnesium composite oxide. As described above, the bonding part 3 contains an amorphous compound containing silicon and oxygen, and more preferably contains an amorphous compound containing silicon, oxygen and magnesium. Therefore, at least a part of the crystal structure of the bonding part 3 is amorphous. However, the bonding part 3 preferably contains not only an amorphous compound but also a crystalline silicon-magnesium composite oxide. By further containing a crystalline silicon-magnesium composite oxide in the bonding part 3, the chemical stability of the inorganic structure 1, 1A can be improved compared to the case where the bonding part 3 is formed only by an amorphous compound. In addition, the silicon-magnesium composite oxide is an oxide containing at least silicon and magnesium, and examples thereof include magnesium silicate.

[0041] As described above, in the inorganic structure 1, 1A, the binding portion 3 preferably contains an amorphous compound containing silicon, oxygen and magnesium. In addition, in the amorphous compound, the ratio of silicon to magnesium is not particularly limited. In addition, in the case where the binding portion 3 contains particles 4, the particles 4 can be particles formed of an amorphous compound containing silicon, oxygen and magnesium, or particles formed of a crystalline silicon-magnesium composite oxide. In addition, in the particles 4, silicon dioxide from silicon dioxide particles as a raw material can also be included. In addition, the binding portion 3 can also contain a silicon-magnesium composite oxide as a crystalline compound.

[0042] As described above, the bonding part 3 is formed by heating and pressurizing amorphous silicon dioxide particles and an aqueous solution containing a metal element other than silicon to react, and thus becomes a dense phase. However, pores may exist inside the bonding part 3 and in at least one portion between the bonding part 3 and the magnesium oxide particles 2.

[0043] Moreover, the porosity in the cross section of the inorganic structure 1, 1A is preferably 20% or less. That is, when observing the cross section of the inorganic structure 1, 1A, the average value of the pore ratio per unit area is preferably 20% or less. When the porosity is 20% or less, the ratio of the magnesium oxide particles 2 to be bonded to each other through the bonding portion 3 increases, so the inorganic structure 1, 1A becomes dense and the strength is improved. Therefore, the machinability of the inorganic structure 1, 1A can be further improved. In addition, when the porosity is 20% or less, cracks can be suppressed from occurring in the inorganic structure 1, 1A starting from the pores, so the bending strength of the inorganic structure 1, 1A can be improved. In addition, the porosity in the cross section of the inorganic structure 1, 1A is preferably 10% or less, more preferably 8% or less, and further preferably 5% or less. The smaller the porosity in the cross section of the inorganic structure 1, 1A, the more cracks starting from the pores can be suppressed, so the strength of the inorganic structure 1, 1A can be improved.

[0044] In this specification, porosity can be calculated as follows. First, observe the cross section of the inorganic structure 1, 1A, and distinguish the magnesium oxide particles 2, the bonding portion 3 and the pores. Then, the unit area and the area of ​​the pores in the unit area are measured, and the pore ratio per unit area is calculated, and this value is used as the porosity. In addition, it is more preferred that after the pore ratio per unit area is calculated for the cross section of the inorganic structure 1, 1A at multiple locations, the average value of the pore ratio per unit area is used as the porosity. When observing the cross section of the inorganic structure 1, 1A, an optical microscope, a scanning electron microscope (SEM) or a transmission electron microscope (TEM) can be used. In addition, the unit area and the area of ​​the pores in the unit area can be measured by binarizing the image observed with a microscope.

[0045] The size of the pores present in the inorganic structure 1, 1A is not particularly limited, and is preferably as small as possible. By making the size of the pores small, cracks starting from the pores can be suppressed, thereby improving the strength of the inorganic structure 1, 1A and improving the machinability of the inorganic structure 1, 1A. In addition, the size of the pores of the inorganic structure 1, 1A is preferably less than 5 μm, more preferably less than 1 μm, and further preferably less than 100 nm. The size of the pores present in the inorganic structure 1, 1A can be obtained by observing the cross section of the inorganic structure 1, 1A using a microscope in the same manner as the above-mentioned porosity.

[0046] The inorganic structure 1, 1A only needs to have a structure in which the magnesium oxide particles 2 are mutually bonded via the bonding portion 3. Therefore, as long as the inorganic structure 1, 1A has such a structure, its shape is not limited. The shape of the inorganic structure 1, 1A can be set to, for example, a plate-like, film-like, rectangular, block-like, rod-like, or spherical shape. In addition, when the inorganic structure 1, 1A is plate-like or film-like, its thickness t is not particularly limited, for example, it can be set to more than 50μm. As described below, the inorganic structure 1, 1A of this embodiment is formed by a pressurized heating method. Therefore, it is easy to obtain an inorganic structure 1, 1A with a large thickness. In addition, the thickness t of the inorganic structure 1, 1A can be set to more than 500μm, can be set to more than 1mm, and can also be set to more than 1cm. The upper limit of the thickness t of the inorganic structure 1, 1A is not particularly limited, for example, it can be set to 50cm.

[0047] In the inorganic structure 1, 1A, the plurality of magnesium oxide particles 2 are mutually bonded via the bonding portion 3, and therefore are not bonded via an organic binder formed of an organic compound, and further, are not bonded via an inorganic binder other than the bonding portion 3. Therefore, the inorganic structure 1, 1A is a structure that retains the properties of the magnesium oxide particles 2 and the bonding portion 3. For example, the magnesium oxide particles 2 have high thermal conductivity, and therefore the obtained inorganic structure 1, 1A is also a structure having excellent thermal conductivity.

[0048] In this way, the inorganic structure 1, 1A of the present embodiment includes: a plurality of magnesium oxide particles 2; and a bonding portion 3 that covers the surface of the magnesium oxide particles 2 and bonds the magnesium oxide particles 2. The bonding portion 3 contains an amorphous compound containing silicon, metal elements other than silicon, and oxygen. In addition, the bonding portion 3 does not substantially contain alkali metals, B, V, Te, P, Bi, Pb, and Zn. In the inorganic structure 1, 1A, a plurality of magnesium oxide particles 2 are bonded via the bonding portion 3 with high density. Therefore, an inorganic structure 1, 1A with excellent density and mechanical strength can be obtained. In addition, since the bonding portion 3 covers the surface of the magnesium oxide particles 2, it is possible to suppress the deliquescence of the magnesium oxide particles 2 and improve the chemical stability of the inorganic structure 1, 1A.

[0049] In addition, the thermal conductivity of magnesium oxide is about 60 W / m·K, which is high among ceramic materials. Therefore, by using magnesium oxide particles 2 and setting the bonding portion 3 to an amorphous compound containing silicon, oxygen and magnesium, an inorganic structure 1, 1A having not only excellent mechanical strength but also excellent thermal conductivity is obtained. In addition, the thermal conductivity of the inorganic structure 1, 1A is preferably greater than 2 W / m·K, and more preferably greater than 5 W / m·K. The upper limit of the thermal conductivity of the inorganic structure 1, 1A is not particularly limited, and can be set to 60 W / m·K, for example. In addition, the thermal conductivity can be measured in accordance with Japanese Industrial Standard JIS R1611 (Determination method of thermal diffusivity / specific heat capacity / thermal conductivity of fine ceramics based on the flash method).

[0050] like Figure 1 and Figure 2 As shown, the inorganic structure 1, 1A of the present embodiment can be set as a structure in which only the magnesium oxide particles 2 are bonded via the bonding portion 3. However, as described below, the inorganic structure 1, 1A can be obtained by heating to 50 to 300°C while applying pressure, so a component with low heat resistance can be added to the inorganic structure 1, 1A. Specifically, the inorganic structure 1, 1A may include organic matter and resin particles in addition to the magnesium oxide particles 2 and the bonding portion 3. In addition, it is not limited to components with low heat resistance such as organic matter, and the inorganic structure 1, 1A may also include particles formed of inorganic compounds in addition to the magnesium oxide particles 2 and the bonding portion 3.

[0051] [Method for producing inorganic structure]

[0052] Next, a method for producing the inorganic structure 1 or 1A will be described. The inorganic structure can be produced by mixing a plurality of magnesium oxide particles, a plurality of amorphous silicon dioxide particles, and an aqueous solution to obtain a mixture, and pressurizing and heating the mixture.

[0053] Specifically, first, a mixture is prepared by mixing magnesium oxide particle powder, silicon dioxide particles and an aqueous solution. The magnesium oxide particles preferably contain 50 mol % or more of magnesium oxide, more preferably 80 mol % or more of magnesium oxide, and particularly preferably 90 mol % or more of magnesium oxide.

[0054] Silica particles are particles formed of amorphous silicon dioxide. Moreover, the silica particles are preferably smoke-like particles, i.e., fumed silica. Fumed silica is amorphous silica particles with a primary particle size of about 5nm to 50nm. The fumed silica is a particle produced by combustion and hydrolysis of silicon tetrachloride, and the primary particles are condensed and agglomerated to form large secondary particles. Therefore, fumed silica has high reactivity with aqueous solutions and can easily form an amorphous compound containing silicon and oxygen.

[0055] As the aqueous solution, an aqueous solution containing a metal element other than silicon is used. In addition, the aqueous solution containing a metal element other than silicon is an aqueous solution containing the metal element in the form of ions. The metal element other than silicon can be set to at least one selected from alkali metals, alkaline earth metals, transition metals, base metals and semimetals. In addition, the solvent for dissolving the metal element is preferably pure water or ion exchange water. However, the solvent may contain an acidic substance or an alkaline substance in addition to water, and may also contain an organic solvent (such as alcohol, etc.). In addition, hereinafter, "an aqueous solution containing a metal element other than silicon" is also referred to as "aqueous solution containing metal elements".

[0056] In addition, as the aqueous solution, an aqueous solution containing magnesium is preferably used. In addition, the aqueous solution containing magnesium is an aqueous solution containing magnesium in the form of ions, for example, a magnesium acetate aqueous solution can be used. In addition, hereinafter, "aqueous solution containing magnesium" is also referred to as "magnesium-containing aqueous solution".

[0057] Then, if Figure 3 As shown, a mixture of magnesium oxide particles 11, silicon dioxide particles 12 and a metal element-containing aqueous solution 13 is filled into the interior of a mold 14. After the mixture is filled into the mold 14, the mold 14 is heated as needed. Then, by applying pressure to the mixture inside the mold 14, the interior of the mold 14 becomes a high-pressure state. At this time, the silicon dioxide particles 12 are amorphous and highly reactive, so the silicon dioxide particles 12 react with the metal element-containing aqueous solution 13 to form a bonding portion 3 containing silicon, oxygen and a metal element other than silicon.

[0058] Here, when fumed silica is used as the silica particles 12, the fumed silica has a particle size of nanometers and is therefore filled without gaps between the magnesium oxide particles 11. Therefore, the resulting bonding portion 3 has a dense structure and can strongly bond the magnesium oxide particles 11 to each other.

[0059] In addition, when a magnesium-containing aqueous solution is used as the aqueous solution, since both the magnesium oxide particles 11 and the magnesium-containing aqueous solution contain magnesium, magnesium can easily diffuse into each other. Figure 3As shown, the compound 15 containing silicon, oxygen and magnesium, such as silicon-magnesium composite oxide, is easily formed on the surface of the magnesium oxide particle 11. Therefore, the obtained bonding part 3 covers the magnesium oxide particle 11 and firmly bonds it, so that the mechanical strength of the inorganic structure 1, 1A can be improved.

[0060] Then, the compact is taken out from the inside of the mold, thereby obtaining the inorganic structure 1 , 1A in which the plurality of magnesium oxide particles 2 are bonded to each other via the bonding portion 3 .

[0061] In addition, the heating and pressurizing conditions of the mixture formed by mixing the magnesium oxide particles 11, the silica particles 12 and the metal element-containing aqueous solution 13 are not particularly limited as long as the reaction between the silica particles 12 and the metal element-containing aqueous solution 13 is carried out. For example, it is preferred that the above-mentioned mixture is pressurized at a pressure of 10 to 600 MPa while being heated to 50 to 300° C. In addition, the temperature when the above-mentioned mixture is heated is more preferably 80 to 250° C., and further preferably 100 to 200° C. In addition, the pressure when the above-mentioned mixture is pressurized is more preferably 50 to 600 MPa, and further preferably 200 to 600 MPa.

[0062] The amorphous silicon dioxide particles 12 may be completely reacted with the metal element-containing aqueous solution 13 to form a compound containing silicon, oxygen and magnesium by the above-mentioned heating and pressing process. Alternatively, the silicon dioxide particles 12 may not completely react with the metal element-containing aqueous solution 13, but may remain in the bonding portion 3 in the form of silicon dioxide.

[0063] In addition, since the bonding part 3 is formed by the reaction of the silica particles 12 and the metal element-containing aqueous solution 13, the bonding part 3 may also include fine particles 4 derived from the silica particles and having an average particle size of 100 nm or less. In addition, the fine particles 4 may also include silica that has not reacted with the metal element-containing aqueous solution 13.

[0064] As described above, the inorganic structure 1, 1A can be obtained by pressing and heating a mixture of magnesium oxide particles 11, silicon dioxide particles 12 and a metal element-containing aqueous solution 13 at 10 to 600 MPa and 50 to 300°C. Then, by such a heating and pressing process, a bonding portion 3 containing an amorphous compound can be formed. However, by extending the heating and pressing time of the above-mentioned mixture, a part of the amorphous compound is crystallized. Therefore, for example, in the case where a crystalline silicon-magnesium composite oxide is further included in the bonding portion 3, it is preferred to extend the heating and pressing time of the mixture of magnesium oxide particles, silicon dioxide particles and the magnesium-containing aqueous solution.

[0065] In the manufacturing method of this embodiment, as amorphous silicon dioxide particles, smoky particles, i.e., fumed silicon dioxide, are preferably used. However, as smoky particles, aluminum oxide (Al2O3) and titanium dioxide (TiO2) also exist. Therefore, in the mixture formed by mixing magnesium oxide particles 11, silicon dioxide particles 12 and the aqueous solution containing metal elements 13, at least one of fumed aluminum oxide and fumed titanium dioxide may be further mixed. Thus, fumed aluminum oxide and / or fumed titanium dioxide react with the aqueous solution containing metal elements 13, so that the reaction product can be contained in the bonding portion 3.

[0066] Among them, as a method for forming an agglomerate of magnesium oxide particles, there is a method of simply pressing the powder of magnesium oxide particles. However, even if the powder of magnesium oxide particles is put into a mold and pressed at room temperature, it is difficult for the particles of magnesium oxide particles to react with each other, and it is difficult to make the particles firmly bonded to each other. Therefore, there are a large number of pores in the obtained powder compact, and the mechanical strength becomes insufficient.

[0067] In addition, as a method for forming an agglomerate of magnesium oxide particles, there is also a method of only pressing the powder of magnesium oxide particles to form a pressed powder body, and then firing it at a high temperature (for example, above 1700°C). When the pressed powder body of magnesium oxide particles is fired at a high temperature, the magnesium oxide particles sinter with each other to form a structure. However, even if the pressed powder body of magnesium oxide particles is fired at a high temperature, the magnesium oxide particles are difficult to sinter with each other, so there are a large number of pores in the obtained structure, and the mechanical strength becomes insufficient. In addition, when the magnesium oxide particles are fired at a high temperature, the manufacturing cost increases because careful temperature control is required.

[0068] In contrast, in the manufacturing method of the present embodiment, a mixture of magnesium oxide particles 11, amorphous silicon dioxide particles 12, and a metal element-containing aqueous solution 13 is heated and pressurized, so that a dense structure with excellent strength can be obtained. In addition, the manufacturing method of the present embodiment can be obtained by heating at 50 to 300° C. and pressurizing, so that careful temperature control is not required, and the manufacturing cost can be reduced.

[0069] Thus, the method for manufacturing the inorganic structure 1, 1A of the present embodiment includes the following steps: a step of obtaining a mixture by mixing a plurality of magnesium oxide particles 11, a plurality of amorphous silicon dioxide particles 12, and an aqueous solution 13 containing a metal element other than silicon. The manufacturing method also includes the following steps: a step of pressurizing and heating the mixture under the conditions of a pressure of 10 to 600 MPa and a temperature of 50 to 300° C. Therefore, the manufacturing method of the present embodiment can produce a highly dense inorganic structure by a simple method.

[0070] [Members with inorganic structures]

[0071] Next, the component having the inorganic structure 1 is described. As described above, the inorganic structure 1 can be made into a plate-like shape with a large thickness, and because it is dense, it is also excellent in stability. In addition, the inorganic structure 1 has a high mechanical strength, can be cut in the same way as a general ceramic component, and can also be surface processed. Therefore, the inorganic structure 1 can be preferably used as a building component. As a building component, there is no particular limitation, for example, outer wall materials (wall panels), roof materials, etc. can be listed. In addition, as a building component, road materials and outer trough materials can also be listed.

[0072] The inorganic structure 1 can also be preferably used as a member for electronic devices. Examples of the member for electronic devices include structural materials, heat-resistant members, insulating members, heat-dissipating members, sealing materials, circuit boards, and optical members.

[0073] Example

[0074] Hereinafter, the present embodiment will be described in more detail with reference to Examples, but the present embodiment is not limited to these Examples.

[0075] [Preparation of test samples]

[0076] First, magnesia powder (MgO, manufactured by Ube Material Industries, Ltd.) and amorphous silica powder (fumed silica, AEROSIL manufactured by Nippon Aerosil Co., Ltd.) were prepared. Then, acetone was added to the magnesia powder and the silica powder in the proportions shown in Table 1 and mixed using an agate mortar and an agate pestle, thereby obtaining a mixed powder of each example. In addition, in the mixed powder of Example 1, the volume ratio (volume %) of magnesia powder (MgO) to silica powder (SiO2) was 62:38 (MgO:SiO2).

[0077] Separately, a magnesium acetate aqueous solution was obtained by dissolving 4 g of magnesium acetate tetrahydrate powder (Mg(CH3COO)2·4H2O, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) in 6 ml of ion-exchanged water.

[0078] [Table 1]

[0079] Magnesia Silicon dioxide Magnesium acetate aqueous solution Example 1 0.2g 0.0747g 160μl Example 2 0.2g 0.02241g 96μl Example 3 0.2g 0.0075g 96μl

[0080] Next, the mixed powder of each example was put into a cylindrical forming mold (φ10) having an internal space. Furthermore, an aqueous solution of magnesium acetate in an amount shown in Table 1 was added to the inside of the forming mold and mixed with a plastic spatula. In addition, in the mixed powder containing the aqueous solution of magnesium acetate of Example 1, SiO2 was 250 mol% relative to Mg(CH3COO)2.

[0081] Then, the mixed powder including the magnesium acetate aqueous solution was heated and pressurized at 150° C. and 400 MPa for 30 minutes to obtain cylindrical test sample 1 of Example 1, test sample 2 of Example 2, and test sample 3 of Example 3, respectively.

[0082] [Evaluation of test samples]

[0083] (Crystal structure analysis)

[0084] The XRD pattern of the powder obtained by pulverizing the test sample 1 was measured using a powder X-ray diffraction (XRD) apparatus. Figure 4 , the XRD pattern of magnesia registered in ICSD and the XRD pattern of test sample 1 of Example 1 are shown.

[0085] like Figure 4 As shown, it can be seen that the XRD pattern of the test sample 1 of Example 1 has a peak at the same position as the magnesia registered in the ICSD, and the magnesia is the main phase. In addition, since no other obvious peaks are confirmed, it can be seen that the crystal structure of the silicon-magnesium composite oxide generated by the reaction of the silicon dioxide powder and the magnesium acetate aqueous solution is amorphous. In other words, it can be seen that the crystal structure of the silicon-magnesium composite oxide constituting the bonding portion 3 is amorphous.

[0086] (Structural Observation)

[0087] The cross section of the cylindrical test sample 1 prepared in Example 1 was observed using a scanning electron microscope (SEM). In addition, gold was sputtered on the observed surface of the test sample 1. Figure 5 (a) shows a SEM image of the test sample 1 magnified 300 times. Figure 5 (b) shows a SEM image of magnesia powder magnified 300 times.

[0088] In addition, the cross section obtained by cutting the cylindrical test sample 1 prepared in Example 1 was observed using an energy dispersive X-ray analyzer (EDX). Figure 6 (a) shows a SEM image of the test sample 1 magnified 500 times. Figure 6 (b) shows Figure 6The EDX spectrum in the symbol A in (a) is Figure 6 (c) shows Figure 6 EDX spectrum in the portion marked B in (a).

[0089] in addition, Figure 7 The SEM image when the energy dispersive X-ray analysis was performed on the test sample 1 of Example 1, and the mapping data of silicon (Si) and magnesium (Mg) are shown. Figure 7 (a) shows a SEM image of the test sample 1 magnified 500 times, Figure 7 (b) shows the mapping data of silicon, Figure 7 (c) shows the mapping data for magnesium.

[0090] according to Figure 5 (a) and Figure 6 The SEM image shown in (a) shows that in the test sample 1 of Example 1, the magnesia powder (magnesium oxide particles 2) are bonded to each other via the bonding portion 3. In addition, a dense structure can be confirmed in the test sample 1. Figure 6 (b) EDX spectrum and Figure 7 (b) and Figure 7 From the mapping data of (c), it can be seen that the portion with symbol A contains Mg and O, so it is the raw material magnesia. Figure 6 (c) EDX spectrum and Figure 7 (b) and Figure 7 The mapping data of (c) show that the portion indicated by symbol B contains Mg, Si and O, and is therefore a silicon-magnesium composite oxide generated by the reaction between the raw material silicon dioxide and the magnesium acetate aqueous solution.

[0091] exist Figure 8 (a) shows a SEM image of the bonding portion 3 in the test sample 1 magnified 3000 times. Figure 8 (b) shows the Figure 8 (a) is a SEM image of the portion marked C magnified 10,000 times. Figure 8 (a) It can be seen that the smoothness of the joint 3 in the test sample 1 is high and a dense phase is formed. Figure 8 As shown by symbol D in (b), it can be confirmed that fine particles 4 having a particle size of 100 nm or less are contained inside the bonding portion 3 .

[0092] (Porosity measurement)

[0093] First, a cross-section polishing process (CP process) was performed on the cross section of the cylindrical test sample 1 of Example 1. Next, a reflected electron image of the cross section of the test sample 1 was observed at a magnification of 50,000 times using a scanning electron microscope (SEM). The reflected electron images obtained by observing three locations (positions 1 to 3) of the cross section of the test sample 1 are shown in FIG. Fig. 9 (a) Fig. 9 (b) Fig. 9 (c) In the observed reflected electron image, the white portion 22 is magnesia, the gray portion 23 is the silicon-containing compound, and the black portion 25 is the pores.

[0094] Next, the SEM images of the three viewing fields were binarized to make the pores clear. Fig. 9 (a) Fig. 9 (b) Fig. 9 The images obtained by binarizing the reflected electron image of (c) are shown in Fig.10 (a) Fig.10 (b) Fig.10 (c) Then, the area ratio of the pores is calculated based on the binarized image, and the average value is taken as the porosity. Fig.10 (a) It can be seen that the area ratio of the pore portion at position 1 is 3.2%. Fig.10 (b) It can be seen that the area ratio of the pore portion at position 2 is 4.6%. Fig.10 (c) It can be seen that the area ratio of the pore portion at position 3 is 3.3%. Therefore, the porosity of the test sample 1 of Example 1 produced this time is the average of the area ratios of the pore portions at positions 1 to 3, that is, 3.7%.

[0095] (Thermal conductivity determination)

[0096] The thermal conductivity of the test sample 1 of Example 1, the test sample 2 of Example 2, and the test sample 3 of Example 3 was measured in accordance with JIS R1611. The thermal conductivity of each test sample is shown in Table 2. As shown in Table 2, the test samples 1, 2, and 3 of this example showed high thermal conductivity of 2.0 W / m·K or more, and the test sample 3 of Example 3 showed a particularly high thermal conductivity of 5.5 W / m·K. Therefore, it can be seen from Tables 1 and 2 that the thermal conductivity of the inorganic structure can be improved by increasing the proportion of magnesia.

[0097] [Table 2]

[0098] Thermal conductivity Example 1 2.0W / m·K Example 2 4.4W / m·K Example 3 5.5W / m·K

[0099] As mentioned above, although this embodiment was demonstrated, this embodiment is not limited to these, Various deformation|transformation is possible within the scope of the summary of this embodiment.

[0100] The entire contents of Tokugan 2020-092468 (filing date: May 27, 2020) are incorporated herein by reference.

[0101] Industrial Applicability

[0102] According to the present disclosure, an inorganic structure that can be produced by a simple method and has high density, and a method for producing the inorganic structure can be provided.

[0103] Explanation of symbols

[0104] 1.1A Inorganic structure

[0105] 2 Magnesium oxide particles

[0106] 3 Joint

[0107] 4 Particles

[0108] 11. Magnesium oxide particles

[0109] 12 Silica particles

[0110] 13 Aqueous solutions containing metal elements other than silicon

Claims

1. An inorganic structure comprising: a plurality of magnesium oxide particles; and a bonding portion that covers the surface of the magnesium oxide particles and bonds the magnesium oxide particles together, The bonding portion contains an amorphous compound including silicon, a metal element other than silicon, and oxygen, and substantially does not contain alkali metals, B, V, Te, P, Bi, Pb, and Zn. The bonding portion includes fine particles having an average particle diameter of 100 nm or less and containing silicon and oxygen.

2. The inorganic structure according to claim 1, in, The bonding portion substantially does not contain Ca, Sr, and Ba.

3. The inorganic structure according to claim 1 or 2, in, The metal element other than silicon is magnesium.

4. The inorganic structure according to claim 1 or 2, in, The volume ratio of the magnesium oxide particles is greater than the volume ratio of the bonding portion. 5 . The inorganic structure according to claim 1 , wherein the porosity is 20% or less.

6. The inorganic structure according to claim 1 or 2, in, The magnesium oxide particles are crystalline. 7 . The inorganic structure according to claim 1 , which has a thermal conductivity of 2 W / m·K or more. 8 . The inorganic structure according to claim 1 , which has a thickness of 500 μm or more.

9. A method for producing an inorganic structure, comprising the following steps: a step of obtaining a mixture by mixing a plurality of magnesium oxide particles, a plurality of amorphous silicon dioxide particles, and an aqueous solution containing a metal element other than silicon; and The mixture is pressurized and heated under the conditions of a pressure of 10 to 600 MPa and a temperature of 50 to 300° C. in, The inorganic structure comprises: the plurality of magnesium oxide particles; and a bonding portion that covers the surface of the magnesium oxide particles and bonds the magnesium oxide particles together, The bonding portion contains an amorphous compound including silicon, a metal element other than silicon, and oxygen, and substantially does not contain alkali metals, B, V, Te, P, Bi, Pb, and Zn. The bonding part includes fine particles derived from the silica particles and having an average particle size of 100 nm or less, The microparticles include silicon and oxygen.

Citation Information

Patent Citations

  • Manufacture of high density magnesia sintered body

    JP1979142212A

  • Stator of rotary electric machine and manufacturing method thereof

    JP2020092468A

  • Formed body, coated body, manufacturing method of formed body and manufacturing method of cutting body

    CN103044062A