Gas explosion resistant structure and preparation method thereof

By combining anti-explosion panels, fiber-reinforced concrete layers and polymer elastomer layers on anti-explosion panels, the problem of insufficient anti-explosion capabilities of existing anti-explosion panels is solved, achieving stronger gas explosion impact protection and protecting petrochemical equipment. and the safety of surrounding buildings.

CN115519862BActive Publication Date: 2024-10-29CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110704041.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-24
Publication Date
2024-10-29
Estimated Expiration
2041-06-24

AI Technical Summary

Technical Problem

Existing anti-explosion panels have insufficient anti-explosion capabilities when faced with gas explosion impacts, making it difficult to effectively protect petrochemical plants and surrounding buildings, resulting in potential casualties and equipment damage.

Method used

An anti-gas explosion structure is adopted, including an anti-explosion panel, a fiber-reinforced concrete layer and a polymer elastomer layer. The fiber-reinforced concrete layer is set between the anti-explosion panel and the polymer elastomer layer. The upper surface of the anti-explosion panel is distributed with concave and convex patterns. , the fiber-reinforced concrete layer is filled with a mesh fiber layer, which absorbs and attenuates explosion energy through this structure.

Benefits of technology

The anti-explosion ability of the anti-explosion panel is significantly improved, which can more effectively resist the impact of gas explosions, protect the safety of surrounding buildings and devices, and enhance the flexibility and impact resistance of the overall structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115519862B_ABST
    Figure CN115519862B_ABST
Patent Text Reader

Abstract

The present invention provides a gas explosion resistant structure and a preparation method thereof, wherein the gas explosion resistant structure comprises: an explosion resistant panel, a fiber reinforced concrete layer and a polymer elastomer layer, wherein the fiber reinforced concrete layer is arranged between the explosion resistant panel and the polymer elastomer layer, and the upper surface of the explosion resistant panel is provided with concave-convex patterns. The gas explosion resistant structure provided by the present invention can better resist the impact of gas explosion, absorb the explosion energy, and protect the safety of surrounding buildings and devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of explosion-proof technology, and in particular to a gas explosion-proof structure and a preparation method of the gas explosion-proof structure. Background Art

[0002] Petrochemical plants are characterized by high temperature, high pressure, high blockage and large size, and there is a risk of flammable gas leakage. The explosion energy of a large amount of flammable gas is huge, which often causes serious damage to important buildings such as control rooms, external operation rooms, cabinet rooms and adjacent tank areas around the petrochemical plants, and even causes casualties to nearby people.

[0003] At present, a large number of single-unit control rooms in service (including offices and external operation rooms) have basically not taken into account the explosion-proof requirements as a whole, and only set up explosion-proof walls on the side of the control room facing the device. Once an explosion occurs, it is very likely to cause great casualties. Therefore, improving the explosion-proof capacity of petrochemical plants and hazardous chemical plants has become an urgent problem that needs to be solved.

[0004] A large number of existing buildings in petrochemical enterprises are brick-concrete structures with low structural strength, great difficulty in renovation, and affecting the normal use of the buildings. Therefore, explosion-proof panels are usually used to improve the explosion-proof capabilities of existing buildings. However, the explosion-proof capabilities of explosion-proof panels in the existing technology are low and it is difficult to meet the protection needs of gas explosion shocks. Summary of the invention

[0005] In view of the technical problem that the explosion-proof ability of explosion-proof panels in the prior art is low and it is difficult to meet the protection needs of gas explosion impact, the present invention provides a gas explosion-proof structure and a method for preparing the gas explosion-proof structure. By adopting the gas explosion-proof structure, the explosion-proof ability of the explosion-proof panels can be improved, the explosion energy can be absorbed, the gas explosion impact can be better resisted, and the safety of surrounding buildings and equipment can be protected.

[0006] To achieve the above objectives, the present invention provides a gas explosion resistant structure, comprising: an explosion-proof panel, a fiber reinforced concrete layer and a polymer elastomer layer, wherein the fiber reinforced concrete layer is arranged between the explosion-proof panel and the polymer elastomer layer, and the upper surface of the explosion-proof panel is distributed with concave and convex patterns.

[0007] Furthermore, the fiber reinforced concrete layer is filled with at least one mesh fiber layer, and the mesh fiber layer is a mesh structure woven from a plurality of explosion-proof fibers.

[0008] Furthermore, the mesh fiber layer has multiple layers, and the layers are filled in the fiber reinforced concrete layer according to a set layer interval.

[0009] Furthermore, the ratio of the diameter of the explosion-proof fiber to the distance between two adjacent explosion-proof fibers in the mesh fiber layer is between 1:3-8.

[0010] Furthermore, the fiber reinforced concrete layer is composed of the following ingredients in weight percentage: 25%-32% silicate cement, 30%-35% quartz sand, 3.6%-12.5% ​​glass fiber, 0.1%-0.3% basalt fiber, 0.05%-0.15% carbon fiber, 8.5%-15.0% silica powder, and the balance water.

[0011] Furthermore, the upper surface of the explosion-proof panel is distributed with trapezoidal convex wave crest patterns and trapezoidal concave wave trough patterns, and the wave crest patterns and the wave trough patterns are evenly distributed on the explosion-proof panel.

[0012] Furthermore, the thickness of the explosion-proof panel is between 0.2 mm and 2 mm.

[0013] Furthermore, the length of the top side of the crest lines is the same as the length of the bottom side of the trough lines.

[0014] Furthermore, the length ratio of the waistline between the top edge of the crest pattern and the bottom edge of the trough pattern to the top edge of the crest pattern is between 1:1-3.

[0015] Furthermore, the angle between the top edge of the crest pattern and the waistline is between 120° and 150°, and the angle between the bottom edge of the trough pattern and the waistline is between 30° and 60°.

[0016] Furthermore, the polymer elastomer layer is made of a first component and a second component, and the volume ratio of the first component to the second component is between 0.75-1.15:1; the first component is composed of the following ingredients in weight percentage: 22%-38% of toluene diisocyanate, 53%-72% of monopentaerythritol, and 6%-12% of a semi-prepolymer obtained by polymerization of polyether ester; the second component is composed of the following ingredients in weight percentage: 11%-26% of diethylaminoethanol, 28%-87% of flexible amine, 7%-15% of flame retardant, and 8%-18% of antioxidant.

[0017] Another aspect of the present invention provides a method for preparing the above-mentioned gas explosion-resistant structure, which comprises the following steps: step 1), mixing silicate cement, quartz sand and silicon powder, stirring until they are evenly dispersed, adding water and stirring for 5-15 minutes, then adding basalt fiber and continuing to stir for 3-8 minutes, then adding carbon fiber and continuing to stir for 8-15 minutes to prepare fiber-reinforced concrete; step 2), laying a layer of mesh fiber layer, pouring fiber-reinforced concrete on the laid layer of mesh fiber layer, laying another layer of mesh fiber layer on the poured fiber-reinforced concrete, and then pouring fiber-reinforced concrete on the laid layer of mesh fiber layer, and so on, until the poured mesh fiber layer is completely filled with fiber. The number of layers reaches the set number of layers; step 3), the composite structure prepared in step 2) is allowed to stand at 20-30°C for 2-5h, then a binder is coated on the surface of the composite structure, and the explosion-proof panel and the composite structure are pressed into an integral structure with high pressure; step 4), the overall structure prepared in step 3) is cured at 60-85°C for 2-5h, and then placed at 20-30°C for 1-3 days; step 5), the bottom surface of the overall structure prepared in step 4) is coated with an adhesive primer at 20-30°C and allowed to stand for 20-90min; step 6), after mixing the first component with the second component, spray them on the bottom surface of the overall structure prepared in step 5) to prepare a gas explosion-resistant structure.

[0018] Through the technical solution provided by the present invention, the present invention has at least the following technical effects:

[0019] The anti-gas explosion structure of the present invention comprises an anti-explosion panel, a fiber-reinforced concrete layer and a polymer elastomer layer, wherein the fiber-reinforced concrete layer is arranged between the anti-explosion panel and the polymer elastomer layer, and the upper surface of the anti-explosion panel is distributed with concave-convex patterns. The anti-explosion panel can resist the explosion shock wave and ensure the integrity of the entire structure, the fiber-reinforced concrete layer has a certain weight and can better include surrounding buildings and devices, and the polymer elastomer layer increases the overall flexibility of the anti-gas explosion structure, which can not only prevent the fiber-reinforced concrete layer from being destroyed, but also has a wrapping and protective effect, can absorb the explosion energy, and attenuate the explosion shock wave. The anti-gas explosion structure provided by the present invention can improve the explosion resistance of the anti-explosion panel, absorb the explosion energy, better resist the gas explosion shock, and protect the safety of surrounding buildings and devices.

[0020] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A cross-sectional view of a gas explosion resistant structure provided by an embodiment of the present invention;

[0022] Figure 2 A schematic diagram of an explosion-proof panel in a gas explosion-proof structure provided by an embodiment of the present invention;

[0023] Figure 3 A schematic diagram of a mesh fiber layer in a gas explosion resistant structure provided by an embodiment of the present invention.

[0024] Description of Reference Numerals

[0025] 1 Explosion-resistant panel 2 Fiber-reinforced concrete layer

[0026] 3 polymer elastic layer 4 mesh fiber layer DETAILED DESCRIPTION

[0027] The specific implementation of the embodiment of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the embodiment of the present invention, and is not used to limit the embodiment of the present invention.

[0028] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0029] In the present invention, unless otherwise specified, directional words such as "up, down, top, bottom" are usually used with reference to the directions shown in the drawings or are used to describe the relative positional relationships of components in the vertical, perpendicular or gravity direction.

[0030] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.

[0031] Please refer to Figure 1 and Figure 2 On the one hand, an embodiment of the present invention provides a gas explosion-proof structure, which includes: an explosion-proof panel 1, a fiber-reinforced concrete layer 2 and a polymer elastomer layer 3, wherein the fiber-reinforced concrete layer 2 is arranged between the explosion-proof panel 1 and the polymer elastomer layer 3, and the upper surface of the explosion-proof panel 1 is distributed with concave-convex patterns.

[0032] Specifically, in the embodiment of the present invention, the gas explosion resistant structure includes an explosion resistant panel 1, a fiber reinforced concrete layer 2 and a polymer elastomer layer 3. The upper surface of the explosion resistant panel 1 is distributed with concave-convex patterns, and the concave-convex patterns can be in any shape, such as wavy, zigzag, etc. The explosion resistant panel 1 faces the explosion point and can resist the explosion shock wave to ensure the integrity of the entire structure. The fiber reinforced concrete layer 2 is arranged between the explosion resistant panel 1 and the polymer elastomer layer 3 and has a certain weight. The fibers in the fiber reinforced concrete layer can enhance the integrity of the concrete, absorb the explosion shock wave, and better include the surrounding buildings and devices. The polymer elastomer layer 3 increases the overall flexibility of the gas explosion resistant structure, which can not only prevent the fiber reinforced concrete layer 2 from being destroyed, but also has a wrapping and protective effect, can absorb the explosion energy, and attenuate the explosion shock wave.

[0033] The gas explosion-proof structure provided by the present invention can improve the explosion-proof capability of the explosion-proof panel, absorb explosion energy, better resist the impact of gas explosion, and protect the safety of surrounding buildings and devices.

[0034] Furthermore, the fiber reinforced concrete layer 2 is filled with at least one mesh fiber layer 4, and the mesh fiber layer 4 is a mesh structure woven from explosion-proof fibers.

[0035] Specifically, in an embodiment of the present invention, at least one mesh fiber layer 4 is included. The mesh fiber layer 4 is a mesh structure woven from explosion-proof fibers. When pouring the fiber reinforced concrete layer 2, at least one mesh fiber layer 4 is filled in the fiber reinforced concrete layer 2. After the fiber reinforced concrete layer 2 is cured, the bonding force between the mesh fiber layer 4 and the fiber reinforced concrete layer 2 can be enhanced, thereby improving the overall gas explosion resistance of the anti-gas explosion structure.

[0036] Furthermore, the mesh fiber layer 4 has multiple layers, and the layers are filled in the fiber reinforced concrete layer 2 according to a set layer interval.

[0037] Specifically, in the embodiment of the present invention, the mesh fiber layer 4 has multiple layers, and the layers are filled in the fiber reinforced concrete layer 2 according to the set layer spacing. In the embodiment of the present invention, the number of mesh fiber layers 4 is between 1 and 5 layers, which can improve the overall gas explosion impact resistance of the gas explosion-resistant structure while ensuring the cost of the gas explosion-resistant structure.

[0038] Furthermore, the ratio of the diameter of the explosion-proof fiber to the distance between two adjacent explosion-proof fibers of the mesh fiber layer 4 is between 1:3-8.

[0039] Please refer to Figure 3 Specifically, in the embodiment of the present invention, each mesh fiber layer 4 is woven from a plurality of explosion-proof fibers, and the ratio of the diameter R of the explosion-proof fiber to the distance W between two adjacent explosion-proof fibers is between 1:3-8. The mesh fiber layer 4 made in this way can not only improve the absorption capacity of the explosion energy, but also improve the overall strength of the mesh fiber layer 4, making it not easy to be damaged, protecting the fiber reinforced concrete layer 2, and further improving the overall gas explosion resistance of the anti-gas explosion structure.

[0040] Furthermore, the fiber reinforced concrete layer 2 is composed of the following components in weight percentage:

[0041] Portland cement 25%-32%, quartz sand 30%-35%, glass fiber 3.6%-12.5%, basalt fiber 0.1-0.3%, carbon fiber 0.05%-0.15%, silica powder 8.5%-15.0%, and the balance water.

[0042] Specifically, in the embodiment of the present invention, silicate cement sets and hardens quickly, has high strength, good frost resistance, and can be quickly solidified to provide high structural strength. The optimal proportion of silicate cement in the fiber reinforced concrete layer 2 is 25%-32%. If the proportion of silicate cement is too high, the corrosion resistance of the fiber reinforced concrete layer 2 will be reduced due to the poor corrosion resistance of silicate. If the proportion is too low, the strength of the fiber reinforced concrete layer 2 will be reduced. The content is preferably 26%-32%, and more preferably 26%-31%.

[0043] Quartz sand has the characteristics of high hardness, high specific gravity, high mechanical strength, and uniform particle size, which can improve the strength of the structure. The optimal proportion of quartz sand in the fiber-reinforced concrete layer 2 is 30%-35%. Compared with other proportions, the fiber-reinforced concrete layer 2 has high structural strength and can meet the explosion-proof requirements of the structure. Otherwise, the explosion-proof ability of the structure is reduced. The content is preferably 31%-35%, and more preferably 31%-34%.

[0044] Glass fiber, basalt fiber and carbon fiber can effectively improve the tensile strength of concrete, prevent the expansion of original cracks in the substrate and delay the generation of cracks, so that the impermeability, antifreeze and other properties of the composite material are significantly improved compared with the substrate. And when the concrete is under tension, even if a large number of cracks have appeared in the substrate, it can still continue to withstand a certain load and have pseudo-ductility, so that the toughness and impact resistance of the fiber-reinforced concrete layer 2 can be significantly improved. The appropriate proportion of fibers will improve the ductility and strength of the fiber-reinforced concrete layer 2. If the overall fiber ratio is too high, the fibers are easy to agglomerate, the volume is large and the dispersibility is poor, but the effect of strengthening and toughening will not be achieved, and the fiber price is high, which will greatly increase the cost. If the ratio is too low, the effect of fiber reinforcement crack resistance and toughening does not meet the explosion-proof performance requirements of the fiber-reinforced concrete layer 2. The glass fiber content is preferably 3.9%-12.1%, more preferably 4.6%-11.5%; the basalt fiber content is preferably 0.11-0.28%, more preferably 0.13-0.27%; the carbon fiber content is preferably 0.06%-0.15%, more preferably 0.06%-0.14%.

[0045] Furthermore, the upper surface of the explosion-proof panel 1 is distributed with trapezoidal convex wave crest patterns and trapezoidal concave wave trough patterns, and the wave crest patterns and the wave trough patterns are evenly distributed on the explosion-proof panel 1 .

[0046] Furthermore, the thickness of the explosion-proof panel 1 is between 0.2 mm and 2 mm.

[0047] Specifically, in the embodiment of the present invention, the explosion-proof panel 1 with a thickness of 0.2 mm to 2 mm can well resist the explosion shock wave and ensure the integrity of the entire structure while ensuring the cost of the gas explosion-proof structure.

[0048] Furthermore, the length of the top side of the crest lines is the same as the length of the bottom side of the trough lines.

[0049] Specifically, in the embodiment of the present invention, the length L1 of the top side of the crest lines is the same as the length L3 of the bottom side of the trough lines.

[0050] Furthermore, the length ratio of the waistline between the top edge of the crest pattern and the bottom edge of the trough pattern to the top edge of the crest pattern is between 1:1-3.

[0051] Specifically, in the embodiment of the present invention, the ratio of the waistline L2 between the top edge L1 of the crest pattern and the bottom edge L3 of the trough pattern to the length L1 of the top edge of the crest pattern is between 1:1-3. The structure with this length ratio has strong explosion impact resistance and the amount of steel used is more economical.

[0052] Furthermore, the angle between the top edge of the crest pattern and the waistline is between 120° and 150°, and the angle between the bottom edge of the trough pattern and the waistline is between 30° and 60°.

[0053] Specifically, in the embodiment of the present invention, the angle β between the top edge of the crest pattern and the waistline is between 120°-150°, and the angle between the bottom edge of the trough pattern and the waistline α is between 30°-60°. The structure at this angle has strong anti-explosion impact performance, and the amount of steel used is more economical.

[0054] Furthermore, the polymer elastomer layer 3 is made of a first component and a second component, and the volume ratio of the first component to the second component is between 0.75-1.15:1; the first component is composed of the following ingredients in weight percentage: 22%-38% of toluene diisocyanate, 53%-72% of monopentaerythritol, and 6%-12% of a semi-prepolymer obtained by polymerization of polyether ester; the second component is composed of the following ingredients in weight percentage: 11%-26% of diethylaminoethanol, 28%-87% of flexible amine, 7%-15% of flame retardant, and 8%-18% of antioxidant.

[0055] Specifically, in the embodiment of the present invention, toluene diisocyanate mainly provides isocyanate, and the optimal ratio is 22%-38%. The viscosity of the prepolymer formed at this content and the reaction performance of the system are relatively balanced. If the prepolymer formed by a lower content has a higher viscosity, the polymer elastomer layer 3 formed by the reaction has higher elasticity, but lower reactivity. If the prepolymer formed by a higher content has a lower viscosity, it is conducive to the mixing of the two components, but it will be easier to react, resulting in an overly fast reaction speed, a higher internal stress in the polymer elastomer layer 3, and a higher hardness. The content is preferably 25%-38%, and more preferably 25%-36%.

[0056] Monopentaerythritol can control the placement time of the prepolymer, maintain the stability of the first component, and improve the mixing efficiency of the system when the two components are mixed, which can enhance the physical properties of the polymer elastomer and improve the leveling performance of the elastomer material. If the ratio is too high, the mixing efficiency of the two components is too high, and an over-reaction occurs, which affects the performance of the formed polymer elastomer material; if the ratio is too low, the mixing efficiency of the two components is low, the reaction is insufficient, and the performance of the formed polymer elastomer is low. Its content is preferably 55%-70%, and more preferably 58%-70%.

[0057] Diethylaminoethanol can react quickly and reliably with the NCO group in the toluene diisocyanate component. If the ratio is too high, the reaction speed will be too high, the side reaction products will be too much, and the mechanical properties of the formed polymer elastic layer 3 will be affected. If the ratio is too low, the reaction will be insufficient and the reaction speed will be reduced, affecting the mechanical properties of the formed polymer elastic layer 3. The content is preferably 12%-25%, more preferably 13%-24%.

[0058] The main function of the flexible amine is chain extension, which can control the reaction mechanism and enable the polymer elastomer layer 3 to form a thin film during the spraying process. If the ratio is too high, the molecular chain of the reaction product formed is too long, the material hardness is large, and the flexibility is low; if the ratio is too low, the molecular chain of the reaction product formed is short, and it is difficult to form a complete film. The content is preferably 30%-86%, more preferably 38%-80%.

[0059] The main function of the flame retardant is to improve the flame retardant properties of the polymer elastomer layer 3. If the content is high, the original mechanical properties of the polymer elastomer material will decrease. If the content is low, the flame retardant effect is not obvious.

[0060] The antioxidant mainly improves the anti-oxidation and aging performance of the high-molecular-weight elastomer layer 3 and increases the material life. However, the addition of excessive antioxidants will also reduce the mechanical properties of the material. The content is preferably 8%-15%, more preferably 9%-15%.

[0061] Specifically, in the embodiment of the present invention, the polymer elastic body layer 3 is formed by mixing and spraying two components on site, wherein the volume ratio of the first component to the second component is between 0.75-1.15:1.

[0062] A second aspect of the present invention provides a method for preparing the gas explosion resistant structure as described above, the method comprising the following steps:

[0063] Step 1), Portland cement, quartz sand and silica powder are mixed and stirred until uniformly dispersed, water is added and stirred for 5-15 minutes, basalt fiber is added and stirred for 3-8 minutes, and carbon fiber is added and stirred for 8-15 minutes to prepare fiber-reinforced concrete;

[0064] Step 2), laying a layer of mesh fiber layer, pouring fiber reinforced concrete on the laid layer of mesh fiber layer, laying another layer of mesh fiber layer on the poured fiber reinforced concrete, and pouring fiber reinforced concrete on the laid layer of mesh fiber layer, and so on, until the number of layers of mesh fiber layer after pouring reaches the set number of layers;

[0065] Step 3), the composite structure prepared in step 2) is allowed to stand at 20-30° C. for 2-5 hours, then a binder is coated on the surface of the composite structure, and the explosion-proof panel and the composite structure are pressed into an integral structure with high pressure;

[0066] Step 4), curing the overall structure prepared in step 3) at 60-85°C for 2-5 hours, and then placing it at 20-30°C for 1-3 days;

[0067] Step 5), coating the bottom surface of the integral structure prepared in step 4) with a bonding primer at 20-30° C. and leaving it to stand for 20-90 minutes;

[0068] Step 6), after mixing the first component and the second component, spraying them on the bottom surface of the overall structure prepared in step 5), to prepare a gas explosion resistant structure.

[0069] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0070] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0071] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A gas explosion resistant structure, characterized in that: The anti-gas explosion structure comprises: An explosion-proof panel (1), a fiber-reinforced concrete layer (2) and a polymer elastomer layer (3), wherein the fiber-reinforced concrete layer (2) is arranged between the explosion-proof panel (1) and the polymer elastomer layer (3), and the upper surface of the explosion-proof panel (1) is distributed with concave-convex patterns; the polymer elastomer layer (3) is made of a first component and a second component, and the volume ratio of the first component to the second component is between 0.75-1.15:1; the first component is composed of the following components in weight percentage: 22%-38% of toluene diisocyanate, 53%-72% of monopentaerythritol, and 6%-12% of a semi-prepolymer obtained by polymerization of polyether ester; the second component is composed of the following components in weight percentage: 11%-26% of diethylaminoethanol, 28%-87% of flexible amine, 7%-15% of a flame retardant, and 8%-18% of an antioxidant.

2. The gas explosion resistant structure according to claim 1, characterized in that: The fiber-reinforced concrete layer (2) is filled with at least one mesh fiber layer (4), and the mesh fiber layer (4) is a mesh structure woven from a plurality of explosion-proof fibers.

3. The gas explosion resistant structure according to claim 2, characterized in that: The mesh fiber layer (4) has multiple layers, and the layers are filled in the fiber reinforced concrete layer (2) according to a set layer interval.

4. The gas explosion resistant structure according to claim 3, characterized in that: The ratio of the diameter of the explosion-proof fiber to the distance between two adjacent explosion-proof fibers in the mesh fiber layer (4) is between 1:3-8.

5. The gas explosion resistant structure according to claim 4, characterized in that: The fiber reinforced concrete layer (2) is composed of the following components in percentage by weight: Portland cement 25%-32%, quartz sand 30%-35%, glass fiber 3.6%-12.5%, basalt fiber 0.1-0.3%, carbon fiber 0.05%-0.15%, silica powder 8.5%-15.0%, and the balance water.

6. The gas explosion resistant structure according to claim 5, characterized in that: The upper surface of the explosion-proof panel (1) is provided with trapezoidal convex wave crest patterns and trapezoidal concave wave trough patterns, and the wave crest patterns and the wave trough patterns are evenly distributed on the explosion-proof panel (1).

7. The gas explosion resistant structure according to claim 6, characterized in that: The thickness of the explosion-proof panel (1) is between 0.2 mm and 2 mm.

8. The gas explosion resistant structure according to claim 7, characterized in that: The length of the top side of the crest lines is the same as the length of the bottom side of the trough lines.

9. The gas explosion resistant structure according to claim 8, characterized in that: The length ratio of the waistline between the top edge of the crest pattern and the bottom edge of the trough pattern to the top edge of the crest pattern is between 1:1-3.

10. The gas explosion resistant structure according to claim 9, characterized in that: The angle between the top edge of the crest pattern and the waistline is between 120° and 150°, and the angle between the bottom edge of the trough pattern and the waistline is between 30° and 60°.

11. A method for preparing a gas explosion resistant structure according to any one of claims 5 to 10, characterized in that: The method comprises the following steps: Step 1), Portland cement, quartz sand and silica powder are mixed and stirred until uniformly dispersed, water is added and stirred for 5-15 minutes, basalt fiber is added and stirred for 3-8 minutes, and carbon fiber is added and stirred for 8-15 minutes to prepare fiber-reinforced concrete; Step 2), laying a layer of mesh fiber layer, pouring fiber reinforced concrete on the laid layer of mesh fiber layer, laying another layer of mesh fiber layer on the poured fiber reinforced concrete, and pouring fiber reinforced concrete on the laid layer of mesh fiber layer, and so on, until the number of layers of mesh fiber layer after pouring reaches the set number of layers; Step 3), the composite structure prepared in step 2) is allowed to stand at 20-30° C. for 2-5 hours, then a binder is coated on the surface of the composite structure, and the explosion-proof panel and the composite structure are pressed into an integral structure with high pressure; Step 4), curing the overall structure prepared in step 3) at 60-85°C for 2-5 hours, and then placing it at 20-30°C for 1-3 days; Step 5), coating the bottom surface of the integral structure prepared in step 4) with a bonding primer at 20-30° C. and leaving it to stand for 20-90 minutes; Step 6), after mixing the first component and the second component, spraying them on the bottom surface of the overall structure prepared in step 5) to prepare a gas explosion-resistant structure; the volume ratio of the first component to the second component is between 0.75-1.15:1; the first component is composed of the following components in weight percentage: 22%-38% toluene diisocyanate, 53%-72% monopentaerythritol, and 6%-12% semi-prepolymer obtained by polymerization of polyether ester; the second component is composed of the following components in weight percentage: 11%-26% diethylaminoethanol, 28%-87% flexible amine, 7%-15% flame retardant, and 8%-18% antioxidant.

Citation Information

Patent Citations

  • Novel fire-proof and explosion-proof pressure reducing plate

    CN109184016A

  • Bionical protection of shocking resistance of compound multilayer structure

    CN204570986U

  • Drum presss from both sides double -deck explosion -proof cabin of bulkhead of core

    CN206290061U