A kind of preparation method of LCP resin composition
By optimizing the shear conditions and selecting appropriate reactive toughening agents in the twin-screw extruder, the reaction degree of LCP resin and toughening agents is controlled, and the problems of thickness uniformity and binding force fluctuations in the LCP film molding process are solved. Good film uniformity and stability are achieved.
Patent Information
- Application Number
- CN202211129866.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-09-16
AI Technical Summary
The prior art is difficult to effectively control the reaction degree of the reactive toughener and LCP resin molecules, resulting in poor thickness uniformity, poor local light transmittance and large fluctuations in the bonding force between FCCL and copper foil during the molding process, and conventional methods It is difficult to operate concisely and detect the degree of reaction.
By setting the length ratio of the shear section to the conveying section in the twin-screw extruder is 1.5~1.8:1, and the rotation speed range is 200~600 rpm, the initial shear viscosity of LCP resin and the shear viscosity of the composition melt are controlled. If the difference is less than or equal to 10 Pa·s, reactive toughening agents such as polyaryl, polyetherimide, and polycarbonate are used to control their reaction degree with LCP by ≥80%.
The uniformity and thickness uniformity of the LCP resin composition are achieved, the dark pattern of the film is reduced, the bonding force stability between FCCL and copper foil is improved, and the serious degradation of the LCP resin is avoided.
Smart Images

Figure DEST_PATH_IMAGE002 
Figure DEST_PATH_IMAGE004
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing an LCP resin composition. Background Art
[0002] With the development of 5G-related industries, thermoplastic liquid crystal polymer film (hereinafter referred to as LCP film) is attracting more and more attention. LCP film has low hygroscopicity, good drug resistance, heat resistance and dimensional stability, and has smaller dielectric loss than PI film at high frequency, and is increasingly used in FCCL.
[0003] In the entire industrial chain of LCP film, film-forming resin is the foundation. The quality of the resin greatly affects the appearance and quality of the film, and indirectly affects its yield rate when used downstream. The rigidity of the LCP resin molecular chain makes it very easy to orient along the MD direction during the film forming process, resulting in low mechanical strength in the TD direction; and the orderly arrangement of the LCP molecular chain makes the material have very small structural entropy during the cooling and solidification process, and the solidification speed is fast, resulting in film appearance defects; in addition, the rigidity of the LCP molecular chain also leads to its low melt strength, and the film bubble is not easy to stabilize during the blow molding process, resulting in poor uniformity of film thickness.
[0004] In order to improve the problems existing in the LCP film forming process, a common improvement method is to blend and modify the LCP film with a toughening agent to destroy the rigidity of the LCP molecular chain segments, thereby increasing the resin melt strength, improving the resin forming properties and the film appearance. There are two main types of LCP toughening agents: one is a physical cross-linking toughening agent, that is, the toughening agent achieves the effect of improving toughness by physically cross-linking with the LCP resin molecular chain segments; the other is a reactive toughening agent, that is, the toughening agent reacts with the LCP molecules to directly disrupt the rigid structure of the LCP molecular chain segments to achieve a toughening effect.
[0005] In actual use, the degree of reaction between the reactive toughening agent and the LCP resin molecules is the key: if the degree of reaction between the two is low, the toughening effect is poor, and the blow-molded film is prone to poor local light transmittance, or even a continuous "dark line". At the same time, the thickness uniformity of the film is also poor, which further leads to large fluctuations in the bonding force between the FCCL, LCP film and copper foil obtained by copper cladding in the later stage, affecting the stability of the product. However, if the residence time of the melt shear is prolonged in order to increase the degree of reaction, the LCP resin will be excessively degraded, thereby reducing the mechanical properties of the LCP resin film. However, most manufacturers in the prior art do not have the conditions to analyze and detect the degree of reaction between the reactive toughening agent and the LCP resin molecules. Therefore, a preparation process that is simple to operate and can directly reflect the degree of reaction is required by the prior art. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing an LCP resin composition, which can simply and accurately control the reaction degree of a reactive toughening agent with LCP resin molecules to be ≥80%, and will not cause serious degradation of the LCP resin.
[0007] The present invention is achieved through the following technical solutions:
[0008] A method for preparing an LCP resin composition comprises the following steps:
[0009] The LCP resin and the reactive toughening agent are mixed uniformly, and extruded through a twin-screw extruder to obtain an LCP resin composition; wherein the twin-screw extruder screw is set to have a length ratio of the shear section to the conveying section of (1.5-1.8):1, a rotation speed range of 200-600 rpm, and a residence time of each component in the screw of 30-60s, so that the absolute value of the difference between the initial shear viscosity of the LCP resin and the shear viscosity of the LCP resin composition melt is less than or equal to 10Pa·s;
[0010] Tm is the melting point of the LCP resin;
[0011] The reactive toughening agent is selected from at least one of polyarylate, polyetherimide and polycarbonate;
[0012] The staggered angle of the screw shearing section is 60-90 degrees, and the staggered angle of the conveying section is 30-45 degrees.
[0013] The initial shear viscosity of the LCP resin is 30-45 Pa·s.
[0014] Preferably, the absolute value of the difference between the initial shear viscosity of the LCP resin and the shear viscosity of the LCP resin composition melt can be further controlled to be less than or equal to 6 Pa·s through the preferred process.
[0015] The reaction degree R of the reactive toughening agent and LCP is ≥80%.
[0016] The present invention has the following beneficial effects:
[0017] The present invention controls the difference between the initial shear viscosity of the LCP resin and the shear viscosity of the LCP resin composition melt to be less than or equal to 10Pa·s (preferably less than or equal to 6Pa·s) by targeting the shear strength and residence time of the material in the screw, thereby being able to control the reaction degree R of the reactive toughening agent and the LCP to be ≥80%, without causing serious degradation of the LCP resin. When the LCP resin composition extruded by the screw is prepared into a film, the appearance is good (no dark lines, indicating good uniformity of the film), the thickness is uniform, and the binding force between the FCCL film and the copper foil fluctuates little. DETAILED DESCRIPTION
[0018] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0019] The sources of experimental raw materials used in the present invention are as follows:
[0020] LCP resin A: initial shear viscosity 35 Pa·s, melting point 280°C, brand Vicryst R8000;
[0021] LCP resin B: initial shear viscosity 40 Pa·s, melting point 315°C, brand Vicryst R8600;
[0022] LCP resin C: initial shear viscosity 36 Pa·s, melting point 325°C, brand Vicryst R8400;
[0023] Polyarylate: Bosheng, brand SEMMSET HP7070;
[0024] Polyetherimide: Sabic, brand ULTEM PEI 1000-1000 / 7101;
[0025] Polycarbonate: Sabic, brand NORYL PPO731S;
[0026] Polycarbonate / polyarylate alloy: obtained by blending and modifying the above-mentioned polycarbonate and polyarylate in a ratio of 1:1.
[0027] Various test methods:
[0028] (1) Shear viscosity: tested using a Malvern capillary rheometer at a temperature of 20°C above the melting point and a shear rate of 1000s -1 , measured using a die with an inner diameter of 1 mm and a length of 20 mm.
[0029] (2) Melting point: measured using DSC 200 F3 manufactured by NETZSCH Company, with a heating rate of 20°C / min, from room temperature to 30°C above the melting point, then cooled to room temperature at 20°C / min, and finally heated to 30°C above the melting point at 20°C / min. The melting point was obtained by taking the highest point of the melting peak of the second heating curve.
[0030] (3) Film thickness uniformity: Use a digital thickness gauge (Mitutoyo 547-401) to cut a film of 0.5 × 0.5 m in size, and measure the film thickness along the MD direction and TD direction at intervals of 1 cm. Calculate the average thickness X, and take the difference between the maximum and minimum thickness values as the thickness deviation M, expressed as X[M].
[0031] (4) Film uniformity: Cut a film of 0.5×0.5 m in size and use a flashlight to illuminate the back of the film. If the film is uniform and the light and dark are consistent when observed with the naked eye, the film uniformity is excellent; if the light and dark of the film are inconsistent when observed with the naked eye, the uniformity is average; if obvious continuous stripes can be observed, the film uniformity is poor.
[0032] (5) Peel strength between LCP film and copper foil and uniformity of peel strength: Cut a 0.5×0.5m size laminate FCCL, and cut 1.5cm wide peel test pieces every 10cm along the MD and TD directions respectively. Fix the surface layer on a flat plate with double-sided tape, adopt 180° peeling, and the peeling speed is 50mm / min. Measure the strength during peeling, calculate the average peel strength X, and take the difference between the maximum peel strength and the minimum peel strength as the peel strength deviation M.
[0033] (6) Reaction degree of toughening agent: The melt-blended resin is crushed and filtered with a 40-mesh screen. M1g of the filtered LCP powder (containing toughening agent m) is placed in excess chloroform and heated under reflux for 24 hours. The solvent is filtered and the remaining powder is dried and weighed to obtain a mass of M2g. The reaction degree of the toughening agent is R = 1-(M1-M2) / m.
[0034] Embodiment and comparative example Continuous preparation process of LCP resin and film: 97 parts by weight of LCP resin (type see table) and 3 parts by weight of reactive toughening agent (type see table) are mixed evenly and extruded through a twin-screw extruder to obtain a LCP resin composition melt; wherein the twin-screw extruder screw is set to a length ratio of the shear section to the conveying section (see table), and the residence time of each component in the screw (see table) is such that the absolute value of the difference between the initial shear viscosity of the LCP resin and the shear viscosity of the LCP resin composition melt (see table). Then, the LCP resin composition melt is melted at Tm~Tm+15°C and extruded through a die head, and a film is prepared under the conditions of a blow-up ratio of 5.5 and a stretch ratio of 4.8. After cooling, the film is rolled up. At 270°C, it is pressed with an 18μm electrolytic copper foil to obtain FCCL. Wherein, Tm is the melting point of LCP resin; the staggered angle of the screw shearing section is 60-90 degrees, and the staggered angle of the conveying section is 30-45 degrees (except for the rotation speed and the length ratio of the shearing section to the conveying section, the embodiment and the comparative example use the same screw setting).
[0035] Table 1: Parameters of the LCP resin film preparation process of the embodiment and the comparative example
[0036]
[0037] It can be seen from the examples that when the absolute value of the shear viscosity difference is controlled within 10 Pa·s, the film uniformity is good and the FCCL peel strength deviation is small. When the absolute value of the shear viscosity difference is controlled within 6 Pa·s, the peel strength deviation can be controlled within 0.1 kg·cm -1 Within, the reaction degree R>84%.
[0038] Table 1 continued:
[0039]
[0040] It can be seen from Comparative Example 1 that if the residence time is too short, the reaction degree of the reactive toughening agent is only 80.4%, and the shear viscosity of the melt is 10.5 Pa·s lower than the initial viscosity of the LCP resin, resulting in general film uniformity and large deviation in peel strength.
[0041] It can be seen from Comparative Example 2 that if the residence time is too long, the reaction degree can only reach 81.5%, but the LCP resin is severely degraded, resulting in poor film-forming properties.
[0042] It can be seen from Comparative Example 3 that if the length ratio of the shearing section to the conveying section is too low, insufficient shearing will result, resulting in too low a reaction degree of the reactive toughening agent.
[0043] It can be seen from Comparative Example 4 that if the length ratio of the shear section to the conveying section is too long, severe shearing will occur, resulting in severe degradation of the LCP resin (shear viscosity difference -15.6 Pa·s), but the reaction degree of the reactive toughening agent is not improved, so the film uniformity is poor and the peel strength deviation of FCCL is also large.
Claims
1. A method for preparing a LCP resin composition, characterized in that: The following steps are involved: The LCP resin and the reactive toughening agent are uniformly mixed and extruded through a twin-screw extruder to obtain an LCP resin composition; wherein the twin-screw extruder screw is set to have a length ratio of the shear section to the conveying section of (1.5-1.8):1, a rotation speed range of 200-600 rpm, and a residence time of each component in the screw of 30-60s, so that the absolute value of the difference between the initial shear viscosity of the LCP resin and the shear viscosity of the LCP resin composition melt is less than or equal to 10Pa·s; Tm is the melting point of the LCP resin; The reactive toughening agent is selected from at least one of polyarylate, polyetherimide, polycarbonate, and polycarbonate / polyarylate alloy; the staggered angle of the screw shearing section is 60-90 degrees, and the staggered angle of the conveying section is 30-45 degrees; The reaction degree R of the reactive toughening agent and LCP is ≥80%.
2. The method for preparing the LCP resin composition according to claim 1, characterized in that: The initial shear viscosity of the LCP resin is 30-45 Pa·s.
3. The method for preparing the LCP resin composition according to claim 1, characterized in that: The absolute value of the difference between the initial shear viscosity of the LCP resin and the shear viscosity of the LCP resin composition melt is less than or equal to 6 Pa·s.
Citation Information
Cited By
High-performance LCP (Liquid Crystal Polymer) resin and preparation method thereof
CN122011713A