Resin composition, prepreg, circuit substrate and printed circuit board
By using hyperbranched polysiloxane coupling agent to treat fillers in the circuit substrate, the problem of poor thermal expansion coefficient of polyphenylene ether resin is solved, the excellent dielectric performance and good heat resistance of the circuit substrate are achieved, and the thermal expansion coefficient is reduced , and improves apparent performance.
Patent Information
- Application Number
- CN202211220069.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-30
AI Technical Summary
Polyphenylene ether resin has poor thermal expansion coefficient in circuit substrates, resulting in poor heat resistance and easy to appear defects. When increasing the amount of filler, traditional methods can easily lead to uneven dispersion and agglomeration problems.
Hyperbranched polysiloxane coupling agent is used to replace traditional coupling agents to treat the filler surface. Through the synergistic effect of its alkoxy group and unsaturated double bond group, the binding stability of the filler and resin are improved and Cross-linking density improves the dispersion of fillers in resin.
The excellent dielectric performance, good apparent performance, low thermal expansion coefficient and improved heat resistance of the circuit substrate are achieved, and the problems of uneven dispersion and agglomeration of fillers are avoided.
Smart Images

Figure CN115537012B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic products, in particular to a resin composition, a prepreg, a circuit substrate and a printed circuit board. Background Art
[0002] In recent years, with the development of communication technology, the high speed of information processing and transmission and the high frequency of wireless communication have placed higher requirements on the electronic materials used, such as excellent dielectric properties, low thermal expansion coefficient, etc. Among them, polyphenylene ether (PPE) is commonly used in the field of circuit substrate production due to its excellent dielectric properties. However, in practical applications, although polyphenylene ether resin has good dielectric properties, it also has the problem of poor thermal expansion coefficient (CTE), which makes it difficult for polyphenylene ether resin to meet higher requirements in terms of CTE.
[0003] To address this problem, conventional techniques mainly increase the content of fillers in the polyphenylene ether resin system to reduce the thermal expansion coefficient of the polyphenylene ether resin system. However, this method of increasing the amount of fillers to improve the CTE performance can easily lead to uneven dispersion of fillers in the polyphenylene ether resin and agglomeration due to the large increase in filler content, resulting in poor heat resistance of the circuit substrate made of the resin composition and prone to surface defects such as dried flowers and resin grains. Summary of the invention
[0004] Based on this, it is necessary to provide a resin composition, a prepreg, a circuit substrate and a printed circuit board to address the above problems, so that the circuit substrate prepared by using the resin composition can have excellent dielectric properties while not only having good heat resistance, low thermal expansion coefficient, but also good surface performance.
[0005] A resin composition, comprising the following components, by weight: 100 parts by weight of unsaturated double bond-terminated polyphenylene ether, 0.1 to 35 parts by weight of a hyperbranched polysiloxane coupling agent, 150 to 350 parts by weight of a filler, and a solvent;
[0006] Wherein, the general structural formula of the hyperbranched polysiloxane coupling agent is shown in formula (I):
[0007]
[0008] Among them, R 1 Selected from hydrocarbon groups; R 2 , R 3 and R 4 Each independently selected from an alkoxy group or a group A containing an unsaturated double bond, and R 2 , R 3 and R 4 At least one of R is selected from alkoxy; 5Selected from the group A containing an unsaturated double bond.
[0009] In one embodiment, R 1 A straight chain hydrocarbon group having 2 to 10 carbon atoms;
[0010] and / or, R 2 , R 3 and R 4 Each independently selected from an alkoxy group having 2 to 9 carbon atoms or a group A containing an unsaturated double bond having 2 to 6 carbon atoms, and R 2 , R 3 and R 4 At least one of them is selected from alkoxy;
[0011] and / or, R 5 A is a group having 2 to 6 carbon atoms and containing an unsaturated double bond.
[0012] In one embodiment, the group A containing an unsaturated double bond includes one of an acrylate group, a methacrylate group and a vinyl group.
[0013] In one embodiment, the alkoxy group accounts for 10%-70% of the terminal groups in the hyperbranched polysiloxane coupling agent, and the group A containing an unsaturated double bond accounts for 30%-90% of the terminal groups in the hyperbranched polysiloxane coupling agent.
[0014] In one embodiment, the number average molecular weight of the hyperbranched polysiloxane coupling agent is 1500-4500.
[0015] In one embodiment, the number average molecular weight of the unsaturated double bond-terminated polyphenylene ether is 1000-3000;
[0016] And / or, the unsaturated double bond-terminated polyphenylene ether includes one or more of vinyl polyphenylene ether, vinyl benzyl polyphenylene ether, acrylate polyphenylene ether, methacrylate polyphenylene ether and allyl polyphenylene ether.
[0017] In one embodiment, in the terminal group of the polyphenylene ether terminated with an unsaturated double bond, the number of the group B containing an unsaturated double bond is 1-3.
[0018] In one embodiment, the resin composition further comprises one or more of a cross-linking curing agent, an initiator and a flame retardant.
[0019] In one embodiment, the filler includes one or more of silicon dioxide, talc, mica or metal hydroxide.
[0020] A prepreg is obtained by coating the above-mentioned resin composition on a reinforcing material and drying the resultant.
[0021] A circuit substrate comprises a dielectric layer and a metal foil arranged on at least one surface of the dielectric layer; wherein the dielectric layer comprises at least one prepreg as described above.
[0022] A printed circuit board is made of the circuit substrate as described above.
[0023] In the resin composition of the present invention, a hyperbranched polysiloxane coupling agent of the structure of formula (I) is used to replace a traditional coupling agent to perform surface treatment on the filler. Since the terminal group of the hyperbranched polysiloxane coupling agent structure simultaneously has an alkoxy group and a group A containing an unsaturated double bond, and the alkoxy group and the group A containing an unsaturated double bond have a synergistic effect, on the one hand, the hyperbranched polysiloxane coupling agent can form an efficient coating on the surface of the filler, improve the bonding stability between the hyperbranched polysiloxane coupling agent and the filler, thereby making the filler more dispersible in the resin composition, and making the circuit substrate prepared by using the resin composition of the present invention have good surface performance; on the other hand, the hyperbranched polysiloxane coupling agent and the resin have a high crosslinking density, which not only improves the bonding strength between the hyperbranched polysiloxane coupling agent and the resin, but also improves the bonding strength between the filler and the resin, thereby further making the filler more dispersible in the resin composition, greatly reducing the thermal expansion coefficient of the circuit substrate prepared by using the resin composition of the present invention; and the heat resistance of the circuit substrate prepared by using the resin composition of the present invention is effectively improved.
[0024] It can be seen that in the resin composition of the present invention, the use of a hyperbranched polysiloxane coupling agent with a structure of formula (I) can not only make the filler more dispersible in the resin composition, but also have a high crosslinking density with the resin, so that the circuit substrate can have excellent dielectric properties while having good heat resistance, a low thermal expansion coefficient, and good surface performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is the reaction formula of the hyperbranched polysiloxane coupling agent prepared in Example 1 of the present invention;
[0026] Figure 2 This is an electron microscope image of the circuit substrate prepared in Example 1 of the present invention;
[0027] Figure 3 This is an electron microscope image of the circuit substrate prepared in Comparative Example 3 of the present invention;
[0028] Figure 4 It is the structural formula of the hyperbranched coupling agent in Comparative Example 5 of the present invention. DETAILED DESCRIPTION
[0029] The resin composition, prepreg, circuit substrate and printed circuit board provided by the present invention will be further described below.
[0030] The resin composition provided by the present invention comprises the following components by weight: 100 parts by weight of unsaturated double bond-terminated polyphenylene ether, 0.1 parts by weight to 35 parts by weight of hyperbranched polysiloxane coupling agent, 150 parts by weight to 350 parts by weight of filler and solvent; preferably, the hyperbranched polysiloxane coupling agent is 10 parts by weight to 20 parts by weight. The general structural formula of the hyperbranched polysiloxane coupling agent is shown in formula (I):
[0031]
[0032] Among them, R 1 Selected from hydrocarbon groups; R 2 , R 3 and R 4 Each independently selected from an alkoxy group or a group A containing an unsaturated double bond, and R 2 , R 3 and R 4 At least one of R is selected from alkoxy; 5 Selected from the group A containing an unsaturated double bond.
[0033] Specifically, R is preferably 1 is a straight-chain hydrocarbon group. On the one hand, it can effectively avoid thermal oxidation and thermal degradation, and ensure the heat resistance and dielectric stability of the circuit substrate made of the resin composition; on the other hand, it can reduce the reaction steric hindrance and increase the synthesis rate of the hyperbranched polysiloxane coupling agent. At the same time, it is preferred that R 1 The straight-chain hydrocarbon group can make the prepared hyperbranched polysiloxane coupling agent have better fluidity, thereby further improving the apparent performance of the circuit substrate made of the resin composition.
[0034] Furthermore, the present invention preferably R 1 It is a straight-chain hydrocarbon group with 2 to 10 carbon atoms, and the carbon chain length is moderate, which can ensure that the hyperbranched polysiloxane coupling agent can better treat and coat the surface of the filler, ensure better compatibility between the filler and the resin, thereby improving the apparent performance of the circuit substrate prepared using the resin composition and reducing the risk of apparent defects in the circuit substrate.
[0035] Taking into account the effect of the carbon chain length on the activity of the end group of the hyperbranched polysiloxane coupling agent, the present invention preferably has an alkoxy group with a carbon number of 2-9, and further preferably has a carbon number of 2-3. The use of an alkoxy group with such a carbon chain length can effectively ensure the activity of the end group of the hyperbranched polysiloxane coupling agent, form an efficient surface treatment on the surface of the filler, and make the filler more dispersed, thereby improving the apparent performance of the circuit substrate.
[0036] In order to meet the requirements of the terminal groups (R 2 , R 3 , R4 and R 5 ), the carbon number of the group A containing an unsaturated double bond of the present invention is preferably 2-6, which can ensure the crosslinking density between the hyperbranched polysiloxane coupling agent and the polyphenylene ether; and R of the group A containing an unsaturated double bond of the carbon chain length is selected from 5 In addition to satisfying the above-mentioned reaction activity, steric hindrance can also be increased, so that the hyperbranched polysiloxane coupling agent of the present invention has a higher density and a more compact structure, and has no intermolecular entanglement and better fluidity, thereby reducing the viscosity of the resin composition, so that the circuit substrate prepared by the resin composition has good apparent performance.
[0037] Furthermore, the group A containing an unsaturated double bond includes one of an acrylate group, a methacrylate group and a vinyl group; further, a vinyl group is preferred, so that the reactivity of the hyperbranched polysiloxane coupling agent is higher, and the reaction crosslinking density of the resin composition can be increased, thereby improving the heat resistance of the circuit substrate prepared using the resin composition.
[0038] It should be noted that R in the present invention 2 , R 3 and R 4 One or two of the above may also be selected from polysiloxane to achieve further grafting of the coupling agent and improve the stability of the hyperbranched structure.
[0039] Optionally, the alkoxy group accounts for 10%-70% of the terminal groups in the hyperbranched polysiloxane coupling agent, and the group A containing an unsaturated double bond accounts for 30%-90% of the terminal groups in the hyperbranched polysiloxane coupling agent; the alkoxy group content within this range can fully react with the hydroxyl group on the surface of the filler, better coat the surface of the filler, improve the compatibility of the resin, make the filler better dispersed in the resin, improve the bonding stability between the filler and the filler, and improve the apparent performance of the circuit substrate; and the excess alkoxy group is combined with water molecules in the air to form a low surface energy layer after hydrolysis and condensation, which has a non-hydrophilic effect, so that the circuit substrate made of the resin composition has excellent heat resistance and good water resistance.
[0040] At the same time, the group A containing an unsaturated double bond within the range can ensure that the hyperbranched polysiloxane coupling agent has sufficient end group activity, so that it undergoes a cross-linking reaction with the resin, thereby improving its compatibility with the resin and the cross-linking density; and the arrangement of the group A containing an unsaturated double bond, especially the group A containing an unsaturated double bond is R 5When the hyperbranched polysiloxane coupling agent chain segments are combined with the alkoxyl group, the steric hindrance between the molecules can be increased, thereby limiting the free movement of the hyperbranched polysiloxane coupling agent chain segments, reducing the entanglement between the molecules, so that the alkoxy group is not wrapped by the hyperbranched polysiloxane coupling agent chain segments, thereby increasing the branching degree of the hyperbranched polysiloxane coupling agent, improving the stability of the hyperbranched polysiloxane, and promoting the surface treatment ability of the alkoxy group on the filler, thereby achieving a synergistic effect between the alkoxy group and the unsaturated double bond group when the filler is surface treated, thereby improving the dispersion effect of the filler in the resin, thereby improving the apparent performance and heat resistance of the circuit substrate.
[0041] It should be noted that, in the present invention, the ratio of the alkoxy group and the group A containing an unsaturated double bond to the terminal group in the hyperbranched polysiloxane coupling agent is the ratio of the number of the alkoxy group and the group A containing an unsaturated double bond to the terminal group R in the hyperbranched polysiloxane coupling agent. 2 , R 3 , R 4 and R 5 ratio of the total number of .
[0042] In one or more embodiments, the present invention preferably has a number average molecular weight of the hyperbranched polysiloxane coupling agent of 1500-4500. The hyperbranched polysiloxane coupling agent within this range is not easily volatile, can better disperse the filler, and enables the circuit substrate prepared using the resin composition to have good surface properties.
[0043] In one or more embodiments, the hyperbranched polysiloxane coupling agent of the present invention is prepared by using an alkoxysilane containing an unsaturated double bond and a terminal hydroxyl compound as raw materials, and undergoing an ester exchange condensation reaction at a temperature of 80° C. to 160° C. for 2 h to 8 h.
[0044] Specifically, the molar ratio of the terminal hydroxyl compound to the alkoxysilane containing an unsaturated double bond is 0.1-1.5. The ratio range is set so that the terminal groups of the hyperbranched polysiloxane coupling agent of the present invention have both alkoxy groups and unsaturated double bond groups, so that the alkoxy groups account for 10%-70% of the terminal groups in the hyperbranched polysiloxane coupling agent, and the group A containing an unsaturated double bond accounts for 30%-90% of the terminal groups in the hyperbranched polysiloxane coupling agent, thereby ensuring that the alkoxy groups can be effectively coated on the surface of the filler, and the filler dispersion can be better achieved while improving the reaction activity with the matrix resin, thereby obtaining a cross-linking structure with a high cross-linking density and a more compact structure, thereby improving the bonding strength between the filler and the matrix resin, and further allowing the filler to be better dispersed in the resin, thereby improving the heat resistance and apparent performance of the circuit substrate prepared using the resin composition.
[0045] Furthermore, the alkoxysilane containing unsaturated double bonds includes any one of vinyltrimethoxysilane, methacryloxypropyltrimethoxysilane (KH570) and vinyltriethoxysilane; the two terminal hydroxyl compounds include one or more of 1,3-propylene glycol, neopentyl glycol, butanediol, ethylene glycol, hexanediol, and 1,12-dodecanediol; and the acidic catalyst includes one or more of p-toluenesulfonic acid, trifluoroacetic acid, trifluoromethanesulfonic acid, tin tetrachloride, hydrochloric acid and sulfuric acid.
[0046] Taking into account the viscosity and fluidity of the resin composition, the present invention further preferably has a number average molecular weight of 1000-3000 for the polyphenylene ether terminated with unsaturated double bonds. The polyphenylene ether terminated with unsaturated double bonds within this molecular range not only effectively improves the dielectric properties and heat resistance of the circuit substrate prepared using the resin composition, but also has good surface performance.
[0047] In one or more embodiments, in the terminal groups of the polyphenylene ether terminated with unsaturated double bonds, the number of the groups B containing unsaturated double bonds is 1-3; the polyphenylene ether terminated with unsaturated double bonds within this range has sufficient reactivity, thereby obtaining a good crosslinking density and improving the heat resistance of the circuit substrate prepared from the resin composition. Preferably, the group B containing unsaturated double bonds includes one of allyl, acrylate, methacrylate, vinyl and vinylbenzyl. Further, the polyphenylene ether terminated with unsaturated double bonds includes one or more of vinyl polyphenylene ether, vinylbenzyl polyphenylene ether, acrylate polyphenylene ether, methacrylate polyphenylene ether and allyl polyphenylene ether.
[0048] In order to make the filler surface have hydroxyl groups so that it can better react with the alkoxy groups in the coupling agent, so that the filler can be evenly dispersed in the resin without agglomeration, thereby improving the apparent performance of the circuit substrate made of the resin composition, the filler preferably includes one or more of silicon dioxide, talc, mica and metal hydroxide. Wherein, the silicon dioxide is one or more of crystalline silicon dioxide, spherical silicon dioxide and fused silicon dioxide.
[0049] Furthermore, in order to make the circuit substrate made of the resin composition have a lower thermal expansion coefficient, the filler is preferably spherical silica; the amount of spherical silica used is 250 parts by weight to 350 parts by weight.
[0050] In one or more embodiments, the preparation method of the resin composition of the present invention is as follows: 100 parts by weight of polyphenylene ether end-capped with unsaturated double bonds is added to 100 parts by weight to 200 parts by weight of a solvent, and the mixture is stirred and dispersed uniformly to obtain a polyphenylene ether solution end-capped with unsaturated double bonds; 0.1 parts by weight to 35 parts by weight of a hyperbranched polysiloxane coupling agent is added to the solvent, and the mixture is stirred at room temperature for 30 minutes to 90 minutes, and then 150 parts by weight to 350 parts by weight of a filler is slowly added while stirring, and the mixture is stirred for 0.5 hours to 1.5 hours to obtain a filler mixture modified by a hyperbranched polysiloxane coupling agent; the filler mixture modified by a hyperbranched polysiloxane is slowly added to the polyphenylene ether solution end-capped with unsaturated double bonds obtained above, and the mixture is stirred for 0.5 hours to 1.5 hours to prepare a resin composition.
[0051] In order to better improve the curing rate of the resin composition, in the present invention, the resin composition also includes a cross-linking curing agent, and the amount of the cross-linking curing agent is 10 parts by weight to 60 parts by weight; the cross-linking curing agent is mainly used for curing and cross-linking reaction with polyphenylene ether end-capped with unsaturated double bonds. Furthermore, it is preferred that the number average molecular weight of the cross-linking curing agent is 100-3000; the molecular weight within this range has good fluidity, so that it is easy to obtain a resin composition with higher heat resistance after curing and cross-linking with polyphenylene ether. It should be noted that in the present invention, the cross-linking curing agent can contain carbon-carbon unsaturated double bonds in the molecule, and there is no limitation on the specific type of the cross-linking curing agent, which can be selected according to demand.
[0052] In order to improve the flame retardancy of the resin composition, the present invention further stipulates that the resin composition also includes a flame retardant; wherein the type of the flame retardant is not particularly limited, and it can be a mixture of one or more of a bromine flame retardant, a phosphate flame retardant, a phosphazene flame retardant, a bis(diphenylphosphine) oxide flame retardant and a hypophosphite flame retardant.
[0053] In order to promote the curing reaction of the resin composition, in the present invention, the resin composition also includes an initiator, and the amount of the initiator is 0.1 parts by weight to 1 part by weight. There is no particular limitation on the type of the initiator, and preferably, the initiator can be α, α'-bis(tert-butylperoxym-isopropyl)benzene. In the present invention, there is no particular limitation on the solvent, for example, the solvent can be toluene, acetone, propylene glycol methyl ether, N, N-dimethylformamide, butanone or xylene.
[0054] The present invention also provides a prepreg, which is obtained by coating the above-mentioned resin composition on a reinforcing material and drying it.
[0055] Specifically, the resin composition prepared above is coated on the reinforcing material, and baked at a temperature of 80° C.-180° C. for 1 min-10 min to obtain a prepreg.
[0056] The prepreg of the present invention, during the preparation process, due to the presence of terminal alkoxy groups in the structure of the hyperbranched polysiloxane coupling agent, after the resin composition is prepared, generally some alkoxy groups will remain, and some of the residual alkoxy groups can react with the moisture in the air to promote the drying rate on the surface of the prepreg, and avoid adhesion between the prepregs; and after preparing the prepreg or the circuit substrate, the alkoxy groups remaining at the end can form a low surface energy layer after hydrolysis and polycondensation, which has a non-hydrophilic effect, thereby improving the water resistance of the prepreg and the circuit substrate. It can be seen from this that the prepreg prepared by the resin composition of the present invention has excellent dielectric properties, and not only the heat resistance is effectively improved, but also the water resistance is effectively improved.
[0057] In the present invention, there is no particular limitation on the reinforcing material, which is usually glass fiber cloth, preferably E glass fiber cloth.
[0058] The present invention further provides a circuit substrate, comprising a dielectric layer and a metal foil disposed on at least one surface of the dielectric layer; wherein the dielectric layer comprises at least one prepreg as described above.
[0059] For example, one or more of the above-mentioned prepregs are laminated to obtain a dielectric layer, and a metal foil is coated on one or both sides of the dielectric layer, and pressed for 1h-5h under 1.5MPa-5.0MPa in a hot press to obtain a circuit substrate.
[0060] In the present invention, the specific type of metal foil is not particularly limited, for example, the metal foil may be copper foil, aluminum foil, etc. Preferably, the metal foil is copper foil.
[0061] Considering that when preparing the circuit substrate, the metal foil bonding surface (rough surface) matching the polyphenylene ether system will be subjected to surface chemical treatment, and certain hydroxyl groups and double bond groups will exist on the metal foil surface after the surface chemical treatment. The hyperbranched polysiloxane coupling agent used in the resin composition of the present invention contains alkoxy groups and more unsaturated double bonds in its structure, so the semi-cured sheet prepared by the resin composition containing the coupling agent must have residual double bonds and alkoxy groups; at this time, the double bonds and alkoxy groups remaining in the semi-cured sheet will react with the hydroxyl groups and double bond groups remaining on the surface of the metal foil, thereby realizing the combination between the semi-cured sheet and the metal foil, and at the same time, due to the long molecular chain segment of the hyperbranched polysiloxane coupling agent, it will be more stable after combining with the surface group of the metal foil; and the -Si-O-Si- segment in the structure of the hyperbranched polysiloxane coupling agent has good flexibility and high tensile strength, so that the peeling strength of the prepared circuit substrate is effectively improved. It can be seen that the circuit substrate of the present invention has excellent dielectric properties, good heat resistance, good surface properties and peel strength.
[0062] A printed circuit board is made of the circuit substrate as described above.
[0063] Specifically, the printed circuit board is mainly made of the circuit substrate through processes such as drilling, hole filling, micro-etching, pre-preg, activation, acceleration, chemical copper and copper thickening.
[0064] Hereinafter, the resin composition, prepreg, circuit substrate and printed circuit board will be further described through the following specific examples.
[0065] Example 1
[0066] Vinyl triethoxysilane and 1,3-propylene glycol are mixed, wherein the molar ratio of 1,3-propylene glycol to vinyl triethoxysilane is 0.7, and reacted at a temperature of 100°C for 7 hours under the action of p-toluenesulfonic acid to obtain a hyperbranched polysiloxane coupling agent with a molecular weight of 3800, in which alkoxy groups account for 62% of the terminal groups in the hyperbranched polysiloxane coupling agent, and groups A containing unsaturated double bonds account for 38% of the terminal groups in the hyperbranched polysiloxane coupling agent.
[0067] Figure 1 The present invention uses a nuclear magnetic resonance spectrometer to test the hyperbranched polysiloxane coupling agent prepared in Example 1 by hydrogen nuclear magnetic resonance spectrum, wherein the nuclear magnetic resonance frequency is 400 MHz and the solvent is CDCl. 3, the standard substance is TMS, and the NMR data are as follows: δ5.45 (m, 1H), δ5.30 (m, 1H), δ5.20 (m, 1H), δ3.77 (m, 4H), δ1.85 (m, 2H), δ1.23 (m, 6H). It can be seen from the NMR data that δ5.45ppm belongs to the terminal group -Si-CH=CH 2 The hydrogen proton peak on the middle carbon, δ5.30-5.20ppm, is attributed to the terminal group -Si-CH=CH 2 The hydrogen proton peak on the terminal carbon, δ3.77ppm, is also attributed to the terminal group Si-O-CH 2 -CH 3 and linker -O-CH 2 -CH 2 -CH 2 The hydrogen proton peak on the carbon connected to oxygen on -O-, δ1.85ppm is attributed to the linking group -O-CH 2 -CH 2 -CH 2 -O- The hydrogen proton peak on the middle carbon, δ1.23ppm is attributed to the terminal group -O-CH 2 -CH 3 The hydrogen proton peak on the terminal carbon can be seen that the terminal group of the hyperbranched polysiloxane coupling agent prepared in Example 1 of the present invention contains both an alkoxy group and a group A containing an unsaturated double bond.
[0068] By weight, 100 parts by weight of vinyl benzyl polyphenyl ether are added to 150 parts by weight of xylene, and the mixture is stirred and dispersed uniformly to obtain a vinyl benzyl polyphenyl ether solution; 20 parts by weight of the hyperbranched polysiloxane coupling agent prepared above are dissolved in 125 parts by weight of xylene, and the mixture is stirred and dispersed at room temperature for 30 minutes, and then 320 parts by weight of silicon dioxide are slowly added while stirring to obtain a silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent; then, the silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent is slowly added to the vinyl benzyl polyphenyl ether solution obtained above, and the mixture is stirred at room temperature for 60 minutes to obtain a resin composition.
[0069] The resin composition was coated on an E-type glass cloth and baked at 145° C. for 3 minutes to obtain a prepreg.
[0070] Six of the above-mentioned prepregs were stacked, and both sides thereof were covered with copper foil with a thickness of 18 μm, and pressed in a vacuum hot press at a pressure of 4 MPa for 3 hours to obtain a circuit substrate.
[0071] Example 2
[0072] Vinyl triethoxysilane and 1,3-propylene glycol are mixed, wherein the molar ratio of 1,3-propylene glycol to vinyl triethoxysilane is 0.4, and reacted at a temperature of 120°C for 5 hours under the action of p-toluenesulfonic acid to obtain a hyperbranched polysiloxane coupling agent with a molecular weight of 4500, alkoxy groups accounting for 69% of the terminal groups in the hyperbranched polysiloxane coupling agent, and groups A containing unsaturated double bonds accounting for 31% of the terminal groups in the hyperbranched polysiloxane coupling agent.
[0073] By weight, 100 parts by weight of vinyl benzyl polyphenyl ether are added to 150 parts by weight of xylene, and the mixture is stirred and dispersed uniformly to obtain a vinyl benzyl polyphenyl ether solution; 20 parts by weight of the hyperbranched polysiloxane coupling agent prepared above are dissolved in 125 parts by weight of xylene solvent, and the mixture is stirred and dispersed at room temperature for 60 minutes, and then 320 parts by weight of silicon dioxide are slowly added while stirring to obtain a silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent; then, the silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent is slowly added to the vinyl benzyl polyphenyl ether solution obtained above, and the mixture is stirred at room temperature for 70 minutes to obtain a resin composition.
[0074] The resin composition was coated on an E-type glass cloth and baked at 145° C. for 3 minutes to obtain a prepreg.
[0075] Six prepregs were stacked, and both sides were covered with copper foil with a thickness of 18 μm, and pressed in a vacuum hot press at a pressure of 4 MPa for 3 hours to obtain a circuit substrate.
[0076] Example 3
[0077] Vinyl triethoxysilane and 1,3-propylene glycol are mixed, wherein the molar ratio of 1,3-propylene glycol to vinyl triethoxysilane is 1.4, and reacted at a temperature of 150°C for 4 hours under the action of p-toluenesulfonic acid to obtain a hyperbranched polysiloxane coupling agent with a molecular weight of 1800, alkoxy groups accounting for 16% of the terminal groups in the hyperbranched polysiloxane, and groups A containing unsaturated double bonds accounting for 84% of the terminal groups in the hyperbranched polysiloxane.
[0078] By weight, 100 parts by weight of vinyl benzyl polyphenyl ether are added to 150 parts by weight of xylene, and the mixture is stirred and dispersed uniformly to obtain a vinyl benzyl polyphenyl ether solution; 20 parts by weight of the hyperbranched polysiloxane coupling agent prepared above are dissolved in 125 parts by weight of xylene solvent, and the mixture is stirred and dispersed at room temperature for 30 minutes, and then 320 parts by weight of silicon dioxide are slowly added while stirring to obtain a silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent; then, the silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent is slowly added to the vinyl benzyl polyphenyl ether solution obtained above, and the mixture is stirred at room temperature for 60 minutes to obtain a resin composition.
[0079] The resin composition is coated on an E-type glass cloth and baked at 145° C. for 3 minutes to obtain a prepreg;
[0080] Six prepregs were stacked, and both sides were covered with copper foil with a thickness of 18 μm, and pressed in a vacuum hot press at a pressure of 4 MPa for 3 hours to obtain a circuit substrate.
[0081] Example 4
[0082] Vinyl triethoxysilane and 1,3-propylene glycol are mixed, wherein the molar ratio of 1,3-propylene glycol to vinyl triethoxysilane is 0.7, and reacted at a temperature of 120°C for 5 hours under the action of p-toluenesulfonic acid to obtain a hyperbranched polysiloxane coupling agent with a molecular weight of 3800, alkoxy groups accounting for 62% of the terminal groups in the hyperbranched polysiloxane coupling agent, and groups A containing unsaturated double bonds accounting for 38% of the terminal groups in the hyperbranched polysiloxane coupling agent.
[0083] By weight, 100 parts by weight of vinyl benzyl polyphenyl ether are added to 150 parts by weight of xylene, and the mixture is stirred and dispersed uniformly to obtain a vinyl benzyl polyphenyl ether solution; 5 parts by weight of the hyperbranched polysiloxane coupling agent prepared above are dissolved in 35 parts by weight of xylene solvent, and the mixture is stirred and dispersed at room temperature for 60 minutes, and then 150 parts by weight of silicon dioxide is slowly added while stirring to obtain a silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent; then, the silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent is slowly added to the vinyl benzyl polyphenyl ether solution obtained above, and the mixture is stirred at room temperature for 70 minutes to obtain a resin composition.
[0084] The resin composition was coated on an E-type glass cloth and baked at 145° C. for 3 minutes to obtain a prepreg.
[0085] Six prepregs were stacked, and both sides were covered with copper foil with a thickness of 18 μm, and pressed in a vacuum hot press at a pressure of 4 MPa for 3 hours to obtain a circuit substrate.
[0086] Example 5
[0087] Vinyl triethoxysilane and 1,3-propylene glycol are mixed, wherein the molar ratio of 1,3-propylene glycol to vinyl triethoxysilane is 0.7, and reacted at a temperature of 120°C for 5 hours under the action of p-toluenesulfonic acid to obtain a hyperbranched polysiloxane coupling agent with a molecular weight of 3800, alkoxy groups accounting for 62% of the terminal groups in the hyperbranched polysiloxane coupling agent, and groups A containing unsaturated double bonds accounting for 38% of the terminal groups in the hyperbranched polysiloxane coupling agent.
[0088] By weight, 100 parts by weight of vinyl benzyl polyphenyl ether are added to 150 parts by weight of xylene, and the mixture is stirred and dispersed uniformly to obtain a vinyl benzyl polyphenyl ether solution; 12 parts by weight of the hyperbranched polysiloxane coupling agent prepared above are dissolved in 95 parts by weight of xylene solvent, and the mixture is stirred and dispersed at room temperature for 60 minutes, and then 250 parts by weight of silicon dioxide are slowly added while stirring to obtain a silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent; then, the silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent is slowly added to the vinyl benzyl polyphenyl ether solution obtained above, and the mixture is stirred at room temperature for 70 minutes to obtain a resin composition.
[0089] The resin composition was coated on an E-type glass cloth and baked at 145° C. for 3 minutes to obtain a prepreg.
[0090] Six prepregs were stacked, and both sides were covered with copper foil with a thickness of 18 μm, and pressed in a vacuum hot press at a pressure of 4 MPa for 3 hours to obtain a circuit substrate.
[0091] Example 6
[0092] Vinyl triethoxysilane and 1,12-dodecanediol are mixed, wherein the molar ratio of 1,12-dodecanediol to vinyl triethoxysilane is 0.7, and reacted at a temperature of 120°C for 5 hours under the action of p-toluenesulfonic acid to obtain a hyperbranched polysiloxane coupling agent with a molecular weight of 4400, alkoxy groups accounting for 62% of the terminal groups in the hyperbranched polysiloxane coupling agent, and groups A containing unsaturated double bonds accounting for 38% of the terminal groups in the hyperbranched polysiloxane coupling agent.
[0093] By weight, 100 parts by weight of vinyl benzyl polyphenyl ether are added to 150 parts by weight of xylene, and the mixture is stirred and dispersed uniformly to obtain a vinyl benzyl polyphenyl ether solution; 20 parts by weight of the hyperbranched polysiloxane coupling agent prepared above are dissolved in 125 parts by weight of xylene solvent, and the mixture is stirred and dispersed at room temperature for 60 minutes, and then 320 parts by weight of silicon dioxide are slowly added while stirring to obtain a silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent; then, the silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent is slowly added to the vinyl benzyl polyphenyl ether solution obtained above, and the mixture is stirred at room temperature for 70 minutes to obtain a resin composition.
[0094] The resin composition was coated on an E-type glass cloth and baked at 145° C. for 3 minutes to obtain a prepreg.
[0095] Six prepregs were stacked, and both sides were covered with copper foil with a thickness of 18 μm, and pressed in a vacuum hot press at a pressure of 4 MPa for 3 hours to obtain a circuit substrate.
[0096] Example 7
[0097] Vinyl triethoxysilane and neopentyl glycol are mixed, wherein the molar ratio of neopentyl glycol to vinyl triethoxysilane is 0.7, and reacted at a temperature of 120° C. for 5 hours under the action of p-toluenesulfonic acid to obtain a hyperbranched polysiloxane coupling agent with a molecular weight of 4000, alkoxy groups accounting for 62% of the terminal groups in the hyperbranched polysiloxane coupling agent, and groups A containing unsaturated double bonds accounting for 38% of the terminal groups in the hyperbranched polysiloxane coupling agent.
[0098] By weight, 100 parts by weight of vinyl benzyl polyphenyl ether are added to 150 parts by weight of xylene, and the mixture is stirred and dispersed uniformly to obtain a vinyl benzyl polyphenyl ether solution; 20 parts by weight of the hyperbranched polysiloxane coupling agent prepared above are dissolved in 125 parts by weight of xylene solvent, and the mixture is stirred and dispersed at room temperature for 60 minutes, and then 320 parts by weight of silicon dioxide are slowly added while stirring to obtain a silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent; then, the silicon dioxide mixture modified by a hyperbranched polysiloxane coupling agent is slowly added to the vinyl benzyl polyphenyl ether solution obtained above, and the mixture is stirred at room temperature for 70 minutes to obtain a resin composition.
[0099] The resin composition was coated on an E-type glass cloth and baked at 145° C. for 3 minutes to obtain a prepreg.
[0100] Six prepregs were stacked, and both sides were covered with copper foil with a thickness of 18 μm, and pressed in a vacuum hot press at a pressure of 4 MPa for 3 hours to obtain a circuit substrate.
[0101] Example 8
[0102] Compared with Example 1, the only difference is that 60 parts by weight of a trialkenyl isocyanurate compound is further added to xylene to prepare a resin composition, a prepreg, and a circuit substrate.
[0103] Example 9
[0104] Compared with Example 1, the only difference is that talcum powder is used to replace silicon dioxide to prepare the resin composition, the prepreg and the circuit substrate.
[0105] Example 10
[0106] Compared with Example 1, the only difference is that the molar ratio of 1,3-propylene glycol to vinyltriethoxysilane is 1.6, and a hyperbranched polysiloxane coupling agent with a molecular weight of 3300 is prepared, in which alkoxy groups account for 8% of the terminal groups in the hyperbranched polysiloxane coupling agent, and the group A containing an unsaturated double bond accounts for 55% of the terminal groups in the hyperbranched polysiloxane coupling agent. The resin composition, the prepreg and the circuit substrate are prepared using the hyperbranched polysiloxane coupling agent.
[0107] Comparative Example 1
[0108] Compared with Example 1, the only difference is that the molar ratio of 1,3-propylene glycol to vinyltriethoxysilane is 2.5, and a hyperbranched polysiloxane coupling agent is prepared in which the alkoxy group accounts for 0% of the terminal groups in the hyperbranched polysiloxane coupling agent, and the group A containing an unsaturated double bond accounts for 50% of the terminal groups in the hyperbranched polysiloxane coupling agent, and a resin composition, a prepreg and a circuit substrate are prepared using the same.
[0109] Comparative Example 2
[0110] Compared with Example 1, the only difference is that methyltriethoxysilane is used to replace vinyltriethoxysilane to prepare the corresponding hyperbranched polysiloxane coupling agent, and the resin composition, prepreg and circuit substrate are prepared using the hyperbranched polysiloxane coupling agent.
[0111] Comparative Example 3
[0112] Compared with Example 1, the only difference is that common silane coupling agent 3-(methacryloyloxy)propyltrimethoxysilane is used to replace the hyperbranched polysiloxane coupling agent for surface treatment of silica filler to prepare the resin composition, prepreg and circuit substrate.
[0113] Comparative Example 4
[0114] Compared with Example 1, the only difference is that phenolic hydroxy polyphenylene ether is used instead of vinyl benzyl polyphenylene ether to prepare the resin composition, the prepreg and the circuit substrate.
[0115] Comparative Example 5
[0116] Compared with Example 1, the only difference is that the structural formula is as follows Figure 4 The hyperbranched coupling agent shown in the method is used to replace the hyperbranched polysiloxane coupling agent to carry out surface treatment of the silica filler, and to prepare a resin composition, a prepreg, and a circuit substrate.
[0117] Various performance analysis
[0118] In the present invention, 20 mL of the resin composition prepared in Examples 1-6 and Comparative Examples 1-3 were respectively placed in corresponding 250 mL measuring cylinders, sealed and allowed to stand for 72 hours, and the bottom was observed for filler precipitation and the filler precipitation height was measured. The test results are shown in Table 1.
[0119] Table 1
[0120] Filler precipitation height (mL) Example 1 1.65 Example 2 1.63 Example 3 2.1 Example 4 2.2 Example 5 1.75 Example 6 3.5 Example 7 1.65 Example 8 1.6 Example 9 3 Example 10 3.7 Comparative Example 1 25 Comparative Example 2 15 Comparative Example 3 7 Comparative Example 4 16 Comparative Example 5 4
[0121] As shown in Table 1, the filler is uniformly dispersed in the resin composition prepared by the present invention, and has a good stability filler. At the same time, in conjunction with the data of Example 1 and Example 10, it can be seen that by controlling the usage ratio of 1,3-propylene glycol and vinyl triethoxysilane, the proportion of alkoxy and group A containing unsaturated double bonds in the hyperbranched polysiloxane coupling agent can be controlled, so that the dispersion effect of the filler in the resin can be controlled. If it exceeds the scope defined by the present invention, the dispersibility of the filler in the resin will be reduced. In addition, in conjunction with the data of Example 1 and Comparative Example 1 and Comparative Example 2, it can be seen that the alkoxy and group A containing unsaturated double bonds in the hyperbranched polysiloxane coupling agent structure in the present invention have a synergistic effect on the surface treatment of the filler, so that the dispersibility of the filler in the resin is better.
[0122] The present invention takes the circuit substrates in Example 1 and Comparative Example 3 respectively, and detects them under an electron microscope respectively, and the other detection conditions are the same. The corresponding electron microscope images are as follows: Figure 2 and Figure 3 As shown. Combined Figure 2 and Figure 3 It can be seen that the filler in the circuit substrate of Example 1 of the present invention is evenly dispersed and there is no filler agglomeration, while the filler agglomeration exists in the circuit substrate of Comparative Example 3. Figure 3 The light-colored area in the framed area is the filler agglomeration, and the maximum agglomerated particle size of the filler is 18 μm. It can be seen that in the circuit substrate prepared by using the resin composition of the present invention, the filler has better dispersibility, thereby facilitating the improvement of the appearance of the circuit substrate.
[0123] The present invention tests the dielectric properties, heat resistance, dielectric stability, CTE (coefficient of thermal expansion) performance, water resistance and surface performance of the circuit substrates prepared in Examples 1-9 and Comparative Examples 1-5 under the same conditions. The test results are shown in Table 2.
[0124] The measurement method is as follows:
[0125] Dielectric properties: Normal dielectric loss Df 1 : Measured according to the method specified in IEC61189-721-2015; that is, the Df of each circuit substrate at a frequency of 10GHz is obtained by testing the separated dielectric column resonator SPDR method 1 value.
[0126] Dielectric stability: thermal dielectric loss Df 2 : After the copper foil on the surface of each circuit substrate is removed, it is treated at 125°C for 72 hours and measured according to the method specified in IEC61189-721-2015; that is, the Df of each circuit substrate with the copper foil removed at a frequency of 10GHz is obtained by testing the separated dielectric column resonator SPDR method. 2; ΔDf=Df 2 -Df 1 The smaller the ΔDf value, the better the dielectric stability of the material.
[0127] Heat resistance: Glass transition temperature (Tg) test: Determined according to the TMA method specified in IPC-TM-650 2.4.24.
[0128] Filler agglomerate particle size: Each circuit substrate is tested using an electron microscope, the dispersion of the filler in the circuit substrate is observed under the electron microscope, and the filler agglomerate particle size is measured.
[0129] CTE (Coefficient of Thermal Expansion): The coefficient of thermal expansion of each circuit substrate is measured using a TMA instrument according to the CTE test method specified in standard IPC-TM-650 2.4.24. The coefficient of thermal expansion is a value of 50 to 260°C on the Z-axis.
[0130] Hydrophobic angle: Use a water contact angle meter to measure the contact angle between distilled water and each circuit substrate in the air. Take the average value of multiple measurements to get the hydrophobic angle.
[0131] Appearance: Observe the appearance of each circuit board with the copper foil removed by human eyes and evaluate every 0.9m 2 The number of dried flowers within the circuit board.
[0132] Table 2
[0133]
[0134] As shown in Table 2, the resin composition of the present invention, by using a hyperbranched polysiloxane coupling agent with a specific structure, is more effective than ordinary silane coupling agents and the resin composition of the present invention. Figure 4 The hyperbranched coupling agent shown in the figure has a synergistic effect between the alkoxy group and the group A containing an unsaturated double bond in its structure, so that the filler has better dispersibility in the polyphenylene ether resin, greatly reduces the thermal expansion coefficient of the resin composition and the circuit substrate, so that the circuit substrate can have excellent dielectric properties while improving not only the heat resistance, but also the water resistance and peel strength, and good surface performance.
[0135] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0136] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A resin composition, It is characterized in that The invention comprises the following components in parts by weight: 100 parts by weight of polyphenylene ether containing unsaturated double bonds as end capping, 0.1 parts by weight to 35 parts by weight of hyperbranched polysiloxane coupling agent, 150 parts by weight to 350 parts by weight of filler and solvent; Wherein, the general structural formula of the hyperbranched polysiloxane coupling agent is shown in formula (I): Formula (I), Among them, R 1 Selected from hydrocarbon groups; R 2 , R 3 and R 4 are independently selected from an alkoxy group or a group containing an unsaturated double bond, and R 2 , R 3 and R 4 At least one of R is selected from alkoxy; 5 is selected from groups containing unsaturated double bonds; The alkoxy group accounts for 10%-70% of the terminal groups in the hyperbranched polysiloxane coupling agent, and the group containing an unsaturated double bond accounts for 30%-90% of the terminal groups in the hyperbranched polysiloxane coupling agent.
2. The resin composition according to claim 1, It is characterized in that R 1 A straight chain hydrocarbon group having 2 to 10 carbon atoms; and / or, R 2 , R 3 and R 4 Each independently selected from an alkoxy group having 2 to 9 carbon atoms or a group containing an unsaturated double bond having 2 to 6 carbon atoms, and R 2 , R 3 and R 4 At least one of them is selected from alkoxy; and / or, R 5 It is selected from groups containing unsaturated double bonds having 2 to 6 carbon atoms.
3. The resin composition according to claim 1, It is characterized in that The group containing an unsaturated double bond includes one of an acrylate group, a methacrylate group and a vinyl group.
4. The resin composition according to any one of claims 1 to 3, It is characterized in that The number average molecular weight of the hyperbranched polysiloxane coupling agent is 1500-4500.
5. The resin composition according to any one of claims 1 to 3, It is characterized in that The number average molecular weight of the unsaturated double bond-terminated polyphenylene ether is 1000-3000; And / or, the unsaturated double bond-terminated polyphenylene ether includes one or more of vinyl polyphenylene ether, vinyl benzyl polyphenylene ether, acrylate polyphenylene ether, methacrylate polyphenylene ether and allyl polyphenylene ether.
6. The resin composition according to any one of claims 1 to 3, It is characterized in that In the terminal groups of the polyphenylene ether terminated with unsaturated double bonds, the number of the groups containing unsaturated double bonds is 1-3.
7. The resin composition according to any one of claims 1 to 3, It is characterized in that The resin composition further comprises one or more of a cross-linking curing agent, an initiator and a flame retardant.
8. The resin composition according to any one of claims 1 to 3, It is characterized in that The filler includes one or more of silicon dioxide, talc, mica or metal hydroxide.
9. A prepreg, It is characterized in that The prepreg is obtained by coating the resin composition according to any one of claims 1 to 8 on a reinforcing material and drying the resultant.
10. A circuit substrate, It is characterized in that It comprises a dielectric layer and a metal foil arranged on at least one surface of the dielectric layer; wherein the dielectric layer comprises at least one prepreg as claimed in claim 9.
11. A printed circuit board, It is characterized in that Made from the circuit substrate as claimed in claim 10.