Ink, hardened material, electronic component, and method for producing electrode member

By using a polymerizable composition containing (meth)acryloylmorpholine, the challenge of forming complex shapes and patterns in high-density installations has been solved, achieving stability of the hardened shape and water solubility at high temperatures, simplifying the process, and reducing environmental impact.

CN115551906BActive Publication Date: 2024-11-19JNC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202180033324.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-17
Filing Date
2021-06-16
Publication Date
2024-11-19
Estimated Expiration
2041-06-16

AI Technical Summary

Technical Problem

Existing technologies struggle to simplify the negative pattern formation process for complex shapes in high-density installations, and require maintaining the stability of the hardened shape under high-temperature conditions. Furthermore, they necessitate the use of water-based stripping fluids to remove materials, which impacts the environment.

Method used

An ionized radiation-hardened material is formed by using a polymeric composition containing (meth)acryloylmorpholine and a specific compound, which is soluble in an aqueous solution and suitable for the manufacture of electrode components.

Benefits of technology

It achieves stability in maintaining the hardened shape under high temperature conditions and allows for material removal using aqueous solutions, simplifying the process and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115551906B_ABST
    Figure CN115551906B_ABST
Patent Text Reader

Abstract

A polymerizable composition, which is an ionizing radiation curable polymerizable composition, comprising: (A) a first component comprising (meth)acryloylmorpholine represented by the following formula (1); and (B) a second component comprising a compound represented by the following formula (2), wherein the total content of the first component and the second component in the polymerizable composition is 50% by weight or more. The polymerizable composition can appropriately maintain the shape after being cured in the curing step S102 even when subjected to a high temperature environment in the heating step S107, and can be dissolved in an aqueous solution in the dissolving step S106. In formula (1), R 1 is hydrogen or methyl. In formula (2), R 2 is hydrogen or a group having 1 to 6 carbon atoms, R 3 and R 4 Each is independently hydrogen or a group having a carbon number of 20 or less, and n is an integer of 1 to 6. The present invention also provides a method for manufacturing an ink, a hardened material, an electronic component, and an electrode member. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymerizable composition that can be preferably used when forming electrodes in batches corresponding to high-density mounting, an ink containing the polymerizable composition, a cured product, an electronic component, a transfer mold containing an ionizing radiation cured product obtained by irradiating the polymerizable composition with ionizing radiation, and a method for manufacturing an electrode component including an electrode group formed on a substrate using the polymerizable composition. Background Art

[0002] Patent Document 1 describes a technology for forming electrodes in batches in a plurality of semiconductor devices (integrated circuits (ICs)) formed on a wafer in a wafer-level chip scale package (WL-CSP) which is a form of high-density packaging. The technology describes a double-layer laminate film having a lower layer comprising a non-radiation-sensitive resin composition and an upper layer comprising a negative-radiation-sensitive resin composition and having both high resolution and easy peelability, and a method for forming bumps using the double-layer laminate film.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2007-79550 Summary of the invention

[0006] Problems to be solved by the invention

[0007] In the double-layer laminated film described in Patent Document 1, when developing, only the portion irradiated with radiation remains in the upper layer, and the portion of the lower layer corresponding to the removed portion (radiation non-irradiated portion) in the upper layer is dissolved and removed. Therefore, only the portion irradiated with radiation remains in the double-layer laminated film, and the radiation non-irradiated portion is removed in the development stage. In this way, a metal paste is embedded in the portion of the double-layer laminated film after removal, and the metal paste is reflowed by heating together with the wafer, thereby forming a plurality of bumps on the wafer in batches. After the bumps are formed in batches in this way, the double-layer laminated film remaining on the wafer is removed using an organic solvent-based stripping liquid such as dimethyl sulfoxide (DMSO).

[0008] In recent years, the mounting density has been continuously improved. Therefore, the shape of the negative pattern (transfer mold) formed on the wafer in order to form the bump has gradually become more complicated (including three-dimensional). However, if a negative pattern of a complex shape is formed by using a double-layer laminated film as described above, the process becomes complicated. Therefore, the simplification of the manufacturing process is expected. In addition, it is required to effectively remove the material constituting the negative pattern remaining on the wafer after the bump is formed, but due to the increased concern for environmental issues, a material that can be removed using an aqueous stripping solution instead of an organic solvent-based stripping solution as described above is sought.

[0009] Furthermore, in recent high-density mounting technologies, fan-out type wafer level packaging (WLP) is used to form a redistribution layer in a large area exceeding the chip area, and a stack module is also realized in which the fan-out type WLP is stacked in multiple layers. In such fan-out type WLP, a large number of conductive columns including copper and the like are formed in the redistribution layer, and connection materials such as solder balls are arranged on the conductive columns. The arrangement accuracy of the connection materials needs to be higher as the mounting density increases, so it is required to arrange the connection materials on the conductive columns more accurately.

[0010] The object of the present invention is to provide an ionizing radiation-curable polymerizable composition sought with the development of such mounting technology, which can properly maintain the shape after curing even in a high temperature environment such as a reflow process (in this specification, the property is referred to as "having heat resistance"), and can be dissolved using a solvent containing water (in this specification, referred to as an "aqueous solvent"). In addition, the object of the present invention is also to provide an ink containing the polymerizable composition, a transfer mold containing an ionizing radiation-cured product obtained by irradiating the polymerizable composition with ionizing radiation, and a method for manufacturing an electrode member including an electrode group on a substrate using the polymerizable composition. Furthermore, in this specification, the so-called "ionizing radiation" refers to electromagnetic waves such as gamma rays, X-rays, ultraviolet rays, visible light, and electrons, as well as protons or ions, which are a general term for energy sources that can generate free radicals by being irradiated to a polymerization initiator or colliding with a polymerization initiator. In addition, in this specification, in order to indicate one or both of "acryloyl morpholine" and "methacryloyl morpholine", it is sometimes expressed as "(meth)acryloyl morpholine". The terms related to (meth)acryloylmorpholine, for example, "(meth)acrylate" and "(meth)acryloyloxy" also have the same meaning.

[0011] Technical means of solving problems

[0012] The present invention provided to solve the above-mentioned problems is as follows.

[0013] [1] A polymerizable composition comprising: (A) a first component comprising (meth)acryloylmorpholine represented by the following formula (1); and (B) a second component comprising a compound represented by the following formula (2), wherein the total content of the first component and the content of the second component in the solid content of the polymerizable composition is 50% by weight or more.

[0014]

[0015] In formula (1), R 1 is hydrogen or methyl. In formula (2), R 2 is hydrogen or a group having 1 to 6 carbon atoms, R 3 and R 4 Each independently represents hydrogen or a group having 20 or less carbon atoms; and n is an integer of 1-6.

[0016] [2] The polymerizable composition according to [1], wherein n in the compound represented by the formula (2) is 1.

[0017] [3] The polymerizable composition according to [2], wherein R in the compound represented by the formula (2) 3 and R 4 Each independently represents hydrogen or a group having 3 or less carbon atoms.

[0018] [4] The polymerizable composition according to [3], wherein R in the compound represented by the formula (2) 2 is hydrogen, R 3 and R 4 It is methyl.

[0019] [5] The polymerizable composition according to any one of [1] to [4], wherein the total content of the first component and the second component in the solid content of the polymerizable composition is 74% by weight or more.

[0020] [6] The polymerizable composition according to any one of [1] to [5], wherein the molar ratio of the first component to the second component in the polymerizable composition is 1 / 5 to 5 / 1 (first component / second component).

[0021] [7] The polymerizable composition according to any one of [1] to [6], further comprising (C) a third component, wherein the third component comprises a compound represented by the following formula (3).

[0022]

[0023] In formula (3), R 6 is a group having 25 or less carbon atoms, R 5and R 7 Each independently represents hydrogen or an alkyl group having 6 or less carbon atoms.

[0024] [8] The polymerizable composition according to [7], wherein R in the compound represented by the formula (3) 6 is a group containing an oxyalkylene group.

[0025] [9] The polymerizable composition according to [7], wherein R in the compound represented by the formula (3) 6 It is a group composed of oxyalkylene.

[0026]

[10] The polymerizable composition according to any one of [1] to [9], further comprising (D) a fourth component, wherein the fourth component includes a polymerization initiator, and the content of the fourth component in the solid content of the polymerizable composition is 5% by weight to 20% by weight.

[0027]

[11] The polymerizable composition according to any one of [1] to

[10] , further comprising (E) an antioxidant, wherein the content of the antioxidant in the solid content of the polymerizable composition is 0.01 wt% to 10 wt%.

[0028]

[12] The polymerizable composition according to any one of [1] to

[11] , wherein the viscosity at 25°C is 2 mPa·s to 30 mPa·s.

[0029]

[13] An ink for inkjet, comprising the polymerizable composition according to any one of [1] to

[12] .

[0030]

[14] A cured product obtained by photocuring the polymerizable composition according to any one of [1] to

[12] .

[0031]

[15] An electronic component made using the cured product according to

[14] .

[0032]

[16] A method for manufacturing an electrode component, wherein a plurality of electrodes are exposed with recessed portions on one side of an insulating substrate in which wiring is buried, the method comprising: a placement step of placing the polymerizable composition according to any one of [1] to

[12] on a substrate; a curing step of irradiating the polymerizable composition placed on the substrate with ionizing radiation to cure the polymerizable composition to obtain a transfer mold containing an ionizing radiation-cured material; a conductive member forming step of placing a conductive material so as to cover the transfer mold to form a conductive member; a peeling step of peeling a structure containing the transfer mold and the conductive member from the substrate to expose the plurality of conductive members corresponding to the plurality of electrodes together with a surface of the transfer mold attached to the conductive member on the substrate side; and a dissolving step of dissolving the transfer mold attached to each of the plurality of conductive members using an aqueous solution containing poly(oxyethylene)=alkyl ether to obtain the plurality of electrodes having the recessed portions having an inverse shape of the transfer mold.

[0033]

[17] The method for manufacturing an electrode component according to

[16] further includes a heating step of heating the transfer mold on the substrate after the hardening step and before the dissolving step.

[0034]

[18] A method for manufacturing an electrode component according to

[16] or

[17] , wherein, in the configuration step, the polymerizable composition is supplied to the substrate, thereby configuring a pattern of the coating of the polymerizable composition on the substrate, and in the curing step, the pattern of the coating of the polymerizable composition on the substrate is cured, thereby forming the pattern of the ionizing radiation cured product on the substrate as the transfer mold.

[0035]

[19] The method for manufacturing an electrode component according to

[18] , wherein the polymerizable composition is an inkjet ink, and in the configuration step, a pattern of a coating of the polymerizable composition is configured on the substrate using an inkjet printer.

[0036]

[20] A method for manufacturing an electrode component according to

[16] or

[17] , wherein, in the configuration step, a layer of the polymerizable composition is formed on the substrate, and in the curing step, a layer of the ionizing radiation cured material is formed from the layer of the polymerizable composition. The method for manufacturing an electrode component further includes a patterning step before the start of the conductive component forming step, wherein the patterning step irradiates a portion of the layer of the ionizing radiation cured material with high-energy rays to remove the ionizing radiation cured material, thereby forming a pattern of the ionizing radiation cured material on the substrate as the transfer mold.

[0037]

[21] A method for manufacturing an electrode component according to any one of

[16] to

[20] , wherein, in the conductive component forming step, a plurality of electrically independent patterns of the conductive components are formed on the substrate, and then the wiring electrically connected to each of the patterns of the plurality of conductive components is formed, and an insulating material is arranged around the patterns of the plurality of conductive components and the wiring to form the insulating substrate on the substrate, and in the stripping step, the structure stripped from the substrate includes the transfer mold and the insulating substrate.

[0038] Effects of the Invention

[0039] According to the present invention, there is provided a polymerizable composition that can form an ionizing radiation-cured product that can appropriately maintain its shape after curing even in a high-temperature environment (having heat resistance) and can be dissolved by an aqueous solvent. In addition, according to the present invention, there is provided an ink containing the polymerizable composition, an ionizing radiation-cured product obtained by irradiating the polymerizable composition with ionizing radiation, and a method for producing an electrode member including an electrode group on a substrate using the polymerizable composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a flowchart of the manufacturing method of this embodiment.

[0041] Figure 2 It is a diagram for explaining the steps from the arrangement step (step S101 ) to the hardening step (step S102 ).

[0042] Figure 3 It is a diagram for explaining the arrangement step (step S101 ), the curing step (step S102 ), and the patterning step (step S103 ).

[0043] Figure 4 It is a diagram for explaining the conductive member forming step (step S104 ), the peeling step (step S105 ), and the dissolving step (step S106 ).

[0044] [Explanation of Symbols]

[0045] 10: Polymerizable composition

[0046] 11: Pattern of coated article of polymerizable composition

[0047] 12: Layer of polymerizable composition

[0048] 12d: Unnecessary ionizing radiation hardening

[0049] 20: Pattern of ionizing radiation hardened material

[0050] 20S: Exposed side

[0051] 21: Layer of ionizing radiation hardened material

[0052] 30: Film of conductive component

[0053] 31: Pattern of conductive components

[0054] 31R: concave part

[0055] 32: Wiring components

[0056] 40, 41: Insulating materials

[0057] 42: Insulation

[0058] 50: Insulation substrate

[0059] 100: Electrode components

[0060] 200: Structure

[0061] LR: Ionizing radiation

[0062] LS: Irradiation device

[0063] PE: High Energy Line

[0064] PJ: Inkjet printer

[0065] PR: Offset printing press

[0066] PS: Screen printing machine

[0067] SB: Substrate

[0068] S101, S102, S103, S104, S105, S106, S107: Steps DETAILED DESCRIPTION

[0069] Hereinafter, a polymerizable composition, ink, ionizing radiation cured product, and method for producing an electrode member according to an embodiment of the present invention will be described.

[0070] A polymerizable composition according to one embodiment of the present invention is used to form a transfer mold, and includes: (A) a first component comprising (meth)acryloylmorpholine represented by the following formula (1); and (B) a second component represented by the following formula (2).

[0071]

[0072] In formula (1), R 1 is hydrogen or methyl. In formula (2), R 2 is hydrogen or a group having 1 to 6 carbon atoms (organic group), R 3 and R 4 Each independently represents hydrogen or a group having 20 or less carbon atoms; and n is an integer of 1-6.

[0073] The polymerizable composition contains (meth)acryloylmorpholine represented by formula (1) and the compound represented by formula (2), thereby ensuring curability and solubility of the ionizing radiation cured product in an aqueous solution and imparting appropriate heat resistance to the ionizing radiation cured product.

[0074] When the polymerizable composition is irradiated with ionizing radiation, the polymerization initiator generates radicals, which serve as a starting point for radical polymerization of the acryloyl groups contained in the polymerizable composition to form a solid component of the ionizing radiation-cured material. When light is used as the ionizing radiation, the polymerizable composition is a photocurable composition.

[0075] The polymerizable composition can ensure photocurability and heat resistance by containing the first and second components which are monofunctional compounds, and can also ensure solubility of the ionizing radiation-cured material in an aqueous solvent.

[0076] By setting the total content of the first component and the second component in the solid content of the polymerizable composition (the component that constitutes the ionizing radiation cured product among the components contained in the polymerizable composition) (hereinafter also referred to as "total content") to 50% by weight or more, the curability, the heat resistance of the ionizing radiation cured product, and the solubility in the aqueous solution can be improved. From the perspective of achieving curability, heat resistance and solubility in a good balance, the total content is more preferably 74% by weight or more, and further preferably 80% by weight or more. In addition, from the perspective of making the photocurability good, the total content is preferably 96% by weight or less, and more preferably 94% by weight or less. The content of the first component in the solid content of the polymerizable composition is preferably 25 to 75% by weight, and the content of the second component is preferably 15 to 65% by weight.

[0077] From the viewpoint of achieving an ionizing radiation-cured material having curability, heat resistance, and solubility in an aqueous solution, the molar ratio of the first component to the second component in the polymerizable composition is preferably 1 / 5 to 5 / 1, more preferably 1 / 3 to 3 / 1, and even more preferably 1 / 2 to 2 / 1.

[0078] From the viewpoint of more stably ensuring the solubility of the ionizing radiation-cured material in the aqueous solution, the second component is preferably a compound in which n in the formula (2) is 1, and more preferably a compound in which R in the formula (2) is 3 and R 4 are independently hydrogen or a group having 3 or less carbon atoms, and preferably R 2 is hydrogen, R 3 and R 4 A compound containing methyl.

[0079] Specific examples of preferred second components include N,N-dimethylacrylamide, N,N-diethylacrylamide, N,N-dimethylmethacrylamide, N-methylmethacrylamide, and N-methylacrylamide. In terms of being dissolved in an aqueous solution (aqueous stripping solution) containing a non-volatile water-soluble compound that is not a so-called volatile organic compound (VOC), N,N-dimethylacrylamide is particularly preferred. By setting the structure that the aqueous solution does not contain volatile organic compounds, the load on the environment can be further suppressed.

[0080] From the viewpoint of improving the residual film ratio of the ionizing radiation-cured product after a high-temperature process, the polymerizable composition preferably further contains a third component comprising a compound represented by formula (3).

[0081]

[0082] In formula (3), R 6 is a group having 25 or less carbon atoms, R 5 and R 7 Each independently represents hydrogen or an alkyl group having 6 or less carbon atoms.

[0083] Furthermore, the so-called residual film rate can be defined by (thickness after heat treatment) / (thickness before heat treatment) before and after the ionizing radiation cured material of this embodiment is heated in the atmosphere (for example, at 200°C for 2 hours, at 230°C for 2 hours, etc.). By increasing the residual film rate, even when a metal such as copper is directly formed on the pattern including the ionizing radiation cured material by a dry process such as evaporation or sputtering, the shape of the pattern is unlikely to change.

[0084] Specific examples of the third component comprising a compound represented by formula (3) include bisphenol F ethylene oxide-modified diacrylate (available as "Aronix M-208" manufactured by Toagosei Co., Ltd.), bisphenol A ethylene oxide-modified diacrylate (available as "Aronix M-211B" manufactured by Toagosei Co., Ltd.), PEG200# diacrylate (available as "Light Acrylate 4EG-A" manufactured by Kyoeisha Chemical Co., Ltd.), tripropylene glycol diacrylate (available as "Biscoat #310HP" manufactured by Osaka Organic Chemical Co., Ltd.), and 1,6-hexanediol diacrylate (available as "Light Acrylate 1,6-HXA" manufactured by Kyoeisha Chemical Co., Ltd.). Among these, from the viewpoint of the solubility of the ionizing radiation cured product in an aqueous solution, the compound represented by the above formula (3) is preferably 6 Bisphenol F ethylene oxide-modified diacrylate, bisphenol A ethylene oxide-modified diacrylate, PEG200# diacrylate, tripropylene glycol diacrylate, and R in the compound represented by the formula (3) are preferred in terms of improving solubility. 6 PEG200# diacrylate and tripropylene glycol diacrylate are groups composed of oxyalkylene.

[0085] In the polymerizable composition, a difunctional acrylate compound having, for example, an aliphatic polycyclic structure instead of a bisphenol structure may be used instead of the third component which is a monomer of the difunctional acrylate compound, within a range not impairing the solubility of the ionizing radiation cured product in the aqueous solvent.

[0086] When the polymerizable composition contains a third component, the content of the third component in the solid content is preferably 5% by weight to 35% by weight, more preferably 8% by weight to 33% by weight, and particularly preferably 10% by weight to 30% by weight, from the viewpoint of maintaining the residual film rate of the ionizing radiation cured product after high temperature treatment and the solubility of the ionizing radiation cured product in the aqueous solution.

[0087] The molar ratio of the third component to the total of the first component and the second component is preferably 1 / 20 to 1 / 2, more preferably 1 / 15 to 1 / 3, and even more preferably 1 / 10 to 1 / 5.

[0088] The polymerizable composition of the present invention may contain compounds other than the above as long as the heat resistance and solubility of the ionizing radiation cured product can be appropriately ensured. Examples of the acrylic compound positioned as an optional added component include monofunctional acrylic compounds having an aliphatic polycyclic structure such as a norbornene skeleton or a dicyclopentadiene skeleton (the acrylic compound is referred to as an "aliphatic polycyclic monoacrylic compound" in this specification). When the polymerizable composition contains an aliphatic polycyclic monoacrylic compound, the glass transition point of the ionizing radiation cured product formed from the polymerizable composition may be increased.

[0089] Specific examples of such aliphatic polycyclic monoacrylic acid compounds include dicyclopentyl methacrylate (available as "FA-513M" manufactured by Hitachi Chemical Co., Ltd.), dicyclopentyl acrylate (available as "FA-513AS" manufactured by Hitachi Chemical Co., Ltd.), isobornyl acrylate (available as "Light Ester IB-XA" manufactured by Kyoeisha Chemical Co., Ltd.), and isobornyl methacrylate (available as "Light Ester IB-X" manufactured by Kyoeisha Chemical Co., Ltd.). When the polymerizable composition contains the aliphatic polycyclic monoacrylic acid compound, the content of the aliphatic polycyclic monoacrylic acid compound is preferably 20% by weight or less, and more preferably 15% by weight or less, in the solid content of the polymerizable composition from the viewpoint of appropriately ensuring the heat resistance and solubility of the ionizing radiation cured product.

[0090] The polymerizable composition of the present invention may further contain (D) a fourth component comprising a polymerization initiator. The polymerization initiator is not limited in type as long as it can generate radicals upon irradiation with ionizing radiation and can initiate a polymerization reaction between the first component and the second component.

[0091] From the viewpoint of solubility of the ionizing radiation cured product, the content of the polymerization initiator in the solid content of the polymerizable composition is preferably 5% by weight or more, and from the viewpoint of heat resistance, it is preferably 20% by weight or less. From the viewpoint of obtaining an ionizing radiation cured product having solubility and heat resistance in a good balance, it is more preferably 8% by weight or more and 15% by weight or less.

[0092] Specific examples of the polymerization initiator include benzophenone, Michler's ketone, 4,4'-bis(diethylamino)benzophenone, xanthone, thioxanthone, isopropylxanthone, 2,4-diethylthioxanthone, 2-ethylanthraquinone, acetophenone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-2-methyl-4'-isopropylpropiophenone, 1-hydroxycyclohexylphenylketone, isopropylbenzoin ether, isobutylbenzoin ether, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1,1'-(methylene-di-4,1-phenylene)bis(2-hydroxy-2-methyl-1-propane), camphorquinone, benzanthrone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2- (4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl)-butan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,4-dimethylaminobenzoic acid ethyl ester, 4-dimethylaminobenzoic acid isopentyl ester, 4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4,4'-tri(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-(4'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2',4'-dimethyl s-triazine, 2-(2'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4'-pentyloxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 4-[p-N,N-bis(ethoxycarbonylmethyl)]-2,6-bis(trichloromethyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(2'-chlorophenyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(4'-methoxyphenyl)-s-triazine, 2-(p-dimethylaminophenylvinyl)benzoxazole, 2-(p-dimethylaminophenylvinyl)benzothiazole, 2-mercaptobenzothiazole, 3,3'-carbonylbis(trichloromethyl)-benzothiazole (7-diethylaminocoumarin), 2-(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetrakis(4-ethoxycarbonylphenyl)-1,2'-biimidazole, 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4-dibromophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 3-(2-methyl-2-dimethylaminopropionyl)carbazole, 3,6-bis(2-methyl-2-morpholinylpropionyl)-9-n-dodecylcarbazole, bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-hexylperoxycarbonyl)benzophenone, 3,3'-di(methoxycarbonyl)-4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4'-di(methoxycarbonyl)-4,3'-di(tert-butylperoxycarbonyl)benzophenone, 4,4'-di(methoxycarbonyl)-3,3'-di(tert-butylperoxycarbonyl)benzophenone, etc. These compounds may be used alone, or a mixture of two or more thereof may be used effectively. As commercially available products, for example, there are: BASF products: Irgacure 379EG, Irgacure 127, Irgacure 184, and IGM Resins B.V. products: Omnirad 379EG, Omnirad 127, Omnirad 184. Among these, 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl)butane-1-one is preferred.

[0093] From the perspective of simplifying the formation process of the ionizing radiation cured product, the polymerizable composition of the present embodiment may not substantially contain a volatile solvent, but from the perspective of adjusting the viscosity of the polymerizable composition, etc., it may also contain a volatile solvent. The volatile solvent can be mixed with other compositions to form a polymerizable composition when used. In the case where the polymerizable composition contains a volatile solvent, the volatile solvent can begin to volatilize in the uncured state of the polymerizable composition, preferably by heating appropriately before, during, and / or after the irradiation of ionizing radiation and at least volatilize in the stage of forming the ionizing radiation cured product. If the unvolatile solvent remains excessively in the state where the polymerizable composition has been cured to a certain extent, the final cured product (ionizing radiation cured product) has a porous structure, and there is a situation where the surface properties (surface smoothness) required as a reverse mold (negative pattern) for reverse transfer are reduced. Therefore, the content of the volatile solvent is preferably 30% by weight or less relative to the entire polymerizable composition.

[0094] Specific examples of the volatile solvent include methanol, ethanol, propanol, butanol, butyl acetate, butyl propionate, ethyl lactate, methyl oxyacetate, ethyl oxyacetate, butyl oxyacetate, methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, methyl 3-oxypropionate, ethyl 3-oxypropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl 2-oxypropionate, 2-oxypropionate, methyl 2-oxypropionate, ethyl ... ethyl ester, 2-oxypropionic acid propyl ester, 2-methoxypropionic acid methyl ester, 2-methoxypropionic acid ethyl ester, 2-methoxypropionic acid propyl ester, 2-ethoxypropionic acid methyl ester, 2-ethoxypropionic acid ethyl ester, 2-oxy-2-methylpropionic acid methyl ester, 2-oxy-2-methylpropionic acid ethyl ester, 2-methoxy-2-methylpropionic acid methyl ester, 2-ethoxy-2-methylpropionic acid ethyl ester, pyruvic acid methyl ester, pyruvic acid ethyl ester, pyruvic acid propyl ester, acetoacetic acid methyl ester, acetoacetic acid ethyl ester, 2-oxobutyric acid methyl ester, 2-oxobutyric acid ethyl ester, 2-hydroxyisobutyric acid Methyl ester, dioxane, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol monophenyl ether, ethylene glycol monobutyl ether, ethylene glycol monophenyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monophenyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monophenyl ether, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerine, benzyl alcohol, cyclohexanol, 1,4-butanediol, triethylene glycol Alcohol, tripropylene glycol, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monobutyl ether acetate, ethylene glycol monobutyl ether acetate, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, toluene, xylene, anisole, γ-butyrolactone, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and dimethylimidazolidinone. These compounds can be used alone or in combination of two or more.

[0095] The polymerizable composition of this embodiment may also contain ingredients other than the above-mentioned ingredients as other additives. Specific examples of other additives include: surfactants, polymerization inhibitors, plasticizers, antioxidants, ultraviolet absorbers, antistatic agents, flame retardants, flame retardant aids, fillers, pigments, dyes, etc., but there are no special limitations as long as they can be uniformly mixed with other ingredients without departing from the scope of the present invention. Specific examples of surfactants include: Polyflow No.45, Polyflow KL-245, Polyflow No.75, Polyflow No.90, Polyflow No.95 (trade names, all manufactured by Kyoeisha Chemical Co., Ltd.); Disperbyk 161, Disperbyk 162, Disperbyk 163, Disperbyk 16 4. Disperbyk 166, Disperbyk 170, Disperbyk 180, Disperbyk 181, Disperbyk 182, BYK 300, BYK 306, BYK 310, BYK 320, BYK 330, BYK 342, BYK 344, BYK 346 (trade names, all are BYK-Chemie Japan); KP-341, KP-358, KP-368, KF-96-50CS, KF-50-100CS (trade names, all manufactured by Shin-Etsu Chemical Co., Ltd.); Surflon SC-101, Surflon KH-40 (trade names, all manufactured by SEIMI Chemical Co., Ltd.); Ftergent 222F, Ftergent 251, FTX-218 (trade names, all manufactured by NEOS Co., Ltd.); TEGO Rad 2100, 2200N, 2250, 2500, 2600, 2700 (trade names, all manufactured by Evonik Degussa Co., Ltd.); EFTOP EF-351, EFTOP EF-352, EFTOP EF-601, EFTOP EF-801, EFTOP EF-802 (trade names, all manufactured by Mitsubishi Materials Corporation);Megafac F-171, Megafac F-177, Megafac F-444, Megafac F-475, Megafac F-477, Megafac F-556, Megafac R-08, Megafac R-30 (trade names, all manufactured by DIC Corporation); fluoroalkylbenzenesulfonates, fluoroalkylcarboxylates, fluoroalkylpolyoxyethylene ethers, fluoroalkylammonium iodides, fluoroalkylbetaines, fluoroalkylsulfonates, perfluoroalkylethylene oxide adducts, diglyceroltetra(fluoroalkylpolyoxyethylene ethers), fluoroalkyltrimethylammonium salts, fluoroalkyl aminosulfonates, polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, polyoxyethylene tridecyl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene laurate, polyoxyethylene oleate, polyoxyethylene stearate, polyoxyethylene laurylamine, sorbitan laurate, sorbitan palmitate, sorbitan stearate, sorbitan oleate, sorbitan fatty acid esters, polyoxyethylene sorbitan laurate, polyoxyethylene sorbitan palmitate, polyoxyethylene sorbitan stearate, polyoxyethylene sorbitan oleate, polyoxyethylene naphthyl ether, alkylbenzene sulfonates, and alkyl diphenyl ether disulfonates. ;

[0096] Specific examples of the polymerization inhibitor include 4-methoxyphenol, hydroquinone, and phenothiazine.

[0097] As the antioxidant, hindered phenol-based antioxidants, phosphorus-based processing heat stabilizers, metal deactivators, sulfur-based heat stabilizers, hydroquinone derivatives, and the like are preferred. Specific examples include Irganox 1010, Irganox 1010FF, Irganox 1035, Irganox 1035FF (W&C), Irganox 1076, Irganox 1076FD, Irganox 1098, Irganox 1135, Irganox 1330, Irganox 1520L, Irganox 245, Irganox 245FF, Irganox 259, and Irganox 260FF. Irganox 3114, Irganox 565 (trade names, both manufactured by BASF); NOCRAC 200, NOCRAC NS-6 (trade names, both manufactured by Ouchi Shinshin Chemical Industry Co., Ltd.); ADEKASTAB AO-40, ADEKASTAB AO-50, ADEKASTAB AO-60, ADEKASTAB AO-80, ADEKASTAB AO-330, ADEKASTAB HP-10, ADEKASTAB HP-11, ADEKASTAB HP-12, ADEKASTAB HP-13, ADEKASTAB HP-14, ADEKASTAB HP-15, ADEKASTAB HP-16, ADEKASTAB HP-17, ADEKASTAB HP-18, ADEKASTAB HP-20, ADEKASTAB HP-21, ADEKASTAB HP-23, ADEKASTAB HP-24, ADEKASTAB HP-25 ARC Luz) GPA5001 (trade name, all manufactured by ADEKA (co., Ltd.); Keminiox 101 (trade name, manufactured by Chemipro Kasei (co., Ltd.); Cyanox CY-1790 (trade name, manufactured by Sun Chemical (co., Ltd.); AntiOx 10 (trade name, manufactured by NOF (co., Ltd.)); butylated hydroxytoluene, 4-methoxyphenol, etc. Among them, Irganox 1330 (melting point: 240°C to 245°C) with a high melting point and low volatility is particularly preferred.

[0098] From the viewpoint of improving the solubility of the cured polymerizable composition, the content of the antioxidant is preferably 0.01 to 10 wt %, more preferably 0.1 to 5 wt %, and even more preferably 0.4 to 2 wt % based on the solid content of the polymerizable composition.

[0099] The polymerizable composition of the present embodiment is supplied to the substrate by coating, dripping, etc. when used, thereby having a film shape or a predetermined pattern on the substrate. From the viewpoint of improving the ease of supplying the polymerizable composition to the substrate in this way, there is a case where the viscosity of the polymerizable composition of the present embodiment at 25°C is preferably 2 to 30 mPa·s. In particular, when the polymerizable composition is supplied to the substrate with an inkjet printer, it is preferred to satisfy the viscosity range. Furthermore, the viscosity of the inkjet ink containing the polymerizable composition of the present embodiment at the ejection temperature (e.g., 25°C) is preferably 25 mPa·s or less, particularly preferably 10 mPa·s or less. Furthermore, the viscosity of the polymerizable composition can be reduced by heating.

[0100] The polymerizable composition of this embodiment is cured by irradiation with ionizing radiation and becomes an ionizing radiation cured product. The ionizing radiation cured product is soluble in an aqueous solution even after being heated at 200°C for 2 hours in the atmosphere. As a specific example, the ionizing radiation cured product after the heat treatment (200°C for 2 hours) is dissolved by immersion in an aqueous solution for 15 hours or less, and in a preferred embodiment, by immersion for 30 minutes or less.

[0101] The aqueous solution is a solution containing water, and may be composed of water, but preferably a mixed solvent with a water-soluble compound having high solubility in water. Any water-soluble compound can be used as long as it has a boiling point of 70°C or more, but in terms of easy handling, it is preferably a compound containing a boiling point of 150°C or more, and in terms of VOC, it is more preferably a compound containing a boiling point of 260°C or more.

[0102] As water-soluble compounds with high solubility in water, from the viewpoint of improving the uniformity of the mixed solution, there can be cited protic polar solvents such as alcohols, or compounds containing oxyethylene groups such as poly(oxyethylene)=alkyl ethers. From the viewpoint of safety and reducing environmental load, non-volatile poly(oxyethylene)=alkyl ethers are more preferred. The water content in the aqueous solution can be appropriately set according to the types of components other than water contained in the aqueous solution and the composition of the ionizing radiation cured product.

[0103] When the aqueous solution comprises a mixed solution of water and poly(oxyethylene)=alkyl ether, that is, a water-poly(oxyethylene)=alkyl ether mixed solution, the poly(oxyethylene)=alkyl ether (H 2m+1 C m -O-(CH 2 -CH 2 -O) nThe number of moles n of ethylene oxide added in the alkylene oxide-H) is not particularly limited, but is preferably 2 to 35, more preferably 15 to 30, and still more preferably 20 to 25. The alkyl chain length m is preferably 4 to 15, and more preferably 12 to 13.

[0104] Examples of the poly(oxyethylene)=alkyl ether include diethylene glycol butyl ether (CAS No: 112-34-5) having an addition mole number of ethylene oxide n=2, triethylene glycol monododecyl ether (CAS No: 3055-94-5) having an addition mole number of ethylene oxide n=3, and polyoxyethylene (23) lauryl ether (CAS No: 9002-92-0) having an addition mole number of ethylene oxide n=23. From the viewpoint of safety and reduction of environmental load, it is preferred to use polyoxyethylene (23) lauryl ether as the poly(oxyethylene)=alkyl ether, and the content thereof in the aqueous solution is preferably 10% by weight or more and 90% by weight or less, more preferably 30% by weight or more and 80% by weight or less, and particularly preferably 50% by weight or more and 70% by weight or less.

[0105] In the case where the aqueous solution includes a mixture of water and alcohol, i.e., a water-alcohol mixture, when the alcohol contained in the water-alcohol mixture includes a substance with a carbon number of less than 4 such as ethanol or isopropanol, the alcohol content is preferably from 25% by weight to 90% by weight, more preferably from 40% by weight to 80% by weight, and particularly preferably from 45% by weight to 75% by weight.

[0106] The aqueous solution may also contain an organic solvent other than alcohol. Examples of such organic solvents include aprotic organic solvents such as N-methylpyrrolidone, acetone, acetonitrile, and dimethyl sulfoxide. From the perspective of reducing environmental load, the content of the organic solvent other than alcohol in the aqueous solution is preferably less than 20% by weight of the entire aqueous solution.

[0107] The aqueous solution is preferably alkaline, i.e., an alkaline solution. As the substance used to make the aqueous solution alkaline, inorganic alkaline substances such as sodium hydroxide and potassium hydroxide or organic alkaline substances such as tetramethylammonium hydroxide can be exemplified. Furthermore, the pH of a general alkaline solution is above 9, and the pH of the aqueous solution is preferably above 9, and more preferably above 10. From the viewpoint of achieving such a pH, the content of the alkaline substance in the aqueous solution is preferably set to 5% by weight or more and 20% by weight or less.

[0108] Hereinafter, a method for manufacturing an electrode member in which a plurality of electrodes are exposed with recesses on one side of an insulating substrate in which wiring is buried, which can also be used as a re-distribution layer (RDL) used in a fan-out WLP, etc., will be described. The material constituting the electrode includes, for example, copper (Cu), and the material constituting the insulating substrate includes, for example, polyimide.

[0109] Figure 1 : is a flow chart of the manufacturing method of this embodiment. Figure 1 As shown, the manufacturing method includes a configuration step (step S101), a hardening step (step S102), a conductive member forming step (step S104), a stripping step (step S105) and a dissolving step (step S106) as necessary steps. The manufacturing method may include a patterning step (step S103) between the hardening step (step S102) and the conductive member forming step (step S104) as needed, and may also include a heating step (step S107) after the hardening step (step S102) and before the dissolving step (step S106) starts.

[0110] Figure 2 This is a diagram for explaining the steps from the arrangement step (step S101 ) to the hardening step (step S102 ) included in an example of the manufacturing method of the present embodiment.

[0111] In the arrangement step (step S101), a plate-shaped or sheet-shaped substrate SB ( Figure 2 The polymerizable composition 10 is disposed on one of the main surfaces of (a). The method for disposing the polymerizable composition 10 is not limited. Figure 2 In Figure 2 (b) shows an example in which a pattern 11 of a coating of a polymerizable composition is formed on a substrate SB using various known configuration units such as a screen printer PS (left side), an offset printer PR using a transfer roller (center), and an inkjet printer PJ (right side).

[0112] In the curing step, the pattern 11 of the coating material of the polymerizable composition disposed on the substrate SB is irradiated with ionizing radiation LR ( Figure 2 (c)), the pattern 11 of the coating of the polymerizable composition is cured, thereby obtaining a pattern 20 of the ionizing radiation cured product on the substrate SB as a transfer mold ( Figure 2(d)). The type of ionizing radiation LR is not particularly limited, and examples thereof include visible light, ultraviolet light, X-rays, gamma rays, electron beams, ion beams, and the like. The irradiation device LS can be appropriately set according to the type of ionizing radiation LR. Specific examples include light emitting diodes (LEDs), halogen lamps, radiation irradiation devices, electron beam irradiation devices, and ion beam generating sources. From the viewpoint of ease of acquisition or ease of handling, it is preferred to use ultraviolet light emitting diodes (UV-LEDs) or halogen lamps having a luminescence peak at about 350 nm to about 400 nm.

[0113] Figure 3 This is a diagram for explaining the arrangement step (step S101 ), the curing step (step S102 ), and the patterning step (step S103 ) included in another example of the manufacturing method of the present embodiment.

[0114] In the arrangement step (step S101), on one of the main surfaces ( Figure 3 (a)) Figure 3 The polymerizable composition layer 12 is formed as shown in (b). Examples of the method for forming the polymerizable composition layer 12 include spin coating, dipping, spray coating, and the like. Thereafter, a curing step (step S102) is performed. Figure 3 As shown in (c), a layer 21 of an ionizing radiation cured material is formed on one of the main surfaces of the substrate SB.

[0115] Thereafter, a portion of the ionizing radiation cured material layer 21 is irradiated with high energy rays PE (specifically, laser or ion beam) to remove unnecessary ionizing radiation cured material 12d. In this manner, a patterning step of forming a transfer mold including a pattern 20 of the ionizing radiation cured material on the substrate SB is performed (step S103).

[0116] Figure 4 It is a diagram for explaining a conductive member forming step (step S104 ), a peeling step (step S105 ), and a dissolving step (step S106 ) included in an example of the manufacturing method of the present embodiment.

[0117] In passing Figure 2 or Figure 3 After obtaining a structure having a pattern 20 of an ionizing radiation cured product formed on the substrate SB by the manufacturing process shown in the figure, a conductive member forming process (step S104) is performed to form a conductive member film 30 by arranging a conductive material so as to cover the pattern 20 of the ionizing radiation cured product on the substrate SB. Figure 4 In (a), as a specific example of the conductive member forming step (step S104), a case where a conductive material is uniformly arranged on one main surface of the substrate SB to form a film 30 of a film-like conductive member is shown.

[0118] The type of conductive material is not particularly limited. As long as the film 30 of the conductive member is water-impermeable and has the function of a protective layer of the pattern 20 of the ionizing radiation cured product, the degree of freedom in setting the subsequent process is increased, so it is preferred. From the above point of view, the conductive material can be exemplified by metal materials such as copper (Cu) and aluminum (Al); inorganic oxide materials such as indium-tin oxide (ITO) and zinc oxide (ZnO); conductive materials formed by dispersing conductive nanowires in resin, etc. The manufacturing method of the film 30 of the conductive member is appropriately set according to the type of the conductive material. When the conductive material is composed of a metal material such as copper (Cu), the following methods can be listed as specific examples: a method of forming the entire film 30 of the conductive component by a dry process such as evaporation or sputtering; a method of forming a thin layer of conductive material in a manner covering the pattern 20 of the ionizing radiation hardened material on the substrate SB by a dry process such as evaporation or sputtering, and then depositing the conductive material by a wet process such as plating to form the film 30 of the conductive component on the substrate SB, etc.

[0119] Furthermore, when the conductive material is deposited by a dry process, the conductive material facing the substrate SB may be at a high temperature or have high kinetic energy. In this case, the substrate SB is heated, and as a result, the pattern 20 of the ionizing radiation cured material on the substrate SB may also become high temperature. In this case, a heating process (step S107) is substantially performed in the conductive member forming process (step S104). Even in the case where the heating process (step S107) is substantially performed, as described above, the pattern 20 of the ionizing radiation cured material can be appropriately dissolved in the subsequent dissolution process using an aqueous solution containing poly(oxyethylene)=alkyl ether, and the shape change caused by heat is also small.

[0120] After the conductive member film 30 is formed on the substrate SB in this manner, a portion of the conductive member film 30 is removed by irradiating with high energy radiation such as laser light, thereby obtaining a conductive member pattern 31 ( Figure 4 (b)). In the above process, the irradiated high energy line may heat the substrate SB or the pattern 31 of the conductive member. In this case, a heating step (step S107) is sometimes substantially performed in the conductive member forming step (step S104). As described above, even if the pattern 20 of the ionizing radiation cured product is heated in this way, the solubility in the aqueous solution can be appropriately maintained and the shape change is not likely to occur.

[0121] Furthermore, in Figure 4 (a) and Figure 4In (b), the conductive member pattern 31 is formed after the conductive member film 30 is formed in the conductive member forming step (step S104), but the present invention is not limited thereto. The conductive member pattern 31 may be directly formed by using an appropriate mask material or the like.

[0122] Then, in order to further facilitate the stacking of the components on the pattern 31 of the conductive components provided on the substrate SB, as shown in FIG. Figure 4 As shown in (c) of the method, an insulating material 40 such as polyimide is arranged around the pattern 31 of the conductive component on the substrate SB. The specific method of the process is arbitrary. For example, it can be arranged by photolithography (including curing) in which the insulating material 40 is applied by spin coating or the like and then subjected to heat treatment. In the case described above, a heat treatment is performed, so that the pattern 20 of the ionizing radiation cured product covered by the pattern 31 of the conductive component in contact with the insulating material 40 is also heated. Therefore, the heat treatment is equivalent to the heating process (step S107) performed before the start of the stripping process (step S105) described below. As described above, even if the ionizing radiation cured product of this embodiment is heated, its solubility in the aqueous solution is not easily reduced, and it is not easy to produce a shape change caused by heating, so a heating process (step S107) for such a heat treatment can be implemented.

[0123] After the insulating material 40 is appropriately arranged around the pattern 31 of the conductive member, the conductive material is further stacked and patterned (the stacking and patterning may be performed simultaneously), thereby forming the wiring member 32 on the pattern 31 of the conductive member, and the insulating material 41 such as polyimide is arranged around the wiring member 32 ( Figure 4 (d)). There is also a case where a plurality of layers including the wiring member 32 and the insulating material 41 are provided. As described above, even if the process of forming the layer including the wiring member 32 and the insulating material 41 includes a heat treatment and is substantially implemented as a heating step (step S107), the ionizing radiation cured material appropriately maintains solubility in the aqueous solution and is not easily changed in shape by heating. In this way, the following structure 200 is arranged on the substrate SB: it includes a pattern 20 of the ionizing radiation cured material constituting the transfer mold, a pattern 31 of the conductive member constituting the electrode, a wiring member 32 constituting the wiring, and an insulating substrate 50 including an insulating portion 42 composed of the insulating material 40 and the insulating material 41.

[0124] The structure 200 thus obtained is turned over so that the substrate SB is located on the upper side of the structure 200 ( Figure 4(e)), the substrate SB is peeled off. At this time, the pattern 20 of the ionizing radiation cured material is in a state of being attached to the pattern 31 of the conductive member, that is, the transfer mold is attached to each of the plurality of conductive members, so that the surface 20S (the surface arranged opposite to the substrate SB) of the pattern 20 of the ionizing radiation cured material in the structure 200 is exposed ( Figure 4 (f)). The pattern 20 of the ionizing radiation cured material including the exposed surface 20S is brought into contact with an aqueous solution, so that the pattern 20 of the ionizing radiation cured material can be dissolved and removed. The result is as follows Figure 4 As shown in (g), the pattern 31 of the conductive member is exposed, and the pattern 31 of the conductive member has a surface of the concave portion 31R which is the reverse shape of the pattern 20 of the ionizing radiation cured product, and these patterns 31 of the conductive member respectively become electrodes of the electrode member. In this way, an electrode member 100 is obtained in which a plurality of electrodes (patterns 31 of the conductive member) are exposed with the concave portion 31R respectively on one side of the insulating substrate 50 in which the wiring (wiring member 32) is buried.

[0125] When the exposed portion of the electrode has the recess 31R, when the electrode member is used for redistribution, the recess 31R functions as a receiving portion for solder balls, thereby improving the stability of the solder balls placed therein. Therefore, the arrangement density of the electrodes in the redistribution can be increased, and the mounting density can be improved.

[0126] By the above manufacturing method, an electrode member can be manufactured in which each conductive member constituting the conductive member pattern 31 becomes an electrode, and the electrode and wiring electrically connected to the electrode are buried in the supporting member (including the insulating material 40 and the insulating material 41).

[0127] Although the present invention has been described with reference to the above-described embodiments, the present invention is not limited to the above-described embodiments, and improvements or changes may be made for the purpose of improvement or within the scope of the concept of the present invention.

[0128] Example

[0129] Hereinafter, the present invention will be described in more detail with reference to Examples and the like, but the scope of the present invention is not limited to these Examples and the like.

[0130] Prepare the following materials.

[0131] (A) First component: (meth)acryloylmorpholine

[0132] ACMO (acryloylmorpholine) (CAS No. 5117-12-4) acryloylmorpholine (Tg: 145°C)

[0133] (B) Second component

[0134] DMAA(N,N-dimethylacrylamide)(CAS No.2680-03-7)N,N-dimethylacrylamide(Tg:119℃)

[0135] DEAA (N,N-diethylacrylamide) (CAS No. 2675-94-7) N,N-diethylacrylamide (Tg: 81℃)

[0136] NIPA (N-isopropylacrylamide) (CAS No. 2210-25-5) Isopropylacrylamide (Tg: 150℃)

[0137] (C) Third component

[0138] 4EG-A (CAS No. 26570-48-9) PEG #200 diacrylate (Tg: 40°C)

[0139] M208 (CAS No.120750-67-6) Bisphenol F EO modified diacrylate (Tg: 75℃)

[0140] (Other compounds)

[0141] NVC (N-vinylcaprolactam) (CAS No. 2235-00-9) N-vinyl-ε-caprolactam (Tg: 145°C)

[0142] 4HBA (4-hydroxybutyl acrylate) (CAS No. 2478-10-6) 4-hydroxybutyl acrylate (Tg: -40℃)

[0143] (D) Fourth component: polymerization initiator

[0144] Irg379EG: 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl)butan-1-one (manufactured by BASF, "IRGACURE 379EG")

[0145] (E) Antioxidants

[0146] Irganox 1330 (manufactured by BASF)

[0147] (Surfactant)

[0148] BYK 342 (manufactured by BYK-Chemie Japan)

[0149] (Example 1 to Example 15 and Comparative Example 1 to Comparative Example 6)

[0150] Various materials were blended as shown in Tables 1 to 4 to prepare polymerizable compositions, wherein the numerical values ​​are parts by weight.

[0151] Table 1

[0152]

[0153] Table 2

[0154]

[0155] Table 3

[0156]

[0157] Table 4

[0158]

[0159] The content (solid content concentration) of each component contained in the polymerizable composition of the examples and comparative examples and the evaluation results are shown in Tables 5 to 8. In addition, in Tables 5 to 8, from the viewpoint of easy comparison, the total content of the first component (A) and the second component (B) in the solid content contained in the polymerizable composition is shown in the item (A) + (B), the molar ratio of each component is shown in the item of molar ratio (A / B / C / others), the first component / second component (molar ratio) is shown in the item of molar ratio (A / B), and the third component / (total of the first component and the second component) (molar ratio) is shown in the item of molar ratio [C / (A+B)]. In addition, % in Tables 5 to 8 means weight %.

[0160] Table 5

[0161]

[0162] -: Not determined

[0163] Table 6

[0164]

[0165] -: Not determined

[0166] Table 7

[0167]

[0168] -: Not determined

[0169] Table 8

[0170]

[0171] -: Not determined

[0172] (Evaluation Example 1) Measurement of Viscosity

[0173] The viscosity at room temperature (25° C.) was measured for each polymerizable composition of Examples and Comparative Examples. The measurement results are shown in Tables 5 to 8.

[0174] (Evaluation Example 2) Evaluation of Photocurability

[0175] For each polymerizable composition of Examples and Comparative Examples, a coating film was obtained using a bar coater under the following conditions: The exposure amount was changed and the minimum exposure amount required to make the coating film tackless was measured.

[0176] Substrate: Aluminum foil

[0177] Rod coater: #42 (target film thickness 70μm to 80μm)

[0178] The obtained coating film of the polymerizable composition was cured under the following conditions to obtain an ionizing radiation cured product.

[0179] UV irradiation device: ASM1503 NM-UV-LED manufactured by Asumi Giken

[0180] Lamp wavelength: 365nm

[0181] The photocurability of the polymerizable composition was evaluated based on the following criteria, based on the exposure amount required for curing the coating film.

[0182] ○: When the exposure is less than 100mJ / cm 2 Time hardening.

[0183] Δ: At an exposure of 100 mJ / cm 2 Above and less than 500mJ / cm 2 Time hardening.

[0184] ×: When the exposure is 500 mJ / cm 2 Above and less than 2000mJ / cm 2 Time hardening.

[0185] ××: At an exposure of 2000mJ / cm 2 Hardens when above.

[0186] (Evaluation Example 3) Evaluation of heat resistance (measurement of glass transition point (Tg))

[0187] For each polymerizable composition of Examples and Comparative Examples, a coating film was obtained using a bar coater under the following conditions.

[0188] Substrate: Aluminum foil

[0189] Rod coater: #42 (target film thickness 70μm to 80μm)

[0190] The coating film of the obtained polymerizable composition was cured under the following conditions to obtain an ionizing radiation cured product.

[0191] UV irradiation device: ASM1503 NM-UV-LED manufactured by Asumi Giken

[0192] Lamp wavelength: 365nm

[0193] Exposure: 1000mJ / cm 2

[0194] Illuminance: 700mW / cm 2

[0195] For the measurement of UV light, a UV monitor ("UV-Pad" manufactured by Opsytec) for measuring UVA (315 nm to 400 nm) was used.

[0196] The glass transition point (Tg) of the obtained ionizing radiation-cured product was measured by a dynamic viscoelasticity measurement method (dynamic mechanical analysis (DMA) method) under the following conditions.

[0197] Measuring device: DMS6000 (manufactured by Hitachi Hightech Science Corporation)

[0198] Frequency mode: Sine wave Frequency: 10kHz

[0199] Heating rate: 10℃ / min

[0200] Based on the measured glass transition point, the heat resistance of the polymerizable composition was evaluated according to the following criteria.

[0201] ◎: Glass transition point is 150°C or higher

[0202] ○: Glass transition point is 120°C or higher and less than 150°C

[0203] Δ: Glass transition point is 100°C or higher and less than 120°C

[0204] ×: Glass transition point is 50°C or higher and less than 100°C

[0205] ××: Glass transition point is less than 50°C

[0206] (Evaluation Example 4-1) Evaluation of solubility

[0207] Each polymerizable composition of the examples and comparative examples was applied on a silicon substrate (silicon wafer) and cured under the same conditions as in Evaluation Example 2 to obtain an ionizing radiation cured product. Subsequently, the obtained ionizing radiation cured product was subjected to heat treatment under the following conditions.

[0208] Clean oven: "DT610" manufactured by Yamato Scientific

[0209] Temperature: 200℃

[0210] Heating time: 2 hours

[0211] Next, (A) an alkaline solution (KOH / water / POE ether solution) containing a mixture of potassium hydroxide (KOH), water and polyoxyethylene (23) lauryl ether (POE ether) (mixing weight ratio: KOH / water / POE ether = 5 / 35 / 60) and (B) an alkaline solution (KOH / water / EtOH solution) containing a mixture of potassium hydroxide (KOH), water and ethanol (EtOH) (mixing weight ratio: KOH / water / EtOH = 5 / 35 / 60) were prepared as aqueous dissolving liquids, and the ionizing radiation cured product after heat treatment was immersed in the KOH / water / POE ether solution at 70°C and the KOH / water / EtOH solution at 25°C, and the dissolution state of the ionizing radiation cured product was observed. The evaluation criteria are as follows. The evaluation results are shown in Tables 5 to 8.

[0212] ◎: Dissolved within 30 minutes.

[0213] ○: Dissolved within 30 minutes to 3 hours.

[0214] Δ: Dissolved between 3 hours and 15 hours later.

[0215] ×: Not dissolved even after 15 hours.

[0216] (Evaluation Example 4-2) Evaluation of solubility

[0217] The dissolution state of the ionizing radiation cured product was observed in the same manner as in Evaluation Example 4-1 except that the heat treatment conditions of the obtained ionizing radiation cured product were changed to the following conditions and only KOH / water / POE ether solution was prepared as the aqueous solution of the ionizing radiation cured product after immersion heat treatment.

[0218] Clean oven: "DT610" manufactured by Yamato Scientific

[0219] Temperature: 230℃

[0220] Heating time: 2 hours

[0221] As shown in Tables 5 to 8, the polymerizable compositions of Examples had a viscosity of 10 mPa·s or less at room temperature, which is preferable as inkjet inks. In addition, all of them had good photocurability.

[0222] The glass transition point (Tg) of the ionizing radiation-cured material formed from the polymerizable composition of the example was 120° C. or higher, and it was confirmed that the glass transition point (Tg) of the obtained ionizing radiation-cured material was high.

[0223] The ionizing radiation-cured materials formed from the polymerizable compositions of the examples have good solubility in KOH / water / EtOH solutions even after heat treatment. Examples 1 to 3, 6 to 8, and 10 to 15 are soluble in KOH / water / POE ether solutions in addition to KOH / water / EtOH solutions, and have good light curing properties and heat resistance.

[0224] In contrast, the ionizing radiation-cured materials formed from the polymerizable compositions of Comparative Examples 1 to 6 tended to have a decreased solubility in the KOH / water / EtOH solution after heat treatment. Although Comparative Examples 2 and 5 were dissolved in the KOH / water / POE ether solution, either or both of the photocurability and the heat resistance were × or Δ.

[0225] According to the results of Examples 2, 10, and 11 to 13, the content of the polymerization initiator is preferably 5 wt % or more from the viewpoint of photocurability, and is preferably 20 wt % or less from the viewpoint of heat resistance.

[0226] By comparing Examples 6 and 8 with Comparative Example 5, it can be said that from the viewpoint of preparing a polymerizable composition having excellent photocurability, heat resistance and solubility, the total content of (A) and the content of (B) in the solid component of the polymerizable composition is preferably 50 wt % or more, more preferably 70 wt % or more.

[0227] When the polymerizable compositions of Example 6 without (E) antioxidant and Examples 14 and 15 containing (E) antioxidant were cured at 200°C in the order described above, the dissolution time in KOH / water / POE ether solution (70°C) was 4 hours, 1 hour, and 0.25 hours; the dissolution time in KOH / water / EtOH solution (25°C) was 1.5 hours, 0.5 hours, and 0.25 hours. In addition, when cured at 230°C, the dissolution time in KOH / water / POE ether solution (70°C) was × (insoluble), 2 hours, and 0.5 hours. Based on these results, it can be said that the solubility of the cured product relative to the aqueous solution is improved by the antioxidant, and the amount of the antioxidant is preferably 0.3% by weight, and more preferably 0.7% by weight or more.

Claims

1. An ink for inkjet, comprising a polymerizable composition, wherein the polymerizable composition comprises: (A) a first component comprising (meth)acryloylmorpholine represented by the following formula (1); and (B) a second component comprising a compound represented by the following formula (2), The total content of the first component and the second component in the solid content of the polymerizable composition is 50% by weight or more, In formula (1), R 1 is hydrogen or methyl; In formula (2), R 2 is hydrogen or a group having 1 to 6 carbon atoms, R 3 and R 4 Each independently represents a group having 20 or less carbon atoms, and n is an integer of 1-6.

2. The ink according to claim 1, wherein In the compound represented by the formula (2), n is 1.

3. The ink according to claim 2, wherein: In the compound represented by the formula (2), R 3 and R 4 Each independently is a group having 3 or less carbon atoms.

4. The ink according to claim 3, wherein In the compound represented by the formula (2), R 2 is hydrogen, R 3 and R 4 It is methyl.

5. The ink according to any one of claims 1 to 4, wherein The total of the content of the first component and the content of the second component in the solid content of the polymerizable composition is 74% by weight or more.

6. The ink according to any one of claims 1 to 4, wherein The molar ratio of the first component to the second component in the polymerizable composition is 1 / 5 to 5 / 1 in terms of first component / second component.

7. The ink according to any one of claims 1 to 4, further comprising (C) a third component, wherein the third component comprises a compound represented by the following formula (3): In formula (3), R 6 is a group having 25 or less carbon atoms, R 5 and R 7 Each independently represents hydrogen or an alkyl group having 6 or less carbon atoms.

8. The ink according to claim 7, wherein In the compound represented by the formula (3), R 6 is a group containing an oxyalkylene group.

9. The ink according to claim 7, wherein: In the compound represented by the formula (3), R 6 It is a group composed of oxyalkylene.

10. The ink according to any one of claims 1 to 4, further comprising (D) a fourth component, wherein the fourth component includes a polymerization initiator, and the content of the fourth component in the solid content of the polymerizable composition is 5% by weight to 20% by weight. 11 . The ink according to claim 1 , further comprising (E) an antioxidant, wherein a content of the antioxidant in the solid content of the polymerizable composition is 0.01% by weight to 10% by weight.

12. The ink according to any one of claims 1 to 4, wherein The viscosity at 25°C is 2 mPa·s to 30 mPa·s.

13. A cured product obtained by photocuring the ink according to any one of claims 1 to 12.

14. An electronic component manufactured using the hardened material according to claim 13.

15. A method for manufacturing an electrode component, wherein a plurality of electrodes are exposed with recessed portions on one side of an insulating substrate in which wiring is buried, the method comprising: A disposing step of disposing the ink according to any one of claims 1 to 12 on a substrate; a curing step of irradiating the ink disposed on the substrate with ionizing radiation to cure the ink and obtain a transfer mold including an ionizing radiation-cured product; a conductive member forming step of arranging a conductive material so as to cover the transfer mold to form a conductive member; a peeling step of peeling the structure including the transfer mold and the conductive member from the substrate so that the plurality of conductive members corresponding to the plurality of electrodes are exposed together with the surface of the transfer mold attached to the conductive member on the substrate side; as well as In the dissolving step, the transfer mold attached to each of the plurality of conductive members is dissolved using an aqueous solution containing polyoxyethylene alkyl ether to obtain the plurality of electrodes having the recessed portion having a reverse shape of the transfer mold. 16 . The method for manufacturing an electrode member according to claim 15 , further comprising a heating step of heating the transfer mold on the substrate after the hardening step and before the dissolving step.

17. The method for manufacturing an electrode member according to claim 15 or 16, wherein: In the arrangement step, the ink is supplied to the substrate, so that a pattern of the ink coating is arranged on the substrate. In the curing step, the pattern of the ink coating on the substrate is cured, so that the pattern of the ionizing radiation cured product is formed on the substrate as the transfer mold.

18. The method for manufacturing an electrode member according to claim 17, wherein: In the arrangement step, a pattern of the ink coating material is arranged on the substrate using an inkjet printer.

19. The method for manufacturing an electrode member according to claim 15 or 16, wherein: In the disposing step, a layer of the ink is formed on the substrate, In the curing step, the layer of the ionizing radiation cured material is formed from the layer of the ink. The manufacturing method of the electrode component also includes a patterning process before the conductive component forming process begins, wherein the patterning process irradiates a portion of the layer of the ionizing radiation hardened material with high-energy rays to remove the ionizing radiation hardened material, thereby forming the pattern of the ionizing radiation hardened material on the substrate as the transfer mold.

20. The method for manufacturing an electrode member according to claim 15 or 16, wherein: In the conductive component forming step, patterns of a plurality of electrically independent conductive components are formed on the substrate, and then the wiring electrically connected to each of the patterns of the plurality of conductive components is formed, and insulating material is arranged around the patterns of the plurality of conductive components and the wiring to form the insulating substrate on the substrate. In the stripping step, the structure stripped from the substrate includes the transfer mold and the insulating substrate.

Citation Information

Patent Citations

  • Resin composition, two-layer laminated film using the same and method for forming bump

    JP2007079550A

  • Active energy ray-curable resin composition and coating agent

    JP2012046687A

  • Active energy ray-curable nanocarbon dispersion, method for manufacturing the same, and active energy ray-curable coating agent using the same

    JP2014152080A

  • Active energy ray curable composition and cured article

    JP2019104867A

  • Polymerizable composition, ink, transfer matrix, and method for manufacturing electrode member