A copolymer cement admixture with conjugated ring-shaped high temperature resistance and preparation method thereof

By introducing quadcopolymer cement admixtures with conjugated ring structures, the problems of insufficient consistency and serious water loss under high temperature and high pressure of deep wells and deep sea wells are solved, and higher high temperature resistance and stability are achieved, ensuring oil and gas Effective closure of the layer.

CN115572342BActive Publication Date: 2024-11-29HUAIYIN INSTITUTE OF TECHNOLOGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211228186.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-09
Publication Date
2024-11-29
Estimated Expiration
2042-10-09

AI Technical Summary

Technical Problem

Existing polymer cement admixtures show insufficient consistency and serious water loss under high temperature and high pressure conditions in deep wells and deep sea wells, making it difficult to effectively fix and seal the oil and gas layer.

Method used

Using a quaternary copolymer cement admixture with a conjugated ring structure, the introduction of monomers such as sodium para-styrene sulfonate, sodium 4-vinylbenzoate, N-phenylacrylamide and vinylpyrrolidone was prepared by aqueous solution polymerization method. , enhance the high temperature resistance of the copolymer and maintain good hydration, salt resistance and shear resistance.

Benefits of technology

It significantly improves the high temperature resistance of cement slurry, reduces water loss, ensures stability and sealing effect under deep wells and deep sea wells, and improves the cementing performance under high temperature and high pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115572342B_ABST
    Figure CN115572342B_ABST
Patent Text Reader

Abstract

The invention discloses a copolymer cement admixture with conjugated cyclic high temperature resistance and a preparation method thereof. The invention prepares the copolymer cement admixture by introducing four vinyl monomers with high temperature resistance cyclic structures from the perspective of enhancing the conjugated rigidity of the monomers. The four monomers include sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenyl acrylamide and vinyl pyrrolidone. Compared with the traditional AMPS monomer, the four monomers not only maintain a series of functional groups with good hydration, salt resistance and shear resistance, such as sodium sulfonate group, amide group, imide group, sodium carbonate group, etc., but also improve the high temperature resistance of the copolymer by introducing conjugated structure phenyl and cyclic pyrrole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and relates to a polymer cement admixture, in particular to a copolymer cement admixture with conjugated ring-shaped high temperature resistance and a preparation method thereof. Background Art

[0002] The lack of energy is one of the common problems faced by most countries at present, especially oil resources. The exploitation of shallow oil has been widely used because the equipment and processes such as drilling and cementing are relatively simple. However, the supply of shallow oil has gradually failed to meet the needs of the country, and the shallow oil has been gradually exhausted, and it is also necessary to find a method for the exploitation of deep oil. In this case, it is urgent to improve the drilling and cementing technology of deep wells, ultra-deep wells, deep-sea wells and other oil resources. However, as the depth of the well increases, the temperature and pressure in the well become higher, and the cement slurry system used for cementing will lose water, settle, and fail to fix and seal the oil and gas layers under high temperature and high pressure conditions. The commonly used method is to add high-temperature and salt-resistant polymer admixtures to stabilize the performance of cement slurry.

[0003] Among them, 2-acrylamide-2-methylpropene sulfonic acid (AMPS, structure as shown in Formula 1) has been widely used as one of the synthetic monomers for preparing polymer cement admixtures due to its superior group properties. As can be seen from the structural diagram, AMPS has an unsaturated double bond that can be used for polymerization reactions, the end group of sodium sulfonate (–SO3Na) has good hydrophilicity, high charge density, and strong hydration ability. The two π bonds and three oxygen atoms in the sulfonate group share a negative charge, making it relatively stable and resistant to salt ions (such as K) in the external cement slurry. + 、Na + , Ca 2+ AMPS is insensitive to the attack of sulfonic acid, etc., which makes it have good salt resistance. In addition, the lone pair of electrons on the sulfonate group is also easy to adsorb with the cations in the cement slurry to form a dense spatial network structure, thereby increasing the water loss of cement. In addition, in addition to adsorption, the amide group (-CONH-) in AMPS also has a strong hydration effect. It increases the thickening of the hydration film by adsorbing cement particles and slows down the thickening process of cement. After polymerization, AMPS can form larger side groups, which effectively increase the steric hindrance and improve the rigidity of the molecular chain, thereby improving the high temperature resistance, salt resistance, shear resistance and other properties to a certain extent. Therefore, a series of copolymers based on AMPS were prepared and used in cement admixtures. Other copolymerized monomers often include acrylamide (AM), acrylic acid (AA), etc.

[0004]

[0005] Formula 1 Chemical structure of AMPS

[0006] However, the upper temperature limit of this series of copolymers is often limited to 200 o C, and is often used in shallow oil wells. Therefore, it is an important task to improve the heat resistance of copolymers by modifying the monomer structure itself, while maintaining the hydration, salt resistance, and shear resistance of various functional groups. This is of great strategic significance for the exploitation of deep wells and deep sea wells. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a copolymer cement admixture with a conjugated cyclic high temperature resistance effect. The copolymer of the present invention has good high temperature resistance. When used as a cementing polymer cement admixture, it can solve the problems of insufficient consistency and severe water loss in deep well and deep sea well cement slurry systems under high temperature and high pressure conditions; the present invention also provides a preparation method of the polymer.

[0008] The present invention is achieved through the following technical solutions:

[0009] A copolymer cement admixture with conjugated ring-shaped high temperature resistance has the following structural formula:

[0010]

[0011] In the formula, m+n+p+q is the number of repeating units, m, n, p, q are integers of 1-10000, and the weight average molecular weight of the copolymer is 10,000 g / mol-5,000,000 g / mol.

[0012] Preferably, m, n, p, and q are integers of 100-1000, and the weight average molecular weight of the copolymer is 100,000 g / mol-1,000,000 g / mol.

[0013] Preferably, m, n, p, and q are integers of 200-400, and the weight average molecular weight of the copolymer is 400,000 g / mol-600,000 g / mol.

[0014] A further improvement of the present invention is:

[0015] A method for preparing a copolymer cement admixture having a conjugated cyclic high temperature resistance effect comprises the following steps:

[0016] The monomers sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenyl acrylamide and vinyl pyrrolidone are dissolved in deionized water, stirred and ultrasonicated to form a uniform solution, and the pH value is adjusted to neutral with an alkaline solution; the obtained neutral solution is evacuated, nitrogen is passed through, and heated to 30-40 o C, add initiator, keep for 10-30 minutes, and continue to raise the temperature to 50-80 oC, react for 6-12 hours; after the reaction is completed, cool to room temperature, wash the solution with acetone to obtain a white precipitate, and vacuum dry to obtain a copolymer cement admixture with conjugated ring and high temperature resistance.

[0017] Furthermore, the molar ratio of sodium styrene sulfonate, sodium 4-vinyl benzoate, N-phenylacrylamide and vinyl pyrrolidone is (1-10): (1-10): (1-10): (1-10).

[0018] Furthermore, the total mass concentration of sodium styrene sulfonate, sodium 4-vinyl benzoate, N-phenylacrylamide and vinyl pyrrolidone in the uniform solution is 10%-30%.

[0019] Furthermore, the alkaline solution is a sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution.

[0020] Furthermore, the initiator is azobisisobutylimidazole hydrochloride.

[0021] Furthermore, the mass of the initiator is 1%-5% of the total mass of sodium styrene sulfonate, sodium 4-vinyl benzoate, N-phenylacrylamide and vinyl pyrrolidone.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention prepares a copolymer cement admixture by introducing four vinyl monomers with a high temperature resistant cyclic structure from the perspective of enhancing the conjugated rigidity of the monomers. The four monomers include sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenyl acrylamide and vinyl pyrrolidone, and their structures are shown below.

[0024] #timg# #timg# #timg# #timg# Sodium p-styrene sulfonate Sodium 4-vinyl benzoate N-phenylacrylamide Vinyl pyrrolidone

[0025] Compared with traditional AMPS monomers, these four monomers not only maintain a series of functional groups with good hydration, salt resistance and shear resistance, such as sodium sulfonate group, amide group, imide group, sodium carbonate group, etc., but also improve the high temperature resistance of the copolymer by introducing conjugated structure phenyl and cyclic pyrrole.

[0026] 2. The present invention introduces a series of hydrophilic, salt-resistant and shear-resistant functional groups such as sulfonate, carbonate and amide groups to ensure the water loss control performance of the copolymer in the cementing slurry system. The tetrapolymer of high-rigidity conjugated cyclic vinyl monomers prepared by the present invention has a high thermal decomposition temperature and has a high application value in high-temperature and high-pressure cementing devices such as deep wells and deep-sea wells. At the same time, the cyclic vinyl monomers selected by the present invention are easy to obtain, low in cost and pollution-free, and the aqueous solution copolymerization is simple and easy to operate, which is convenient for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the infrared spectrum of the tetrapolymer prepared in Example 1;

[0028] Figure 2 This is the thermal degradation curve of the tetrapolymer prepared in Example 1. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with specific embodiments.

[0030] Example 1

[0031] Four monomers, sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenyl acrylamide and vinyl pyrrolidone, were weighed in a molar ratio of 3:3:1:3, and then dissolved in deionized water to a mass concentration of 20%. The solution was stirred and ultrasonicated to form a uniform solution, and then the pH value was adjusted to neutral with an alkaline sodium hydroxide solution. The obtained neutral solution was evacuated, nitrogen was passed through, and heated to 40 o C, add the initiator, keep it for 20 minutes, and then continue to raise the temperature to 80 o C, react for 8 hours; after the reaction is completed, cool to room temperature, then wash the solution with acetone to obtain a white precipitate, and vacuum dry to obtain a copolymer cement admixture with conjugated ring and high temperature resistance; the mass of the initiator is 2% of the total mass of the four monomers; the initiator is azobisisobutylimidazole hydrochloride.

[0032] Example 2

[0033] The four monomers sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenyl acrylamide and vinyl pyrrolidone were weighed in a molar ratio of 3:2:2:3, and then dissolved in deionized water to a mass concentration of 20%, stirred and ultrasonicated to make a uniform solution, and then the pH value was adjusted to neutral with an alkaline sodium hydroxide solution; the obtained neutral solution was evacuated, nitrogen was passed through, and heated to 40 o C, add the initiator, keep it for 20 minutes, and then continue to raise the temperature to 80 o C, react for 8 hours; after the reaction is completed, cool to room temperature, then wash the solution with acetone to obtain a white precipitate, and vacuum dry to obtain a copolymer cement admixture with conjugated ring and high temperature resistance; the mass of the initiator is 2% of the total mass of the four monomers; the initiator is azobisisobutylimidazole hydrochloride.

[0034] Example 3

[0035] Four monomers, sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenylacrylamide and vinyl pyrrolidone, were weighed in a molar ratio of 3:3:2:2, and then dissolved in deionized water to a mass concentration of 20%. The solution was stirred and ultrasonicated to form a uniform solution, and then the pH value was adjusted to neutral with an alkaline sodium hydroxide solution. The obtained neutral solution was evacuated, nitrogen was passed through, and heated to 40 o C, add the initiator, keep it for 20 minutes, and then continue to raise the temperature to 80 o C, react for 8 hours; after the reaction is completed, cool to room temperature, then wash the solution with acetone to obtain a white precipitate, and vacuum dry to obtain a copolymer cement admixture with conjugated ring and high temperature resistance; the mass of the initiator is 2% of the total mass of the four monomers; the initiator is azobisisobutylimidazole hydrochloride.

[0036] Example 4

[0037] The four monomers sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenyl acrylamide and vinyl pyrrolidone were weighed in a molar ratio of 4:4:1:1, and then dissolved in deionized water to a mass concentration of 20%, stirred and ultrasonicated to make a uniform solution, and then the pH value was adjusted to neutral with alkaline sodium hydroxide solution; the obtained neutral solution was evacuated, nitrogen was passed through, and heated to 40 o C, add the initiator, keep it for 20 minutes, and then continue to raise the temperature to 80 o C, react for 8 hours; after the reaction is completed, cool to room temperature, then wash the solution with acetone to obtain a white precipitate, and vacuum dry to obtain a copolymer cement admixture with conjugated ring and high temperature resistance; the mass of the initiator is 2% of the total mass of the four monomers; the initiator is azobisisobutylimidazole hydrochloride.

[0038] The general structure formula of the tetrapolymers prepared in Examples 1 to 4 is as follows:

[0039]

[0040] Comparative Example 1

[0041] The three monomers 2-acrylamide-2-methylpropene sulfonic acid (AMPS), acrylic acid (AA), and acrylamide (AM) were weighed in a molar ratio of 4:3:3, and then dissolved in deionized water to a mass concentration of 20%. The solution was stirred and ultrasonicated to form a uniform solution, and then the pH value was adjusted to neutral with an alkaline sodium hydroxide solution. The obtained neutral solution was evacuated, nitrogen was passed through, and heated to 40 o C, add the initiator, keep it for 20 minutes, and then continue to raise the temperature to 80 oC, react for 8 hours; after the reaction is completed, cool to room temperature, then wash the solution with acetone to obtain a white precipitate, and vacuum dry it for standby use; the mass of the initiator is 2% of the total mass of the four monomers; the initiator is azobisisobutylimidazole hydrochloride.

[0042] The general structural formula of the terpolymer prepared in Comparative Example 1 is as follows.

[0043]

[0044] The present invention uses FTS3000 Fourier transform infrared spectrometer to analyze the functional groups of copolymers. Figure 1 : is the infrared spectrum of the tetrapolymer prepared in Example 1. Wave number 3429 cm -1 Represents the absorption peak of the stretching vibration of the NH bond in the amide; wave number 2929 cm -1 Represents the -CH2 stretching vibration absorption peak; wave number 1673 cm -1 Represents the stretching vibration peak of the C=O bond in -CONH2; wave number 1400-1600 cm -1 Represents the characteristic peaks of cyclic phenyl and pyrrole vibration; wave number 1555 cm -1 Represents the absorption peak of the stretching vibration of the CN bond in pyrrole; wave number 1300 cm -1 Represents the characteristic vibration peak of carbonate group; wave number 1223 cm -1 Represents the stretching vibration absorption peak of CN in amide; wave number 1040 cm -1 It represents the stretching vibration absorption peak of S=O in the sulfonate group.

[0045] The present invention uses a TGA-50 thermogravimetric analyzer to test the heat resistance of the copolymer. Figure 2 This is the thermal degradation curve of the quaternary copolymer prepared in Example 1. When the temperature is less than 300°C, the mass percentage of the sample does not change significantly, and the material degrades by less than 5% near 300°C. When the temperature reaches around 400°C, the material degrades by only about 10%. As the temperature continues to rise, the material degradation rate accelerates until the polymer loses its water loss reduction function completely. The copolymers prepared in the present invention all select the temperature at which the material degrades to 5% as their thermal decomposition temperature. Figure 2 It can be seen that the temperature at which the mass of the tetrapolymer prepared in Example 1 decreases by 5% is about 325°C.

[0046] The present invention adopts a TG-71 high temperature and high pressure fluid loss reducer to characterize the fluid loss reduction performance of the copolymer-doped cement slurry. The prepared copolymer admixtures are respectively added to the G-grade oil well cement to prepare slurry, and then the cement slurry is placed in a thickener device for curing for 30 minutes at a set temperature. The cured slurry is placed in an intelligent high temperature and high pressure fluid loss reducer, a pressure of 6.9 MPa is applied to the top of the instrument, a beaker is placed at the bottom water outlet valve, the water outlet valve is opened, the timing is started, and the volume of the solution in the beaker in 30 minutes is calculated, which is the standard fluid loss reduction.

[0047] The comparison results are as follows:

[0048] Thermal decomposition temperature / ℃ Water loss reduction / mL Example 1 325 52 Example 2 315 48 Example 3 310 42 Example 4 350 35 Comparative Example 1 230 86

[0049] The present invention introduces conjugated phenyl and cyclic structure into vinyl monomers, and prepares a new type of high temperature resistant tetrapolymer cement admixture through a simple and efficient aqueous solution polymerization method. Studies have shown that the introduction of cyclic phenyl and pyrrole improves the thermal performance of the polymer admixture to above 300 °C. At the same time, the presence of important water loss reducing, salt resistance, and shear resistance groups such as sulfonate, carbonate, and amide further improves the material's control over the water loss performance of cement slurry.

Claims

1. A copolymer cement admixture having a conjugated cyclic high temperature resistant effect, characterized in that: It has the following structural formula: ; In the formula, m+n+p+q is the number of repeating units, and m, n, p, and q are integers of 100-1000, and the weight average molecular weight of the copolymer is 100,000 g / mol-1,000,000 g / mol.

2. The copolymer cement admixture having a conjugated cyclic high temperature resistance according to claim 1, characterized in that: The m, n, p, and q are integers of 200-400, and the weight average molecular weight of the copolymer is 400,000 g / mol-600,000 g / mol.

3. A method for preparing a copolymer cement admixture having a conjugated cyclic high temperature resistance as claimed in claim 1, characterized in that: The following steps are involved: The monomers sodium p-styrene sulfonate, sodium 4-vinyl benzoate, N-phenyl acrylamide and vinyl pyrrolidone are dissolved in deionized water, stirred and ultrasonicated to form a uniform solution, and the pH value is adjusted to neutral with an alkaline solution; the obtained neutral solution is evacuated, nitrogen is passed through, and heated to 30-40 o C, add initiator, keep for 10-30 minutes, and continue to raise the temperature to 50-80 o C, react for 6-12 hours; after the reaction is completed, cool to room temperature, wash the solution with acetone to obtain a white precipitate, and vacuum dry to obtain a copolymer cement admixture with conjugated ring and high temperature resistance.

4. The method for preparing a copolymer cement admixture having a conjugated cyclic high temperature resistant effect according to claim 3, characterized in that: The molar ratio of sodium styrene sulfonate, sodium 4-vinyl benzoate, N-phenylacrylamide and vinyl pyrrolidone is (1-10): (1-10): (1-10): (1-10).

5. The method for preparing a copolymer cement admixture having a conjugated cyclic high temperature resistant effect according to claim 3, characterized in that: The total mass concentration of sodium styrene sulfonate, sodium 4-vinyl benzoate, N-phenylacrylamide and vinyl pyrrolidone in the uniform solution is 10%-30%.

6. The method for preparing a copolymer cement admixture having a conjugated cyclic high temperature resistance according to claim 3, characterized in that: The alkaline solution is a sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution.

7. The method for preparing a copolymer cement admixture having a conjugated cyclic high temperature resistance according to claim 3, characterized in that: The initiator is azobisisobutylimidazole hydrochloride.

8. A method for preparing a conjugated cyclic high temperature resistant copolymer cement admixture according to any one of claims 3 or 7, characterized in that: The mass of the initiator is 1%-5% of the total mass of sodium styrene sulfonate, sodium 4-vinyl benzoate, N-phenylacrylamide and vinyl pyrrolidone.

Citation Information

Patent Citations

  • Filtration-reducing agent for synthetic polymer oil-well cement

    CN102127406A

  • High-temperature-resistant and salt-resistant fluid loss agent and preparation method therefor

    CN105441040A

  • Fluid loss additive for oil well cement as well as preparation method and application of agent