A low-cost and high-efficiency production process for high-strength 7 series aluminum alloy

By adopting alloy composition ratio, uniform heat treatment, extrusion, cooling and stretching in the production of high-strength 7 series aluminum alloys, combined with rapid cooling of standing wave water cooling devices, the problems of difficult extrusion and long production cycle are solved and achieved The efficient and low-cost production process improves the mechanical properties of aluminum alloy products.

CN115582446BActive Publication Date: 2024-10-29SHANDONG NANSHAN ALUMINUM
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211094112.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-08
Publication Date
2024-10-29
Estimated Expiration
2042-09-08

AI Technical Summary

Technical Problem

High-strength 7-series aluminum alloys have high deformation resistance during the extrusion process, which results in difficult extrusion and low production efficiency. In addition, the offline quenching process in the traditional technical route causes high production costs and long production cycles.

Method used

The alloy composition ratio, round ingot uniform heat treatment, extrusion treatment, cooling treatment, stretching treatment and artificial aging process are adopted, and a standing wave water cooling device and a water penetration cooling device are installed at the outlet of the front beam of the extruder for rapid cooling. Stretching treatment to reduce residual stress and replace the traditional offline quenching process.

Benefits of technology

Effectively reduce production costs and shorten production cycles. The obtained aluminum alloy extrusion products have a tensile strength of ≥570MPa, a yield strength of ≥515MPa, and an elongation of ≥7%. The production costs are reduced by 5-8% and the production efficiency is improved by 5%. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003838284250000061
    Figure BDA0003838284250000061
  • Figure BDA0003838284250000071
    Figure BDA0003838284250000071
  • Figure BDA0003838284250000081
    Figure BDA0003838284250000081
Patent Text Reader

Abstract

The present invention provides a low-cost and high-efficiency production process for high-strength 7-series aluminum alloy, the main processes of which are: alloy component ratio, uniform heat treatment of round ingots, extrusion treatment, cooling treatment, stretching treatment, and artificial aging; wherein the cooling treatment is: installing a standing wave water cooling device and a water-penetrating cooling device at the outlet of the front beam of the extruder, so that the length of the extruded aluminum alloy product in the water is ≥2.0m. The use of this production process can effectively reduce production costs and shorten production cycles; the tensile strength of the obtained aluminum alloy extruded products is ≥570MPa, the yield strength is ≥515MPa, and the elongation is ≥7%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum extrusion material production, and in particular to a low-cost and high-efficiency production process for high-strength 7 series aluminum alloy. Background Art

[0002] The main alloying elements of high-strength 7 series aluminum alloys are Zn, Mg and Cu. This series of aluminum alloys are widely used in aerospace and industrial fields after extrusion, heat treatment and machining due to their low density, good formability and high specific strength. When this type of alloy is used in the aerospace field, there are strict requirements on the comprehensive performance of corrosion and strength, so the over-aging process is usually used for production; when used in general industrial fields, there are no special requirements for corrosion performance, so the peak aging state T6 or T6511 state is usually used.

[0003] The high-strength 7 series aluminum alloy has a high deformation resistance during the extrusion process, resulting in problems such as great extrusion difficulty and low production efficiency. At present, the traditional technical route is: after extrusion, use a heat treatment furnace for solid solution heat treatment and artificial aging treatment to a state with corresponding performance; and for products for general industrial use, because there are no special corrosion performance requirements, therefore, the traditional technology produces products with excess quality, and the offline quenching process is used in the traditional technical route, resulting in technical disadvantages of high production costs and long production cycles.

[0004] It can be seen that for general industrial 7 series aluminum alloys, it is of great significance to provide a production process with low cost and short production cycle. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a low-cost and high-efficiency production process for high-strength 7 series aluminum alloy, including alloy component ratio, uniform heat treatment of round ingots, extrusion treatment, cooling treatment, stretching treatment, and artificial aging; the use of this production process can effectively reduce production costs and shorten production cycles; the obtained aluminum alloy extruded products have a tensile strength of ≥570MPa, a yield strength of ≥515MPa, and an elongation of ≥7%.

[0006] The technical solution of the present invention is as follows:

[0007] A low-cost and high-efficiency production process for high-strength 7 series aluminum alloy, the main processes of which are: alloy component proportioning, round ingot uniform heat treatment, extrusion treatment, cooling treatment, stretching treatment, and artificial aging;

[0008] Among them, the cooling treatment is: installing a standing wave water cooling device and a water-penetrating cooling device at the outlet of the front beam of the extruder, so that the length of the extruded aluminum alloy product in the water is ≥2.0m; this setting can cool the extruded aluminum alloy product to room temperature in a short time; the standing wave water cooling device can increase the water level to form a water wall; the water-penetrating cooling device is to allow the product to pass through the water wall for cooling.

[0009] Furthermore, the above-mentioned high-strength 7 series aluminum alloy low-cost and high-efficiency production process has the following specific process:

[0010] (1) Alloy composition ratio:

[0011] A round ingot is selected as the raw material, and the round ingot includes the following elements in percentage by weight:

[0012] Si 0.05-0.50%, Fe 0.13-0.60%, Cu 1.80-2.60%, Mn≤0.30%, Mg 1.90-2.70%, Cr 0.15-0.25%, Zn 5.00-5.80%, Ti 0.04-0.10%, the balance is A1 and unavoidable impurities; the single content of unavoidable impurities shall not exceed 0.05%, and the total content shall not exceed 0.15%;

[0013] (2) Uniform heat treatment of round ingots:

[0014] During the homogenization heat treatment process, the heating rate is ≤35℃ / hour, the first-level insulation temperature is 430-440℃, and the insulation time is 8-12 hours; the second-level insulation temperature is 465-478℃, and the insulation time is 20-26 hours; after the second-level insulation is completed, air-cooling is performed to below 250℃;

[0015] (3) Extrusion treatment:

[0016] s1, design of extrusion die:

[0017] Adopt reverse extrusion die, die working band 1.5-5.0mm;

[0018] s2, the extrusion process is as follows:

[0019] Using reverse extrusion, the temperature of the mold is 370-410℃, the temperature of the extrusion barrel is 370-410℃, the temperature of the round ingot before extrusion is 365-400℃; the product extrusion speed is 1.30-2.00m / min; the metal surface temperature before entering the cooling water is 410-450℃;

[0020] (4) Cooling treatment:

[0021] A standing wave water cooling device and a water-penetrating cooling device are installed at the outlet of the front beam of the extruder, so that the length of the extruded aluminum alloy product in the water is ≥2.0m; this setting can cool the extruded aluminum alloy product to room temperature in a short time;

[0022] (5) Stretching treatment:

[0023] The cooled product is passed through a stretching machine to produce a tensile deformation of 1.20-2.50% to reduce the residual stress inside the product;

[0024] (6) Artificial aging:

[0025] The stretched product is artificially aged at a holding temperature of 115135°C for 2430 hours.

[0026] Preferably, in step (2), the heating rate is 28°C / hour, the first-level insulation temperature is 435°C, and the insulation time is 8 hours; the second-level insulation temperature is 465°C, and the insulation time is 24 hours; after the second-level insulation is completed, air cooling is performed to below 250°C.

[0027] Preferably, in step (2), the air volume during the air cooling process is determined based on whether the round ingot generates cooling cracks; and the start time of heat preservation is based on the metal surface temperature reaching a certain temperature.

[0028] Preferably, in step (3) s2, a reverse extrusion method is adopted, the temperature of the mold is 400°C, the temperature of the extrusion barrel is 384-392°C, the temperature of the round ingot before extrusion is 365-373°C; the product extrusion speed is 1.30-1.70m / min; and the metal surface temperature before entering the cooling water is 416-428°C.

[0029] Preferably, during the cooling process of step (4), the water temperature of the standing wave water cooling device and the water-penetrating cooling device are both ≤80°C.

[0030] Preferably, during the stretching treatment in step (5), the cooled product is subjected to a 1.8% stretching deformation by a stretching machine within 4 hours to eliminate the straightness difference and residual stress caused by the traction and cooling deformation to the greatest extent.

[0031] Preferably, during the artificial aging process in step (6), the holding temperature is 121±5° C. and the holding time is 24 hours, which can maximize the precipitation strengthening potential of the material.

[0032] Compared with the prior art, the beneficial effects of the present invention are:

[0033] 1. In the present invention, by controlling the alloy composition ratio, controlling the homogenization heat treatment process of the round ingot for extrusion, designing the extrusion process, designing the cooling device, and designing a unique artificial aging treatment, an aluminum alloy extrusion product with high tensile strength, high yield strength, and elongation ≥7% can be obtained.

[0034] 2. Compared with the traditional solution heat treatment technology in a heat treatment furnace, the production process provided by the present invention reduces the cost by 5-8% and increases the production efficiency of the entire production technology process by 5%.

[0035] 3. The production process provided by the present invention uses a cooling device for cooling treatment, replacing the traditional off-line quenching process, thereby effectively reducing production costs. DETAILED DESCRIPTION

[0036] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0037] Example 1

[0038] A low-cost and high-efficiency production process for high-strength 7 series aluminum alloy, the specific process is as follows:

[0039] (1) Alloy composition ratio:

[0040] A round ingot with a diameter of 320 mm was selected as the raw material, and a direct reading spectrometer was used to detect the alloy composition of the round ingot for extrusion. The element composition of the round ingot is as follows:

[0041] Si 0.10%, Fe 0.14%, Cu 1.9%, Mn 0.04%, Mg 2.6%, Cr 0.2%, Zn 5.5%, Ti0.06%, the balance is Al and unavoidable impurities; the single content of unavoidable impurities shall not exceed 0.05%, and the total content shall not exceed 0.15%;

[0042] (2) Uniform heat treatment of round ingots:

[0043] The round ingot of step (1) is subjected to homogenization heat treatment: the heating rate is 28°C / hour, the first-level insulation temperature is 435°C, and the insulation time is 8 hours; the second-level insulation temperature is 465°C, and the insulation time is 24 hours; after the second-level insulation is completed, it is air-cooled to below 250°C;

[0044] (3) Extrusion treatment:

[0045] s1, design of extrusion die:

[0046] Adopt reverse extrusion die, die working belt 3.0mm;

[0047] s2, the extrusion process is as follows:

[0048] The extrusion barrel diameter of the extruder is selected to be 330 mm, and the die is a double-hole die, so that the extrusion ratio is 21.78;

[0049] Using reverse extrusion, the temperature of the mold is 400℃, the temperature of the extrusion barrel is 384-392℃, the temperature of the round ingot before extrusion is 365-373℃; the product extrusion speed is 1.30-1.70m / min; the metal surface temperature before entering the cooling water is 416-428℃;

[0050] (4) Cooling treatment:

[0051] A standing wave water cooling device and a water-penetrating cooling device are installed at the exit of the front beam of the extruder, and the length of the extruded aluminum alloy product in the water is controlled to be ≥2.0m. The water temperature of the standing wave water cooling device and the water-penetrating cooling device are both 60-70℃, so that the surface temperature of the product after cooling is 20.0-27.0℃; this setting can cool the extruded aluminum alloy product to room temperature in a short time;

[0052] (5) Stretching treatment:

[0053] The cooled product is stretched by a stretching machine within 4 hours to produce 1.8% tensile deformation, so as to eliminate the straightness difference and residual stress caused by traction and cooling deformation to the greatest extent;

[0054] (6) Artificial aging:

[0055] The stretched product is artificially aged at a holding temperature of 121±5°C for 24 hours.

[0056] The room temperature tensile properties test was carried out on the aged 7 series alloy samples, and the results are shown in Table 1;

[0057] Table 1 Room temperature tensile properties of 7 series bars (diameter 50 mm) after aging

[0058]

[0059] It can be seen from the test data that the high-strength 7 series 50mm diameter rod produced by the process of the present invention can have a T6 state room temperature tensile strength of more than 600MPa, which is more than 30MPa higher than the standard value in the industry.

[0060] Example 2

[0061] A low-cost and high-efficiency production process for high-strength 7 series aluminum alloy, the specific process is as follows:

[0062] (1) Alloy composition ratio:

[0063] A round ingot with a diameter of 146 mm was selected as the raw material, and a direct reading spectrometer was used to detect the alloy composition of the round ingot for extrusion. The element composition of the round ingot is as follows:

[0064] Si 0.06%, Fe 0.18%, Cu 1.9%, Mn 0.02%, Mg 2.6%, Cr 0.25%, Zn 5.6%, Ti0.05%, the balance is Al and unavoidable impurities; the single content of unavoidable impurities shall not exceed 0.05%, and the total content shall not exceed 0.15%;

[0065] (2) Uniform heat treatment of round ingots:

[0066] The round ingot of step (1) is subjected to homogenization heat treatment: the heating rate is 35°C / hour, the first-level insulation temperature is 435°C, and the insulation time is 8 hours; the second-level insulation temperature is 465°C, and the insulation time is 24 hours; after the second-level insulation is completed, it is air-cooled to below 250°C;

[0067] (3) Extrusion treatment:

[0068] s1, design of extrusion die:

[0069] Adopt reverse extrusion die, die working belt 3.0mm;

[0070] s2, the extrusion process is as follows:

[0071] The special-shaped solid profile has a weight of 0.97kg / m. The extrusion barrel diameter of the extruder is selected to be 151mm, and the mold adopts a single-hole mold, so that the extrusion ratio is 51.7; the special-shaped solid profile is made by designing the section and manufacturing a mold with the cross-sectional shape of the profile, and the heated round cast rod is extruded from the mold by the extruder;

[0072] The reverse extrusion method is adopted, the mold heating temperature is 420℃, the extrusion barrel temperature is 395-407℃, the round ingot temperature before extrusion is 398-405℃; the product extrusion speed is 1.30-1.70m / min; the metal surface temperature before entering the cooling water is 424-430℃;

[0073] (4) Cooling treatment:

[0074] A standing wave water cooling device and a water-penetrating cooling device are installed at the exit of the front beam of the extruder, and the length of the extruded aluminum alloy product in the water is controlled to be ≥2.0m. The water temperature of the standing wave water cooling device and the water-penetrating cooling device are both 60-70℃, so that the surface temperature of the product after cooling is 18.0-23.0℃; this setting can cool the extruded aluminum alloy product to room temperature in a short time;

[0075] (5) Stretching treatment:

[0076] The cooled product is stretched by 2.2% in a stretching machine within 4 hours to eliminate the straightness difference and residual stress caused by traction and cooling deformation to the greatest extent;

[0077] (6) Artificial aging:

[0078] The stretched product is artificially aged at a holding temperature of 121±5°C for 24 hours.

[0079] The room temperature tensile properties test was carried out on the aged 7 series alloy samples, and the results are shown in Table 2;

[0080] Table 2 Room temperature tensile properties of 7 series profiles after aging

[0081]

[0082]

[0083] It can be seen from the test data that the process of the present invention is used to produce high-strength 7 series solid special-shaped materials with a meter weight of 0.97 kg / m, and the T6 state room temperature tensile strength is more than 50 MPa higher than the standard value in the industry.

[0084] Example 3

[0085] A low-cost and high-efficiency production process for high-strength 7 series aluminum alloy, the specific process is as follows:

[0086] (1) Alloy composition ratio:

[0087] A round ingot with a diameter of 410 mm was selected as the raw material, and a direct reading spectrometer was used to detect the alloy composition of the round ingot for extrusion. The element composition of the round ingot is as follows:

[0088] Si 0.1%, Fe 0.25%, Cu 1.85%, Mn 0.12%, Mg 2.4%, Cr 0.24%, Zn 5.2%, Ti0.07%, the balance is Al and unavoidable impurities; the single content of unavoidable impurities shall not exceed 0.05%, and the total content shall not exceed 0.15%;

[0089] (2) Uniform heat treatment of round ingots:

[0090] The round ingot of step (1) is subjected to homogenization heat treatment: the heating rate is 35°C / hour, the first-level insulation temperature is 435°C, and the insulation time is 8 hours; the second-level insulation temperature is 465°C, and the insulation time is 24 hours; after the second-level insulation is completed, it is air-cooled to below 250°C;

[0091] (3) Extrusion treatment:

[0092] s1, design of extrusion die:

[0093] Adopt reverse extrusion die, die working belt 3.0mm;

[0094] s2, the extrusion process is as follows:

[0095] The extrusion barrel diameter of the extruder is selected to be 420 mm, and the die is a single-hole die, so that the extrusion ratio is 17.64;

[0096] The reverse extrusion method is adopted, the mold heating temperature is 420℃, the extrusion barrel temperature is 387-393℃, the round ingot temperature before extrusion is 398-405℃; the product extrusion speed is 1.50-1.80m / min; the metal surface temperature before entering the cooling water is 422-428℃;

[0097] (4) Cooling treatment:

[0098] A standing wave water cooling device and a water-penetrating cooling device are installed at the front beam outlet of the extruder, and the length of the extruded aluminum alloy product in the water is controlled to be ≥4.0m. The water temperature of the standing wave water cooling device and the water-penetrating cooling device are both 50-60℃, so that the surface temperature of the product after cooling is 25.0-34.0℃; this setting can cool the extruded aluminum alloy product to room temperature in a short time;

[0099] (5) Stretching treatment:

[0100] The cooled product is stretched by a stretching machine within 4 hours to produce 1.7% tensile deformation, so as to eliminate the straightness difference and residual stress caused by traction and cooling deformation to the greatest extent;

[0101] (6) Artificial aging:

[0102] The stretched product is artificially aged at a holding temperature of 121±5°C for 24 hours.

[0103] The room temperature tensile properties test was carried out on the aged 7 series alloy samples, and the results are shown in Table 3;

[0104] Table 3 Room temperature tensile properties of 7 series bars (diameter 100 mm) after aging

[0105]

[0106] It can be seen from the test data that the high-strength 7 series 100mm diameter rod produced by the process of the present invention can have a T6 state room temperature tensile strength of more than 610MPa, which is more than 40MPa higher than the standard value in the industry.

[0107] Comparative Example 1

[0108] Traditional production process, the specific process is as follows:

[0109] (1) Alloy composition ratio:

[0110] A round ingot with a diameter of 410 mm was selected as the raw material, and a direct reading spectrometer was used to detect the alloy composition of the round ingot for extrusion. The element composition of the round ingot is as follows:

[0111] Si 0.1%, Fe 0.25%, Cu 1.85%, Mn 0.12%, Mg 2.4%, Cr 0.24%, Zn 5.2%, Ti0.07%, the balance is Al and unavoidable impurities; the single content of unavoidable impurities shall not exceed 0.05%, and the total content shall not exceed 0.15%;

[0112] (2) Uniform heat treatment of round ingots:

[0113] The round ingot of step (1) is subjected to homogenization heat treatment: the heating rate is 35°C / hour, the first-level insulation temperature is 435°C, and the insulation time is 8 hours; the second-level insulation temperature is 465°C, and the insulation time is 24 hours; after the second-level insulation is completed, it is air-cooled to below 250°C;

[0114] (3) Extrusion treatment:

[0115] s1, design of extrusion die:

[0116] Adopt reverse extrusion die, die working belt 3.0mm;

[0117] s2, the extrusion process is as follows:

[0118] The extrusion barrel diameter of the extruder is selected to be 420 mm, and the die is a single-hole die, so that the extrusion ratio is 17.64;

[0119] The reverse extrusion method is adopted, the mold heating temperature is 420, the extrusion barrel temperature is 357-363℃, the round ingot temperature before extrusion is 378-385℃; the product extrusion speed is 1.50-1.80m / min;

[0120] (4) Pre-stretching treatment:

[0121] The extruded product is stretched by a stretching machine to produce 0.3-1.0% tensile deformation to eliminate the bending after extrusion and avoid the bending affecting the quenching in the vertical quenching furnace;

[0122] (5) Pre-sawing process:

[0123] Intermittent sawing of the product to ensure that the length of the product after sawing is shorter than the length of the vertical quenching furnace, so that the product can be smoothly loaded into the vertical quenching furnace;

[0124] (6) Solution heat treatment:

[0125] The interrupted product is subjected to solution heat treatment, with a holding temperature of 471±5℃, a holding time of 210min, a quenching transfer time of ≤30s, and a cooling water temperature of ≤50℃.

[0126] (7) Stretching treatment:

[0127] For the products after solution heat treatment, a tensile deformation of 1.7% is generated by a stretching machine within 4 hours to eliminate the straightness difference and residual stress caused by traction and cooling deformation to the greatest extent;

[0128] (8) Artificial aging:

[0129] The stretched product is artificially aged at a holding temperature of 121±5°C for 24 hours.

[0130] The room temperature tensile properties test was carried out on the aged 7 series alloy samples, and the results are shown in Table 4;

[0131] Table 4 Room temperature tensile properties of 7 series bars (diameter 100 mm) after aging

[0132]

[0133] From the comparison between the process of the present invention and the traditional process, it can be concluded that the production by the process of the present invention can reduce the process routes such as pre-stretching, pre-sawing, and solution heat treatment, shorten the production cycle and effectively reduce the production cost.

[0134] Although the present invention has been described in detail by reference to the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. A low-cost and high-efficiency production process for high-strength 7 series aluminum alloy, characterized in that: The process is as follows: (1) Alloy composition ratio: A round ingot is selected as the raw material, and the round ingot includes the following elements in percentage by weight: Si 0.05-0.50%, Fe 0.13-0.60%, Cu 1.80-2.60%, Mn≤0.30%, Mg 1.90-2.70%, Cr0.15-0.25%, Zn 5.00-5.80%, Ti 0.04-0.10%, the balance is Al and unavoidable impurities; the single content of unavoidable impurities shall not exceed 0.05%, and the total content shall not exceed 0.15%; (2) Uniform heat treatment of round ingots: During the homogenization heat treatment process, the heating rate is ≤35℃ / hour, the first-level insulation temperature is 430-440℃, and the insulation time is 8-12 hours; the second-level insulation temperature is 465-478℃, and the insulation time is 20-26 hours; after the second-level insulation is completed, air-cooling is performed to below 250℃; (3) Extrusion treatment: s 1, design of extrusion die: Adopt reverse extrusion die, die working band 1.5-5.0mm; s 2, the extrusion process is as follows: Using reverse extrusion, the temperature of the mold is 370-410℃, the temperature of the extrusion barrel is 370-410℃, the temperature of the round ingot before extrusion is 365-400℃; the product extrusion speed is 1.30-2.00m / min; the metal surface temperature before entering the cooling water is 410-450℃; (4) Cooling treatment: Install standing wave water cooling device and water-penetrating cooling device at the exit of the front beam of the extruder, so that the length of the extruded aluminum alloy product in the water is ≥2.0m; (5) Stretching treatment: The cooled product is passed through a stretching machine to produce a stretching deformation of 1.20-2.50%; (6) Artificial aging: The stretched product is artificially aged at a holding temperature of 115-135°C for 24-30 hours.

2. The low-cost and high-efficiency production process of high-strength 7 series aluminum alloy according to claim 1 is characterized in that: In step (2), the heating rate is 28°C / hour, the first-level insulation temperature is 435°C, and the insulation time is 8 hours; the second-level insulation temperature is 465°C, and the insulation time is 24 hours; after the second-level insulation is completed, air cooling is performed to below 250°C.

3. The low-cost and high-efficiency production process of high-strength 7 series aluminum alloy according to claim 1 is characterized in that: In step (2), the air volume during the air cooling process is determined based on the premise that no cooling cracks are generated.

4. The low-cost and high-efficiency production process of high-strength 7 series aluminum alloy according to claim 1 is characterized in that: In step (3) s2, reverse extrusion is adopted, the temperature of the mold is 400°C, the temperature of the extrusion barrel is 384-392°C, the temperature of the round ingot before extrusion is 365-373°C; the product extrusion speed is 1.30-1.70m / min; the metal surface temperature before entering the cooling water is 416-428°C.

5. The low-cost and high-efficiency production process of high-strength 7 series aluminum alloy according to claim 1 is characterized in that: During the cooling process of step (4), the water temperature of the standing wave water cooling device and the water-penetrating cooling device are both ≤80°C.

6. The low-cost and high-efficiency production process of high-strength 7 series aluminum alloy according to claim 1, characterized in that: During the stretching treatment in step (5), the cooled product is subjected to a 1.8% stretching deformation by a stretching machine within 4 hours.

7. The low-cost and high-efficiency production process of high-strength 7 series aluminum alloy as described in claim 1, in the artificial aging process of step (6), the holding temperature is 121±5°C and the holding time is 24 hours.

Citation Information

Patent Citations

  • High-strength 6xxx aluminum alloy for mobile phone parts and machining method thereof

    CN105296811A

  • 6082 aluminium alloy thick-wall pipe production technology

    CN108866363A

  • Method for improving strength and ductility of 7xxx aluminum alloy at same time

    CN110284085A