Method and device for improving molding quality of additive manufacturing

The vibration reinforcement zone is formed in additive manufacturing by paired vibration exciters, which solves the problems of single vibration source and energy waste, and achieves the improvement of refined grains and molding quality.

CN115592288BActive Publication Date: 2024-11-26BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211131639.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-11-26
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

In the existing ultrasonic-assisted additive manufacturing technology, the vibration source is too single, resulting in serious energy waste and lack of targeted vibration application areas, affecting the molding quality.

Method used

A first vibration exciter is arranged in pairs, and its vibration waves are superimposed on each other to form a vibration reinforcement zone. By adjusting the vibration parameters, flexible vibration reinforcement of the melt pool is achieved, avoiding a single vibration source, and ensuring the targetedness and efficiency of the vibration application area. .

Benefits of technology

By refining the grains, the additive molding quality is significantly improved, energy loss is reduced, molding performance is improved, and the targeted and flexible vibration strengthening effect is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115592288B_ABST
    Figure CN115592288B_ABST
Patent Text Reader

Abstract

The present invention provides a method and device for improving the molding quality of additive manufacturing, comprising the following steps: arranging at least one pair of first vibrators beside a molten pool formed by a welding gun acting on a workpiece; driving the first vibrators to move with the welding gun to perform additive operations on the top surface of the workpiece; wherein the vibration waves of each pair of first vibrators are superimposed on each other and form a first vibration enhancement zone acting on the molten pool, and the first vibration enhancement zone can adjust the moving position and superposition frequency based on the vibration parameters of each pair of first vibrators. The method and device for improving the molding quality of additive manufacturing described in the present invention can solve the defects of the prior art of severe energy waste, too single vibration source, and lack of specificity in the vibration application area during ultrasonic-assisted additive processes, and can achieve grain refinement and improve the molding effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a method and device for improving the molding quality of additive manufacturing. Background Art

[0002] Based on the discrete-deposition principle, metal additive manufacturing technology can directly realize the forming of metal parts. The required metal wire is melted by using electric arc, laser or electron beam as the heat source, and then accumulated layer by layer on the substrate according to the prescribed forming path, and finally the three-dimensional forming of the parts is realized. It has the advantages of cost saving and complex forming, and has been widely used in many industries such as aerospace, automobile, and shipbuilding, and plays a huge role in the field of national intelligent manufacturing.

[0003] Additive manufacturing involves many physical processes, including complex problems such as thermal cycles and stress reconstruction, which are prone to defects such as surface roughness and pores. The performance of the material is largely affected by the grain growth during the melting and solidification of the metal. The additional energy field in the additive manufacturing process can affect the grain growth process and the molding results.

[0004] At present, for the process of ultrasonic assisted additive manufacturing, since the vibration source in the existing technology is mostly applied to the substrate, the vibration wave will produce a large energy attenuation during the transmission process, which will weaken the vibration effect of the molten pool and cause a large waste of energy; moreover, the vibration source used in the additive process is too single and lacks specificity, which can easily lead to a weak improvement in the performance of the formed workpiece after additive manufacturing, and thus cause the surface position that should have been processed and removed to be strengthened instead, while the position that should have been strengthened is not strengthened significantly. Summary of the invention

[0005] The present invention provides a method and device for improving the molding quality of additive manufacturing, which are used to solve the defects of severe energy waste, too single vibration source and lack of specificity in the vibration application area in the ultrasonic assisted additive process of the prior art, and can achieve grain refinement and improve the molding effect.

[0006] The present invention provides a method for improving the molding quality of additive manufacturing, comprising the following steps:

[0007] At least one pair of first vibrators is arranged beside a molten pool formed by the welding gun acting on the workpiece;

[0008] driving the first vibrator to move along with the welding gun to perform an additive operation on the top surface of the workpiece;

[0009] The vibration waves of each pair of the first vibrators are superimposed on each other to form a first vibration enhancement zone acting on the molten pool, and the first vibration enhancement zone can adjust the moving position and the superposition frequency based on the vibration parameters of each pair of the first vibrators.

[0010] According to the method for improving the molding quality of additive manufacturing described in the present invention, under the placement condition that any two of the first vibrators do not interfere with each other, at least one pair of the first vibrators is provided, and the two first vibrators in each pair are provided on the same side of the molten pool; or, the two first vibrators in each pair are provided on both sides of the molten pool, respectively.

[0011] According to the method for improving the molding quality of additive manufacturing of the present invention, the vibration parameters of the first exciter include phase and frequency;

[0012] Taking one of the first vibrators in each pair as a reference, adjusting the phase of the other first vibrator to drive the first vibration reinforcement zone to move within the entire molten pool; and / or,

[0013] Taking one of the first exciters in each pair as a reference, the frequency of the other first exciter is adjusted to control the superposition frequency of the first vibration reinforcement zone.

[0014] According to the method for improving the molding quality of additive manufacturing of the present invention, all the first vibrators are divided into at least two groups, and each group of the first vibrators includes at least one pair of first vibrators arranged on both sides of the welding gun;

[0015] The phase and vibration frequency of each pair of the first exciters in the same group are the same; and the distance between two adjacent groups of the first exciters is at least a minimum integer multiple of the wavelength.

[0016] According to the method for improving the additive manufacturing molding quality of the present invention, two groups of the first vibrators are started in sequence according to the progress of the additive operation of the workpiece; after the two groups of the first vibrators are in contact with the workpiece, the waveform phases of the two groups of the first vibrators (300) remain the same.

[0017] According to the method for improving the additive manufacturing molding quality of the present invention, the method for improving the additive manufacturing molding quality further comprises the following steps:

[0018] Arranging a plurality of second vibration exciters on the side of the workpiece;

[0019] When the height of the workpiece added material meets the placement height requirement of the second vibrator, the second vibrator is started, and the second vibrator is raised and lowered as the height of the workpiece added material changes;

[0020] The vibration waves of the two second vibrators adjacent to the welding gun can be superimposed on each other to form a second vibration enhancement zone acting on the molten pool, and the second vibration enhancement zone can adjust the moving position and superposition frequency based on the vibration parameters of the second vibrator;

[0021] Among them, the vibration wave transmission direction of the first exciter is set at an angle to the vibration wave transmission direction of the second exciter, so that the first vibration enhancement zone formed by the vibration wave of the first exciter and the second vibration enhancement zone formed by the vibration wave of the second exciter are superimposed on each other, thereby generating coupled vibration to the molten pool.

[0022] According to the method for improving the molding quality of additive manufacturing described in the present invention, the corresponding two second vibrators are started according to the position of the welding gun on the workpiece, so that the molten pool is always located in the second vibration enhancement zone formed by the mutual interference of vibration waves emitted by the two second vibrators.

[0023] According to the method for improving the molding quality of additive manufacturing of the present invention, the vibration parameters of the second exciter include phase and frequency;

[0024] Among the two second vibrators adjacent to the welding gun, one of the second vibrators is used as a reference to adjust the phase of the other second vibrator to drive the second vibration enhancement area to move within the entire molten pool; and / or,

[0025] Taking one of the second exciters as a reference, the frequency of another second exciter is adjusted to control the superposition frequency of the second vibration enhancement zone.

[0026] The method for improving the molding quality of additive manufacturing according to the present invention comprises:

[0027] Step S1, arranging the positions of the first vibration exciter and the second vibration exciter relative to the workpiece;

[0028] Step S2, starting the first vibrator according to the workpiece additive process, and driving the welding gun to move on the top surface of the workpiece to perform additive operation; during the movement of the welding gun, the first vibrator follows the movement of the welding gun, and regulates the movement position and superposition frequency of the first vibration reinforcement zone formed by the vibration waves of each pair of the first vibrator;

[0029] Step S3, when the material addition height of the workpiece meets the placement requirements of the second vibrator array and there is no equipment space interference, start the corresponding two second vibrators according to the position of the welding gun on the workpiece, and adjust the moving position and superposition frequency of the second vibration enhancement zone formed by the vibration waves of each pair of the second vibrators, so that the first vibration enhancement zone formed by the vibration wave of the first vibrator and the second vibration enhancement zone formed by the vibration wave of the second vibrator are superimposed on each other, thereby generating coupled vibration to the molten pool;

[0030] Step S4: as each layer of the additive process is completed, the second vibrator moves in the height direction;

[0031] Repeat the above steps S2 to S4 to sequentially complete the stacking and forming of each layer of the workpiece until the additive manufacturing of the workpiece is completed.

[0032] The present invention also provides a device for improving the molding quality of additive manufacturing, which is used to perform the method for improving the molding quality of additive manufacturing as described above;

[0033] The device for improving the molding quality of additive manufacturing comprises a welding gun, a first vibrator and a first driving member;

[0034] At least one pair of the first vibrators is arranged beside a molten pool formed when the welding gun acts on the workpiece;

[0035] The first driving member is connected to the welding gun and each of the first vibrators, and can drive the welding gun and each pair of the first vibrators to move together.

[0036] The device for improving the molding quality of additive manufacturing according to the present invention further includes a second vibrator and a second driving member;

[0037] A plurality of second vibration exciters are arranged on the side of the workpiece;

[0038] The second driving member is respectively connected to each of the second vibrators, and can drive the second vibrators to move along the height direction of the workpiece.

[0039] The method and device for improving the molding quality of additive manufacturing provided by the present invention utilizes the vibration waves of the first vibrators arranged in pairs to be superimposed on each other, thereby forming a first vibration reinforcement zone within the molten pool, thereby achieving grain refinement and improving the molding effect. The first vibrators arranged in pairs can act on the molten pool together, thereby avoiding the situation where the vibration source is too single.

[0040] The present invention is based on the characteristics of waves and the principle of interference. By starting the first exciter, the molten pool in the additive process is always subjected to vibration reinforcement in the corresponding direction. By flexibly adjusting the vibration parameters of the first exciter, the moving position and superposition frequency of the first vibration reinforcement zone can be flexibly adjusted, thereby increasing the pertinence and flexibility of the vibration reinforcement effect on the molten pool, and making the vibration application area more precise and effective. Moreover, the change of the superposition frequency of the first vibration reinforcement zone can also make the vibration effect of the vibration area more varied through the differentiation of the vibration laws of the local frequency bands, the molten pool stirring and grain refinement effects are more obvious, and the vibration reinforcement effect is more efficient.

[0041] Furthermore, in the present invention, the first vibrator moves along with the movement of the welding gun, thereby ensuring that the vibration source and the molten pool are always at a relatively close distance, thereby avoiding excessive energy loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0043] Figure 1 This is one of the flow charts of the method for improving the molding quality of additive manufacturing provided by an embodiment of the present invention;

[0044] Figure 2 This is a second flow chart of the method for improving the molding quality of additive manufacturing provided by an embodiment of the present invention;

[0045] Figure 3 is a schematic structural diagram of a device for improving additive manufacturing molding quality provided by an embodiment of the present invention;

[0046] Figure 4 is a schematic diagram of the arrangement structure of the first exciter provided in an embodiment of the present invention;

[0047] Figure 5 is a schematic diagram of waveform interference superposition provided by an embodiment of the present invention;

[0048] Figure 6 It is a principle diagram of interference superposition after waveform phase shifting provided by an embodiment of the present invention;

[0049] Figure 7 It is a principle diagram of interference superposition after waveform frequency modulation provided by an embodiment of the present invention.

[0050] Reference numerals:

[0051] 100, workpiece; 200, welding gun; 300, first vibrator; 400, second vibrator; 500, molten pool; A~H, placement position of the first vibrator. DETAILED DESCRIPTION

[0052] The following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0053] In the description of the embodiments of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limitations on the embodiments of the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0054] In the description of the embodiments of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present invention can be understood according to specific circumstances.

[0055] In the embodiments of the present invention, unless otherwise clearly specified and limited, the first feature being "above" or "below" the second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, the first feature being "above", "above" and "above" the second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. The first feature being "below", "below" and "below" the second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0056] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0057] Combine the following Figure 1 to Figure 7 The method of improving the quality of additive manufacturing molding of the present invention is described. The method comprises the following steps:

[0058] At least one pair of first vibrators 300 is arranged beside a molten pool 500 formed by the welding gun 200 acting on the workpiece;

[0059] The first vibrator 300 is driven to move along with the welding gun 200 to perform an additive operation on the top surface of the workpiece 100 ;

[0060] The vibration waves of each pair of first vibrators 300 are superimposed on each other to form a first vibration enhancement zone acting on the molten pool 500 . The first vibration enhancement zone can adjust the moving position and superposition frequency based on the vibration parameters of each pair of first vibrators 300 .

[0061] See also Figure 1 and Figure 3 , under the condition that any two first vibrators 300 do not interfere with each other, it is preferred that at least one pair of first vibrators 300 is provided. The specific placement of the first vibrators 300 can be in the following two situations: the two first vibrators 300 in each pair are arranged on the same side of the molten pool 500; or the two first vibrators 300 in each pair are arranged on both sides of the molten pool 500.

[0062] In fact, each pair of first vibration exciters 300 can be arranged at any position on the same side or both sides of the molten pool 500. Figure 4 As shown, taking the position of any pair of first vibration exciters 300 as an example, one of the first vibration exciters can be placed at position A, and the other first vibration exciter 300 arranged in pair with the first vibration exciter 300 at position A can be arranged at position B, position C, or position D, so as to arrange the pair of first vibration exciters 300 on the same side of the molten pool 500; or, the other first vibration exciter 300 arranged in pair with the first vibration exciter 300 at position A can be arranged at position E, position F, position G, or position H, so as to arrange the pair of first vibration exciters 300 on both sides of the molten pool 500.

[0063] It should be noted that Figure 4 The arrows shown are the travel direction of the welding torch 200. It can be seen that the same side or both sides of the molten pool 500 refer to the front side and / or the rear side along the travel direction of the welding torch 200. Positions A to H are only used to simply illustrate the positions where the first exciter 300 can be placed. In fact, the relative distance between the placement position of the first exciter 300 and the molten pool 500 is not limited to Figure 4 As shown, the number of rows of the placement positions of the first vibrators 300 on both sides of the molten pool 500 can be one row or more rows, and the specific number is determined according to the vibration parameters of the first vibrators 300, as long as the adjacent first vibrators 300 do not interfere with each other, and the first vibrators 300 arranged in pairs can form the first vibration enhancement zone as described above within the range of the molten pool 500.

[0064] It should be noted that the welding direction mentioned in this embodiment is Figure 1 In the X direction, the height direction is Figure 1 In the Z direction, the width direction is Figure 1 Center Y direction.

[0065] It should be noted that the molten pool 500 refers to a portion of metal on the workpiece that undergoes a melting process under the action of the heat source of the welding gun during melting welding.

[0066] Based on the placement position of the first vibrator mentioned above, the moving position of the first vibration enhancement zone relative to the molten pool 500 and the superposition frequency of the first vibration enhancement zone are flexibly controlled by adjusting the vibration parameters of the first vibrator 300. Preferably, the vibration parameters of the first vibrator 300 include phase and frequency. Based on one first vibrator 300 in each pair as a reference, the phase of the other first vibrator 300 is adjusted to drive the first vibration enhancement zone to move within the entire molten pool 500, so as to achieve a targeted vibration enhancement effect of the first vibration enhancement zone relative to the molten pool 500, and to efficiently utilize energy; and / or, based on one first vibrator 300 in each pair as a reference, the frequency of the other first vibrator 300 is adjusted to control the superposition frequency of the first vibration enhancement zone, thereby achieving a targeted improvement in the vibration enhancement effect of the local frequency band of the first vibration enhancement zone, so that the vibration enhancement effect acts more efficiently on the molten pool 500 and more fully utilizes energy.

[0067] It should be noted that the above-mentioned “taking one first exciter 300 in each pair as a reference” means that the relevant vibration parameters of the first exciter 300 serving as a reference remain unchanged, and the parameter adjustment corresponding to the above-mentioned first vibration enhancement zone is achieved by adjusting the relevant vibration parameters of the other first exciter 300.

[0068] In some specific embodiments, see Figure 3 and Figure 4 Preferably, all first vibrators 300 are divided into at least two groups, and each group of first vibrators 300 includes at least one pair of first vibrators 300 disposed on both sides of the welding gun 200. Figure 3As shown, two groups of first vibrators 300 are arranged on both sides of the welding gun 200, one group of first vibrators 300 is placed at a position closer to the welding gun 200, and the other group of first vibrators 300 is placed at a position farther from the welding gun 200. There is a gap between the two groups of first vibrators 300 to avoid mutual interference. In the two groups of first vibrators 300, each group includes at least two pairs of first vibrators 300, and in this embodiment, each group includes two pairs of first vibrators 300. The two pairs of first vibrators 300 in the same group are spaced apart from each other to avoid mutual interference; and, in the two pairs of first vibrators 300 in the same group, each pair of first vibrators 300 is symmetrically arranged on both sides of the welding gun 200. In other words, the two first vibrators 300 in a pair of first vibrators 300 are at an equal distance from the welding gun 200.

[0069] It should be noted that, on the one hand, preferably, under the placement condition that any two first vibrators 300 do not interfere with each other, each pair of first vibrators 300 in the same group is adjusted to have the same phase and vibration frequency, so that there is always a pair of first vibrators 300 on both sides of the welding gun 200 that can emit two groups of waves with the same phase and frequency, which act together on the molten pool 500 to achieve vibration coupling, thereby making the vibration application area more targeted, reducing the vibration intensity of a single vibration source, and reducing damage to the workpiece surface. On the other hand, it is preferred that the spacing between two adjacent groups of first vibrators 300 is at least a minimum integer multiple of the wavelength to avoid mutual interference.

[0070] It should be noted that in the above specific embodiments, Figure 3 As shown, it is preferred that each pair of first vibrators 300 are placed under the premise of non-interference to ensure that the phase and vibration frequency are the same; and, the spacing between a group of first vibrators 300 farther from the welding gun 200 and a group of first vibrators 300 closer to the welding gun 200 is an integer multiple of the wavelength, and should be as small as possible. The purpose of such a setting is to allow the vibration waves generated by each pair of first vibrators 300 farther from the welding gun 200 and the vibration waves generated by each pair of first vibrators 300 closer to the welding gun to also produce an interference enhancement effect, and at the same time, it can also make the first vibrators 300 always be at a closer distance to the molten pool 500 generated between the welding gun 200 and the workpiece 100 during the entire workpiece 100 additive process, so as to avoid excessive energy loss.

[0071] It should be noted that the number of the first vibrators 300 in each group can be adaptively selected according to the material and length of the workpiece 100, and can be one pair, two pairs, three pairs, etc. The first vibrators 300 in each group are arranged in intervals along the welding direction of the workpiece 100 with the welding gun 200 as the center. Figure 3As shown, the spacing between each pair of first vibrators 300 is limited to n+1 / 2 times the wavelength, wherein n is the smallest positive integer that satisfies the condition that there is no spatial interference between the devices; if there are at least two groups of first vibrators 300 around the welding gun 200, and the two first vibrators 300 of the same group are respectively located on both sides of the welding gun 200, it is preferred to limit the spacing between each pair of first vibrators 300 in a group of first vibrators 300 farther from the welding gun 200 to n+1 / 2+2m times the wavelength, wherein m is the smallest positive integer that satisfies the condition that there is no spatial interference between the devices.

[0072] It should be noted that the placement positions of the above-mentioned two groups of first vibrators 300 should ensure that they do not interfere with each other. And the distance between any two columns of first vibrators 300 in the same group of first vibrators 300 should also meet the requirement of not interfering with each other. It is only necessary to ensure that the waveforms generated by each column of first vibrators 300 have the same phase and ensure that the molten pool 500 of the welding gun 200 is in the first vibration enhancement zone generated by the first vibrator 300. In other words, the placement distance of the above-mentioned two groups of first vibrators 300 is not limited to the above-mentioned n+1 / 2 times the wavelength, and the expression of the placement distance n+1 / 2 times the wavelength is only for the convenience of explanation. In fact, according to the relationship between the placement position, wavelength and phase of each group of first vibrators 300, the initial phase of the two groups of first vibrators 300 can be adjusted accordingly to ensure that the central area between the two groups of first vibrators 300 generates a reinforcement zone, as long as the first vibration reinforcement zone can always act on the molten pool formed by the moving welding gun 200, and the placement positions of the two groups of first vibrators 300 do not interfere with each other in space. Moreover, the distance between the first vibrators 300 of each column on the same side of the welding gun 200 in all pairs of first vibrators 300 of the same group also needs to meet the requirement of non-interference placement, and the molten pool 500 can be ensured to be in the same reinforcement zone by ensuring that the phase of the waveform generated by them is the same as that of the waveform generated by each column of first vibrators 300 on the other side.

[0073] In other embodiments of the present invention, the number of the first vibrators 300 can be adaptively selected according to the material and length of the workpiece 100, and can be two, four, six, etc., that is, under the premise of meeting the vibration intensity at the molten pool 500, the vibration intensity requirement of each first vibrator 300 is reduced. By increasing the number of first vibrators 300, the vibration intensity requirement at the molten pool 500 is met, thereby preventing the workpiece 100 from being damaged by excessive vibration intensity of a single vibration source, thereby enhancing the machinability of the surface of the workpiece 100.

[0074] See also Figure 1 and Figure 3, two sets of first vibrators 300 are sequentially started according to the progress of the material addition operation of the workpiece 100; after the two sets of first vibrators 300 are in contact with the workpiece 100, the vibration parameters of the first vibrators 300 can be adjusted according to the material addition needs so that the waveform phases of the two sets of first vibrators 300 remain the same. During the material addition process of the workpiece 100, the first vibrator 300 moves with the movement of the welding gun 200, and the vibration wave emitting end of the first vibrator 300 is in contact with the upper surface of the workpiece 100.

[0075] Specifically, each group of first vibrators 300 is turned on synchronously; as the welding gun 200 moves, the first vibrator 300 located at the front end side of the welding gun 200 in each group of first vibrators 300 (hereinafter referred to as "the first vibrator 300 located at the front end side of the welding gun 200") preferentially contacts the workpiece 100 and generates ultrasonic vibration at the top of the workpiece 100, so that the vibration wave generated by the first vibrator 300 located at the front end side of the welding gun 200 generates a vibration reinforcement effect on the molten pool 500 through interference superposition, so as to refine the grains of the metal in the solidification process, precipitate gas, and improve the forming performance; as the welding gun 200 moves When the first vibrator 300 located at the rear end side of the welding gun 200 in the moving direction of each group of first vibrators 300 (hereinafter referred to as "the first vibrator 300 located at the rear end side of the welding gun 200") contacts the workpiece 100, the vibration wave generated by the first vibrator 300 located at the rear end side of the welding gun 200 and the first vibrator 300 located at the front end side of the welding gun 200 have the same waveform phase and work synchronously. In this state, the vibration waves generated by the first vibrators 300 located on both sides of the welding gun 200 interfere with each other and superimpose, thereby generating a vibration enhancement effect on the molten pool 500. After completing the additive operation of one layer of the workpiece 100, the first vibrators 300 are closed in sequence according to the order in which the first vibrators 300 located on both sides of the welding gun 200 leave the surface of the workpiece 100, and the operation is repeated when the additive operation of the next layer begins. In the above welding process, the phase and / or frequency of the first vibrator 300 can be dynamically adjusted according to the control process and method described in the embodiment of the present invention.

[0076] It should be noted that the order of opening the first vibrators 300 located on both sides of the welding gun 200 can be opened synchronously or one after another. If the first vibrators 300 located on both sides of the welding gun 200 are opened one after another, as long as the first vibrators 300 located on both sides of the welding gun 200 are opened respectively according to the order of contacting the workpiece 100, and when the first vibrator 300 located on the rear end side of the welding gun 200 is opened, it should be ensured that the waveform phases of the vibration waves of the first vibrators 300 located on both sides of the welding gun 200 in the same group are the same.

[0077] In the embodiment of the present invention, please refer to Figure 3On the basis of the above, the method for improving the molding quality of additive manufacturing further comprises the following steps:

[0078] A plurality of second vibration exciters 400 are arranged on the side of the workpiece 100;

[0079] When the height of the workpiece 100 increases, the second vibrator 400 is started, and the second vibrator 400 is raised and lowered as the height of the workpiece 100 increases;

[0080] The vibration waves of the two second vibrators 400 adjacent to the welding gun 200 can be superimposed on each other to form a second vibration enhancement zone acting on the molten pool 500, and the second vibration enhancement zone can adjust the moving position and superposition frequency based on the vibration parameters of the second vibrator 400;

[0081] Among them, the vibration wave transmission direction of the first exciter 300 is set at an angle to the vibration wave transmission direction of the second exciter 400, so that the first vibration enhancement zone formed by the vibration wave of the first exciter 300 and the second vibration enhancement zone formed by the vibration wave of the second exciter 400 are superimposed on each other, thereby generating coupled vibration to the molten pool 500.

[0082] It should be noted that in this embodiment, the first exciter 300 and the second exciter 400 can emit vibration waves, ultrasonic waves, and waves of different frequencies or different types for interference; the choice of waveform can be adapted according to the material of the actual additive workpiece 100, and no excessive restrictions are made in this embodiment.

[0083] See also Figure 1 and Figure 3 , the positions of the first vibration exciter 300 and the second vibration exciter 400 are arranged relative to the workpiece 100. The placement position of the first vibration exciter 300 is referred to the above content, which will not be repeated here.

[0084] It is understandable that the second vibrator 400 is preferably placed on the side of the workpiece 100 in an array structure, as long as adjacent second vibrators 400 do not interfere with each other, and during the movement of the welding gun 200, there are always two adjacent second vibrators 400 that can jointly form a second vibration enhancement zone acting on the molten pool 500.

[0085] It is understandable that, based on the arrangement of the placement position of the second vibration exciter 400, the movement position of the second vibration enhancement zone relative to the molten pool 500 and the superposition frequency of the second vibration enhancement zone can be flexibly controlled by adjusting the vibration parameters of the second vibration exciter 400. Preferably, the vibration parameters of the second vibration exciter 400 include phase and frequency. Taking one of the two adjacent second vibrators 400 as a reference, the phase of the other second vibrator 400 is adjusted to drive the second vibration enhancement zone to move within the entire molten pool 500, so that the second vibration enhancement zone can play a targeted vibration enhancement role relative to the molten pool 500, so that the second vibration enhancement zone can be more accurately superimposed with the first vibration enhancement zone, ensuring that the molten pool 500 is subjected to a more targeted and flexible vibration enhancement effect, and the above-mentioned regulation can efficiently utilize energy; and / or, taking one of the two adjacent second vibrators 400 as a reference, the frequency of the other second vibrator 400 is adjusted to adjust the superimposed frequency of the second vibration enhancement zone, thereby achieving a targeted improvement in the vibration enhancement effect of the local frequency band of the second vibration enhancement zone, so that the vibration enhancement effect acts more efficiently on the molten pool 500 and more fully utilizes energy.

[0086] See also Figure 1 and Figure 3 , the position of the second vibrator 400 relative to the workpiece 100 is arranged according to the vibration parameters of the second vibrator 400; further, the vibration wave transmission direction of the first vibrator 300 is set at an angle to the vibration wave transmission direction of the second vibrator 400, so that the first vibration reinforcement zone formed by the vibration wave of the first vibrator 300 and the second vibration reinforcement zone formed by the vibration wave of the second vibrator 400 are superimposed on each other, thereby generating coupled vibration to the molten pool 500, and further refining the grains and precipitating gas during the metal solidification process, thereby improving the forming performance of the workpiece 100.

[0087] In this embodiment, the first vibrator 300 is perpendicular to the upper surface of the workpiece 100, and the second vibrator 400 is perpendicular to the side surface of the workpiece 100, so that the vibration wave transmission direction of the first vibrator 300 and the vibration wave transmission direction of the second vibrator 400 form an angle of 90 degrees; and when the additive height of the workpiece 100 meets the placement requirements of the second vibrator 400 and there is no equipment space interference, the vibration wave of the first vibrator 300 and the vibration wave of the second vibrator 400 act together on the molten pool 500.

[0088] In other embodiments of the present invention, the arrangement positions of the first vibrator 300 and the second vibrator 400 are not limited to the top surface and the side surface of the workpiece 100, but may also be arranged at an angle, that is, to ensure that the vibration waves generated by the first vibrator 300 and the second vibrator 400 act on the molten pool 500 in two different directions.

[0089] See also Figure 1 and Figure 3 In order to make the area where the first vibration enhancement zone formed by the first vibrator 300 and the second vibration enhancement zone formed by the second vibrator 400 generate coupled vibrations always act on the molten pool 500, it is preferred that, based on the specific setting of the placement position of the first vibrator 300, a plurality of second vibrators 400 are arranged in an array along the welding direction, and the second vibrators 400 are in contact with the side surface of the workpiece 100. Specifically, in the present embodiment, six second vibrators 400 are arranged at intervals along the welding direction. It should be noted that the number of second vibrators 400 can be adaptively selected according to the material and length of the workpiece 100, and can be two, four, eight, etc.; a certain distance is left between the second vibrators 400 corresponding to the two ends of the workpiece 100 and the two end boundaries of the workpiece 100 in the welding direction, and the distance is preferably not less than 5 mm; a certain distance is left between the second vibrator 400 and the un-added top of the workpiece 100, and the distance is preferably not less than 5 mm.

[0090] It should be noted that the second vibrator 400 can move in the height direction as the height of the workpiece 100 increases, as long as the boundary distances of all the second vibrators 400 from the two ends of the welding direction of the workpiece 100 are kept unchanged during the movement of the second vibrator 400; the moving distance of the second vibrator 400 in the height direction can be kept unchanged during the movement of the second vibrator 400; and the distance between the second vibrator 400 and the unprocessed surface at the top of the workpiece can be kept unchanged. The purpose of the above settings is to ensure that the second vibrator 400 is at a closer distance to the top of the workpiece 100 to avoid excessive energy loss, and secondly, to facilitate the actual lifting and lowering motion control of the second vibrator 400.

[0091] See also Figure 1 and Figure 3 When the additive height of the workpiece 100 meets the placement requirements of the second vibrator 400 and there is no equipment space interference, the corresponding two second vibrators 400 are started according to the position of the welding gun 200 on the workpiece 100, so that the molten pool 500 generated between the welding gun 200 and the workpiece 100 during the movement can always be subjected to the vibration enhancement effect of the second vibration enhancement zone formed by the mutual interference of the vibration waves emitted by the two second vibrators 400.

[0092] With reference to the above-mentioned control process of the vibration parameters of the second vibrator 400, it is preferred that, among the two second vibrators 400 adjacent to the welding gun 200, the phase of the vibration wave emitted by one remains unchanged, while the phase of the vibration wave emitted by the other shifts along the welding direction; the frequency parameters can also be adjusted at the same time, the frequency of the vibration wave emitted by one remains unchanged, and the frequency of the vibration wave emitted by the other is changed, so as to enhance the vibration effect.

[0093] It should be noted that, in this embodiment, in order to ensure that the molten pool 500 can always be subjected to the vibration enhancement effect of the second vibration enhancement zone formed by the mutual interference of the vibration waves emitted by the two second vibrators 400, the principle of vibration wave interference superposition is adopted, and multiple second vibrators 400 are arranged in an array along the welding direction. By changing the vibration parameters of one of the two second vibrators 400 adjacent to the welding gun 200, such as the waveform phase, the second vibration enhancement zone can move with the welding gun 200; similarly, by changing the frequency of one of the two second vibrators 400 adjacent to the welding gun 200, the superposition frequency of the second vibration enhancement zone can be controlled, thereby changing the vibration in the local frequency band, and realizing the vibration changes of the second vibration enhancement zone including different frequency bands, for example, forming a local superposition of high frequency and low frequency; or the two vibration parameters can be changed at the same time to realize the movement of the second vibration enhancement zone and the combination of high and low vibration frequencies.

[0094] During the additive operation of the workpiece 100, the first second vibrator 400 along the welding direction is preferentially turned on. When the welding gun 200 passes through the first second vibrator 400, the second second vibrator 400 is turned on, and the vibration parameters of the second vibrator 400 are adjusted so that the interference superposition area of ​​the two waveforms follows the movement of the molten pool 500 until it passes through the second second vibrator 400. Then, the first second vibrator 400 is turned off and the third second vibrator 400 is turned on. Similarly, the above process is repeated until the additive process of the current layer is completed; when the additive manufacturing of the next layer begins, the second vibrator 400 is turned on according to the above process until the entire additive process is completed.

[0095] It should be noted that, based on the above-mentioned regulation of the vibration parameters of the first exciter 300 and the second exciter 400, it is preferred that the vibration parameters of the first exciter 300 and the second exciter 400 also include wavelength. The phase adjustment rule of the first exciter 300 can be determined based on the placement position and wavelength of the first exciter 300. Similarly, the phase adjustment rule of the second exciter 400 can be determined based on the placement position and wavelength of the second exciter 400.

[0096] The wavelength is calculated by the following steps:

[0097] Testing the emission frequency of the first exciter 300 or the second exciter 400;

[0098] Testing the propagation speed of the vibration wave emitted by the first vibration exciter 300 or the second vibration exciter 400 in the workpiece 100;

[0099] The wavelength of the vibration wave during the material addition operation of the workpiece 100 is determined according to the emission frequency and the propagation speed.

[0100] In addition, this embodiment also provides a specific formula for calculating the wavelength: v=λ×f; wherein v is the propagation speed of the vibration wave (m / s), λ is the wavelength (m), and f is the frequency of the vibration wave.

[0101] In summary, the waveforms of the first exciter 300 and the second exciter 400 are analyzed through a specific example.

[0102] Please refer to Figure 5 , line B is two waveforms with the same frequency and phase and opposite propagation directions emitted by the two first vibrators 300; line A is the waveform after the interference and superposition of the two waves; two waves with the same frequency and phase and opposite propagation directions will produce interference and superposition phenomenon. Further, after the above-mentioned phase adjustment, the two first vibrators 300 are in a certain static state, that is, when the waveform phases and frequencies of the two first vibrators 300 are equal, and when the two second vibrators 400 are n+1 / 2 times the wavelength apart, the peaks or troughs of the two waves will meet correspondingly at the center position of the line connecting the two second vibrators 400, so that the amplitude increases exponentially, which is the vibration enhancement zone, where n is a positive integer.

[0103] Please refer to Figure 6 , line B1 is Figure 5 The waveform emitted by the first exciter 300; line A is Figure 5 Line C is the waveform of the vibration wave emitted by a first vibrator 300 after phase shifting; Line D is the waveform of the interference superposition of the phase-shifted waveform (line C) and the waveform without phase shifting (line B1); when the phase of the waveform of one of the first vibrators 300 is shifted, the vibration enhancement zone corresponds to the intersection node of the two waveforms, thereby causing the position corresponding to the vibration enhancement zone to change.

[0104] Please refer to Figure 7 , line B2 is Figure 5 The waveform emitted by one of the first exciters 300; Line C1 is the waveform of the vibration wave emitted by another first exciter 300 to change the vibration output frequency. In one and a half propagation cycles, a half-cycle waveform is output, which is a low-frequency output waveform relative to the original waveform output of one and a half cycles; Line A is Figure 5 The waveform of the two waves after interference and superposition; when the waveform frequency of one of the first exciters 300 changes, the vibration law in the vibration enhancement area changes.

[0105] It is understandable that although the above Figure 5 , Figure 6 and Figure 7are schematic diagrams of waveforms of the two first exciters 300, but according to the content of the present invention and related embodiments, it can be verified that the changes in the waveform phase and frequency of the two second exciters 400 and the interference relationship are the same as Figure 5 , Figure 6 and Figure 7 Almost the same.

[0106] In summary, please refer to Figure 2 The present invention further provides a specific method for improving the molding quality of additive manufacturing, comprising the following steps:

[0107] Step S1, arranging the placement positions of the first vibration exciter 300 and the second vibration exciter 400 relative to the workpiece 100 according to the above-mentioned setting method;

[0108] Step S2, starting the first vibrator 300 according to the additive process of the workpiece 100, and driving the welding gun 200 to move on the top surface of the workpiece 100 to perform the additive operation; during the movement of the welding gun 200, the first vibrator 300 moves with the welding gun 200, and adjusts the movement position and superposition frequency of the first vibration reinforcement zone formed by the vibration waves of each pair of the first vibrators 300;

[0109] Step S3, when the material addition height of the workpiece 100 meets the requirements for the placement of the second vibrator 400 array and there is no equipment space interference, start the corresponding two second vibrators 400 according to the position of the welding gun 200 on the workpiece 100, and adjust the moving position and superposition frequency of the second vibration enhancement zone formed by the vibration waves of each pair of second vibrators 400, so that the first vibration enhancement zone formed by the vibration wave of the first vibrator 300 and the second vibration enhancement zone formed by the vibration wave of the second vibrator 400 are superimposed on each other, thereby generating coupled vibration to the molten pool 500;

[0110] Step S4: As each layer of the additive process is completed, the second vibrator 400 moves in the height direction;

[0111] The above steps S2 to S4 are repeated to sequentially complete the stacking and forming of each layer of the workpiece 100 until the additive manufacturing forming of the workpiece 100 is completed.

[0112] See also Figure 3 The present invention also provides a device for improving the molding quality of additive manufacturing, including a welding gun 200, a first vibrator 300 and a first driving member; at least one pair of first vibrators 300 are arranged beside a molten pool 500 formed by the welding gun 200 acting on a workpiece 100; the first driving member connects the welding gun 200 and each first vibrator 300) and can drive the welding gun 200 and each pair of first vibrators 300 to move together.

[0113] In some embodiments, see Figure 3The above-mentioned device for improving the molding quality of additive manufacturing also includes a second vibrator 400 and a second driving member; a plurality of second vibrators 400 are arranged on the side of the workpiece 100; the second driving member is respectively connected to each second vibrator 400, and can drive the second vibrator 400 to move along the height direction of the workpiece 100.

[0114] It should be noted that the specific operation process of the device for improving the molding quality of additive manufacturing is described in the above-mentioned method for improving the molding quality of additive manufacturing, and will not be repeated here.

[0115] It should be noted that the first driving member and the second driving member mentioned above can be components with driving force such as a cylinder, a hydraulic cylinder, an oil cylinder, a motor, etc.

[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for improving the molding quality of additive manufacturing, characterized in that: The following steps are involved: At least one pair of first vibrators (300) is arranged beside a molten pool (500) formed by a welding gun (200) acting on a workpiece (100); driving the first vibrator (300) to move following the welding gun (200) to perform an additive operation on the top surface of the workpiece (100); wherein the vibration waves of each pair of the first vibration exciters (300) are superimposed on each other to form a first vibration reinforcement zone acting on the molten pool (500), and the first vibration reinforcement zone can adjust the movement position and the superposition frequency based on the vibration parameters of each pair of the first vibration exciters (300); The vibration parameters of the first vibration exciter (300) include phase and frequency; Taking one of the first vibrators (300) in each pair as a reference, adjusting the phase of another first vibrator (300) to drive the first vibration reinforcement zone to move within the entire molten pool (500); and / or, Taking one of the first vibration exciters (300) in each pair as a reference, adjusting the frequency of another of the first vibration exciters (300) to control the superposition frequency of the first vibration reinforcement zone; The method for improving the additive manufacturing molding quality also includes the following steps: Arranging a plurality of second vibration exciters (400) on the side of the workpiece (100); When the height of the workpiece (100) increases, the second vibrator (400) is started, and the second vibrator (400) is raised and lowered as the height of the workpiece (100) increases; The vibration waves of two second vibrators (400) adjacent to the welding gun (200) can be superimposed on each other to form a second vibration enhancement zone acting on the molten pool (500), and the second vibration enhancement zone can adjust the movement position and superposition frequency based on the vibration parameters of the second vibrator (400); wherein the vibration wave transmission direction of the first vibration exciter (300) and the vibration wave transmission direction of the second vibration exciter (400) are arranged at an angle, so that a first vibration reinforcement zone formed by the vibration wave of the first vibration exciter (300) and a second vibration reinforcement zone formed by the vibration wave of the second vibration exciter (400) are superimposed on each other, thereby generating coupled vibration on the molten pool (500); The vibration parameters of the second vibration exciter (400) include phase and frequency; Of the two second vibrators (400) adjacent to the welding gun (200), taking one of the second vibrators (400) as a reference, adjusting the phase of the other second vibrator (400) to drive the second vibration reinforcement zone to move within the entire molten pool (500); and / or, Taking one of the second vibration exciters (400) as a reference, the frequency of another of the second vibration exciters (400) is adjusted to control the superposition frequency of the second vibration reinforcement zone.

2. The method for improving the molding quality of additive manufacturing according to claim 1, characterized in that: Under the placement condition that any two of the first vibrators (300) do not interfere with each other, at least one pair of the first vibrators (300) is provided, and the two first vibrators (300) in each pair are provided on the same side of the molten pool (500); or, the two first vibrators (300) in each pair are provided on both sides of the molten pool (500), respectively.

3. The method for improving the molding quality of additive manufacturing according to claim 2, characterized in that: Dividing all the first vibration exciters (300) into at least two groups, each group of the first vibration exciters (300) comprising at least one pair of first vibration exciters (300) arranged on both sides of the welding gun (200); The phase and vibration frequency of each pair of the first exciters (300) in the same group are the same; and the spacing between two adjacent groups of the first exciters (300) is at least a minimum integer multiple of the wavelength.

4. The method for improving the molding quality of additive manufacturing according to claim 3, characterized in that: The two groups of the first vibrators (300) are started in sequence according to the progress of the material addition operation of the workpiece (100); after the two groups of the first vibrators (300) are in contact with the workpiece (100), the waveform phases of the two groups of the first vibrators (300) remain the same.

5. The method for improving the molding quality of additive manufacturing according to any one of claims 1 to 4, characterized in that: The corresponding two second vibrators (400) are activated according to the position of the welding gun (200) on the workpiece (100), so that the molten pool (500) is always located in the second vibration enhancement zone formed by the mutual interference of vibration waves emitted by the two second vibrators (400).

6. The method for improving the molding quality of additive manufacturing according to any one of claims 1 to 4, characterized in that: include: Step S1, arranging the positions of the first vibration exciter (300) and the second vibration exciter (400) relative to the workpiece (100); Step S2, starting the first vibrator (300) according to the material addition process of the workpiece (100), and driving the welding gun (200) to move on the top surface of the workpiece (100) to perform the material addition operation; during the movement of the welding gun (200), the first vibrator (300) moves along with the welding gun (200), and regulates the movement position and superposition frequency of the first vibration reinforcement zone formed by the vibration waves of each pair of the first vibrator (300); Step S3, when the material addition height of the workpiece (100) meets the requirements for the placement of the second vibrator (400) array and there is no equipment space interference, start the corresponding two second vibrators (400) according to the position of the welding gun (200) on the workpiece (100), and adjust the movement position and superposition frequency of the second vibration enhancement zone formed by the vibration wave of each pair of the second vibrators (400), so that the first vibration enhancement zone formed by the vibration wave of the first vibrator (300) and the second vibration enhancement zone formed by the vibration wave of the second vibrator (400) are superimposed on each other, thereby generating coupled vibration on the molten pool (500); Step S4: as each layer of the material adding process is completed, the second vibrator (400) moves in the height direction; The above steps S2 to S4 are repeated to sequentially complete the stacking and forming of each layer of the workpiece (100) until the additive manufacturing forming of the workpiece (100) is completed.

7. A device for improving the quality of additive manufacturing, characterized in that: Used to perform the method for improving the additive manufacturing molding quality according to any one of claims 1 to 6; The device for improving the additive manufacturing molding quality comprises a welding gun (200), a first vibrator (300) and a first driving member; At least one pair of the first vibrators (300) is arranged beside a molten pool (500) formed when the welding gun (200) acts on a workpiece (100); The first driving member is connected to the welding gun (200) and each of the first vibrators (300), and is capable of driving the welding gun (200) and each pair of the first vibrators (300) to move together; The device for improving the molding quality of additive manufacturing further comprises a second vibrator (400) and a second driving member; A plurality of second vibration exciters (400) are arranged on a side surface of the workpiece (100); The second driving member is respectively connected to each of the second vibration exciters (400), and is capable of driving the second vibration exciters (400) to move along the height direction of the workpiece (100).