A method for densifying a ceramic matrix composite assembly
Through the assembly and separation method and the pin hole position design, the problem of uneven density in the density enhancement of the ceramic matrix composite assembly is solved, and the density uniformity and riveting effectiveness of the ceramic matrix composite assembly are achieved, which meets the Product performance requirements.
Patent Information
- Application Number
- CN202211369214.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-03
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-03
AI Technical Summary
It is difficult to achieve density uniformity in the process of density enhancement of existing ceramic matrix composite assembly, resulting in the inability to meet product requirements.
Using the method of assembly and splitting, first determine the accuracy of the temporary assembly of multiple parts, then split and perform CVI density separately to prepare the pin bottom hole and pin hole to ensure the accuracy and effectiveness of subsequent riveting welding, through bonding The agent and fixture are temporarily fixed and semi-finished to ensure that the surface of the part is clean and dense.
The density uniformity of ceramic matrix composite assembly is achieved, the operation is simplified, the scope of application is improved, and the effectiveness and density of riveting welding are ensured through precise pin hole position and interference coordination.
Abstract
Description
Technical Field
[0001] The invention relates to a method for densifying a material, and in particular to a method for densifying a ceramic-based composite material assembly. Background Art
[0002] Ceramic matrix composites are a new type of thermal structural / functional integrated material that combines the performance advantages of metal materials, ceramic materials and carbon materials. They have the characteristics of high temperature resistance, low density, high specific strength, high specific modulus, oxidation resistance, ablation resistance, insensitivity to cracks, and no catastrophic damage. They are widely used in the fields of machinery, aerospace, nuclear, and energy. Chemical vapor infiltration (CVI) is currently the only commercial method for manufacturing complex braided toughened CMCs. It has a wide range of adaptability and is applicable to all inorganic non-metallic materials in principle. This method can avoid damage to fibers caused by high temperatures and facilitates the manufacture of large, thin-walled, complex near-net-shape components.
[0003] At present, ceramic-based composite products are usually formed by forming a single part and then assembled and riveted. For parts with higher strength requirements or main load-bearing parts, multiple parts are generally stacked to form an assembly (an assembly refers to a stacked structure with ≥2 parts in the wall thickness direction) to improve the overall strength of ceramic-based composite products. When assembling the assembly, the surface of each part of the assembly needs to be polished and repaired. After polishing, the density of a single part decreases significantly. Usually, the assembled assembly will be densified by CVI. The final density and uniformity are crucial to the final performance of the ceramic-based composite assembly. However, the wall thickness of the assembly after stacking, repairing and riveting is relatively large. After densification by the CVI process, it is difficult to densify the internal parts in the assembly, resulting in uneven final density of the assembly, which is difficult to meet product requirements. Summary of the invention
[0004] The purpose of the present invention is to solve the technical problem that the existing method of densifying a ceramic-based composite assembly easily leads to uneven final density of the assembly and is difficult to meet product requirements, and to provide a method for densifying a ceramic-based composite assembly.
[0005] The technical solution of the present invention is as follows:
[0006] A method for densifying a ceramic matrix composite assembly, wherein the assembly comprises a plurality of parts stacked along the wall thickness direction of the assembly, and the method is special in that it comprises the following steps:
[0007] 1) For multiple parts that have reached the assembly density, repair them according to the assembly requirements to ensure that the assembly clearance meets the requirements;
[0008] 2) Multiple parts are superimposed into an assembly and temporarily fixed, then the assembly is clamped with a fixture, the assembly shape is semi-finished, and the subsequent assembly benchmark is determined;
[0009] 3) Disassemble the temporarily fixed assembly into multiple parts, and clean the surfaces of the multiple parts separately to ensure that the surfaces of the parts are clean and free of foreign matter;
[0010] 4) Perform CVI densification on multiple parts separately until the density meets the assembly requirements;
[0011] 5) According to the assembly datum determined in step 2), the multiple parts are reassembled into an assembly, and the multiple parts in the assembly are fixed by riveting and welding with pins.
[0012] Furthermore, it also includes steps 2-3):
[0013] After step 2) and before step 3, first determine the pin riveting position on the assembly, and then prepare the pin bottom hole for the finished assembly according to the pin riveting position;
[0014] The diameter of the pin bottom hole is d-(0.9-1.1) mm, d is the theoretical diameter of the pin, and d≥2 mm.
[0015] Furthermore, step 5) is specifically as follows: according to the assembly reference determined in step 2), multiple parts are reassembled into an assembly, and then the pin bottom hole prepared in step 2-3) is expanded into a pin hole, the diameter of the pin hole is d-(0.1~0.3) mm, and then the multiple parts in the assembly are fixed by riveting and welding by inserting the pin into the pin hole.
[0016] Further, in step 2), the diameter of the bottom hole of the pin is (d-1.0) mm;
[0017] In step 5), the diameter of the pinning hole is (d-0.2) mm.
[0018] Furthermore, in step 2), stacking the multiple parts into an assembly and temporarily fixing them means using an adhesive to bond the multiple parts into the assembly.
[0019] Furthermore, in step 2), the adhesive is 502 glue.
[0020] Furthermore, in step 2), the clamp is a bow-shaped clamp.
[0021] Furthermore, in step 2), the clamp is a bow-shaped clamp.
[0022] Beneficial effects of the present invention:
[0023] (1) The present invention provides a method for densifying a ceramic-based composite assembly, which adopts a method of combining assembly and disassembly. First, multiple parts are temporarily assembled to determine the assembly accuracy, and then each part is disassembled and densified separately to ensure that the density uniformity after assembly is better. The method is simple, highly operable, and has a wide range of applications.
[0024] (2) In a method for densifying a ceramic-based composite assembly of the present invention, a reference surface is processed on the assembly after the first assembly to ensure the accuracy of the position of the bottom hole of the pin during disassembly and reassembly.
[0025] (3) The present invention provides a method for densifying a ceramic-based composite assembly, which ensures accurate positioning of subsequent reassembly by preparing bottom holes for pins before disassembly.
[0026] (4) The densification method of a ceramic-based composite assembly of the present invention requires that the pin hole of the assembly before riveting is (d-0.2) mm, so that the pin and the pin hole are interference fit, thereby ensuring the effectiveness of riveting.
[0027] (5) A method for densifying a ceramic-based composite assembly of the present invention comprises preparing a pin bottom hole for the assembly and then disassembling it for deposition, which not only ensures the assembly requirements of subsequent parts, but also the pin bottom hole is conducive to the densification of subsequent parts;
[0028] (6) The present invention provides a method for densifying a ceramic-based composite assembly. Each part of the assembly is provided with a pin bottom hole, which can be used as a deposition vent during deposition, so that the density of the parts is deposited more evenly, thereby making the density of the assembly qualified and uniform. DETAILED DESCRIPTION
[0029] The present invention provides a densification method for a ceramic matrix composite assembly, which is to prepare a pin bottom hole after the product is repaired before riveting, and not rivet temporarily, separate the parts involved in the assembly and with the pin riveting bottom hole prepared, and perform CVI densification separately, expand the pin bottom hole after the density reaches the required value, and perform riveting and welding to form the final assembly product. The assembly of the present invention refers to a stacked structure formed by stacking multiple parts (≥2) along the wall thickness direction of the assembly.
[0030] The present invention provides a method for densifying a ceramic-based composite material assembly, comprising the following steps:
[0031] 1) For multiple parts that have reached the assembly density, repair them according to the assembly requirements to ensure that the assembly clearance meets the requirements;
[0032] 2) Use adhesive to bond and stack multiple parts into an assembly for temporary fixation. The adhesive can be 502 glue or other adhesives, and then clamp the assembly with a fixture. After the glue solidifies, semi-finish the assembly shape (semi-finishing is to complete the processing of secondary surfaces and prepare for the finishing of the main surfaces. The dimensional accuracy is close to the finishing state. When necessary, some dimensions and surfaces can be finished as needed), determine the subsequent assembly datum and the pin riveting position on the assembly; then prepare the pin bottom hole for the completed assembly according to the pin riveting position; the diameter of the pin bottom hole is d-(0.9~1.1)mm, d is the theoretical diameter of the pin, d≥2mm.
[0033] 3) Disassemble the temporarily fixed assembly into multiple parts, clean the surfaces of the multiple parts separately, remove surface scum, residual glue, etc., to ensure that the surface of the parts is clean and free of foreign matter;
[0034] 4) Perform CVI densification on multiple parts separately until the density reaches the assembly requirements;
[0035] 5) According to the assembly datum determined in step 2), the multiple parts are reassembled into an assembly, and then the prepared pin bottom hole is expanded into a pin hole, so that the diameter of the pin hole is d-(0.1~0.3)mm, so as to ensure an interference fit between the pin and the pin hole, and finally the pin is wedged into the pin hole with a certain preload force to fix the multiple parts in the assembly by riveting.
[0036] The core of the assembly densification method adopted by the present invention is the process method of assembly combined with disassembly, and the size requirements of the pin bottom hole before and after assembly are designed. In the method of the present invention, in order to ensure the correct riveting hole position after the assembly is disassembled and densified, 502 glue and bow clamps are used to temporarily fix the assembly, and then the temporarily fixed assembly is semi-finished, the benchmark is determined, and the final pin hole is reserved and prepared in the form of a bottom hole.
[0037] In order to ensure that no repair is required during the subsequent assembly of parts and to accelerate the densification of parts, the pin bottom hole needs to be prepared for the repaired and processed assembly according to the pin riveting position. The diameter of the pin bottom hole is d-(0.9~1.1)mm, where d is the theoretical diameter of the final pin.
[0038] The above method embodiment is described in detail below through a densification process of a specific product.
[0039] The load-bearing parts of a certain type of ceramic matrix composite product are composed of five superimposed parts, and the density of a single part reaches an assembly density of 1.9g / cm 3 After that, each part is repaired and polished. After repair and polishing, the density of each part decreases by 0.05-0.15g / cm 3502 glue is used to temporarily fix the repaired parts, and the assembly is clamped with clips such as bow clips. After the glue solidifies, the appearance of the assembly is semi-finished, and the subsequent assembly benchmark of the assembly is processed. The pin bottom hole is prepared according to the pin riveting position of the completed assembly. The pin bottom hole diameter is (d-1.0) mm, and then the temporarily fixed assembly is disassembled, and the surface scum and residual glue are cleaned. The 5 parts involved in the assembly are chemically vaporized using the MTS-H2 system. The silicon carbide substrate is deposited at a temperature of 950±50℃ and a deposition time of 200±50h. The vacuum is maintained at ≤500Pa throughout the process until the density reaches the final requirement. After the density of the five parts reaches the standard, they are reassembled according to the processed benchmark. The bottom hole of the pin is expanded to a pin hole. The diameter of the pin hole is (d-0.2)mm. The pin and the pin hole are ensured to have an interference fit. CVI chemical vapor deposition is performed with unchanged parameters and a deposition time of 250±20h. The vacuum is maintained at ≤500Pa throughout the process. The assembly is riveted and welded. The density of the assembly after riveting and welding reaches the standard and is uniform.
[0040] A certain type of ceramic-based composite material product prepared by this process has completed ground tests (static test, thermal test, vibration test). All performance of the product meets the use requirements, and there is no looseness or nail loss, which proves the reliability and feasibility of this method.
Claims
1. A method for densifying a ceramic matrix composite assembly, wherein the assembly comprises a plurality of parts stacked along the wall thickness direction of the assembly, characterized in that: The following steps are involved: 1) For multiple parts that have reached the assembly density, repair them according to the assembly requirements to ensure that the assembly clearance meets the requirements; 2) Multiple parts are stacked into an assembly for temporary fixation, and then the assembly is clamped with a fixture, and the assembly shape is semi-finished to determine the subsequent assembly benchmark; The said stacking of multiple parts into an assembly for temporary fixation means using 502 glue to bond and stack multiple parts into an assembly; the said clamp is a bow-shaped clamp; 2-3) First determine the pin riveting position on the assembly, and then prepare the pin bottom hole for the finished assembly according to the pin riveting position; The diameter of the pin bottom hole is d-(0.9~1.1) mm, d is the theoretical diameter of the pin, d≥2 mm; 3) Disassemble the temporarily fixed assembly into multiple parts, and clean the surfaces of the parts separately to ensure that the surfaces of the parts are clean and free of foreign matter; 4) Perform CVI densification on multiple parts separately until the density reaches the assembly requirements; 5) According to the assembly datum determined in step 2), multiple parts are reassembled into an assembly, and multiple parts in the assembly are fixed by riveting and welding with pins; specifically: According to the assembly datum determined in step 2), multiple parts are reassembled into an assembly, and then the pin bottom hole prepared in step 2-3) is expanded into a pin hole with a diameter of d-(0.1~0.3) mm. Then, pins are inserted into the pin holes to fix multiple parts in the assembly by riveting.
2. A method for densifying a ceramic matrix composite assembly according to claim 1, characterized in that: In step 2), the diameter of the bottom hole of the pin is (d-1.0) mm; In step 5), the diameter of the pin hole is (d-0.2) mm.