A method for preparing negative electrode material of ion battery using waste rubber as raw material

By crushing, cleaning, pyrolysis and solution treatment of waste rubber, the negative electrode material of lithium/sodium/potassium ion battery was prepared, which solved the problem of waste rubber recycling and achieved efficient carbon resource regeneration and electrochemical performance. Improvement, environmental protection and economic advantages.

CN115594167BActive Publication Date: 2024-10-01CHANGSHA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211326781.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-10-01
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

The recycling of waste rubber is difficult, especially due to its high degree of cross-linking and impurity content, which results in poor compatibility with matrix materials, making it difficult to process and separate. Existing treatment methods are costly, inefficient and cause secondary pollution.

Method used

It is prepared by crushing waste rubber into rubber powder, cleaning it with organic solution and vacuum drying, cooling it in a nitrogen or argon atmosphere after high-temperature pyrolysis, then treating it with an acidic or alkaline solution to remove impurities, and finally drying it under vacuum conditions. Develop negative electrode materials for lithium/sodium/potassium ion batteries.

Benefits of technology

It improves the impurity removal effect of zinc sulfide in waste rubber, maintains the electrochemical properties of carbon materials, and realizes high value-added utilization of waste rubber. It has short process flow, low cost, is green and environmentally friendly, and improves the utilization rate of waste rubber. and reduce environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115594167B_ABST
    Figure CN115594167B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing negative electrode materials for ion batteries using waste rubber as raw materials, comprising: crushing the rubber part of waste rubber products into rubber powder; washing the rubber powder with an organic solution for 2h~4h at a temperature of 30℃~60℃, filtering after washing; pyrolyzing the rubber powder at a high temperature of 700℃~1000℃, and obtaining a carbon material after cooling to room temperature; treating the carbon material with an acidic solution, an alkaline solution, sequentially using an acidic solution, an alkaline solution or sequentially using an alkaline solution, an acidic solution; or treating the carbon material with a mixed solution of an organic solvent and an alkaline solution, washing to neutrality; and vacuum drying the filtered product at a temperature of 80℃~120℃ for 6h~10h to obtain the obtained product. The invention regulates zinc sulfide in waste rubber, improves the impurity removal effect, and does not lose the electrochemical performance of the carbon material. The carbon material can be used as a negative electrode material for lithium / sodium / potassium ion batteries, turning waste rubber into treasure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste rubber regeneration, and relates to a method for preparing an ion battery negative electrode material using waste rubber as a raw material, which can be used for lithium / sodium / potassium ion batteries. Background Art

[0002] The large-scale stacking of waste tires will cause serious harm to the environment, mainly including: occupying a large amount of land resources, flammable when exposed to open flames, and easily breeding mosquitoes, carrying germs, and spreading diseases. Improving the comprehensive utilization rate of waste tires is an effective way to recycle and harmlessly dispose of these "solid wastes", which is of great significance to achieving "carbon peak" and "carbon neutrality". The recycling of waste tires needs to take advantage of the momentum and drive innovation to promote green development.

[0003] The recycling of waste rubber products is very difficult, especially waste tires. Rubber is a thermosetting material that cannot be directly cast into the desired shape by heating like thermoplastic materials used in plastic products. The vulcanization process of vulcanized rubber is a chemical process that converts natural rubber or related polymers into materials with more outstanding performance by adding vulcanizing agents. Such additives form a cross-linked network structure by forming cross-links (bridges) between polymer chains. Therefore, two other important substances that appear in the composition of rubber mixtures are sulfur (and its compounds) and zinc oxide, which are usually used as vulcanizing agents and vulcanization activators. The vulcanized rubber becomes a cross-linked structure containing a large number of CS, CC, SS bonds and cross-linked and entangled structures between polymer chains. In order to further improve the comprehensive performance, antioxidants, anti-corrosion agents, anti-ozonants and anti-aging agents are added to rubber products, so that rubber products have strong dynamic and static mechanical properties, and are resistant to oxidation, corrosion, biodegradation and ultraviolet rays, which greatly increases the difficulty of recycling and reuse of rubber resources. Waste rubber products contain a lot of impurities, and the degree of cross-linking between rubbers is high, making them difficult to handle and separate. When waste rubber is reused into other materials, its compatibility with the matrix material is poor, making it difficult to recycle.

[0004] At present, the main methods for disposing waste tires include refurbishment, landfill, incineration, pyrolysis, etc. Although they can achieve the purpose of recycling waste tire resources, they also have disadvantages such as high cost, low efficiency and utilization rate, and will cause secondary pollution. Using waste rubber as a carbon source to prepare high-value-added lithium-ion battery negative electrode materials can not only solve the environmental pollution problem caused by waste rubber, but also turn waste into treasure and improve the utilization rate of waste rubber, which has broad development prospects. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing negative electrode materials for ion batteries using waste rubber as raw material, which regulates zinc sulfide in waste rubber, improves the impurity removal effect, and does not lose the electrochemical properties of carbon materials. It can be used as a negative electrode material for lithium / sodium / potassium ion batteries, turning waste rubber into treasure, and solving the problems existing in the prior art.

[0006] The technical solution adopted by the present invention is a method for preparing negative electrode materials for ion batteries using waste rubber as raw materials, characterized in that it comprises the following steps:

[0007] S1: crushing the rubber parts of waste rubber products into rubber powder;

[0008] S2: at a temperature of 30°C to 60°C, wash the rubber powder with an organic solution for 2 h to 4 h, filter it after washing, and vacuum dry the filtered product at a temperature of 60°C to 120°C for 5 h to 12 h;

[0009] S3: Pyrolyze the rubber powder at 700℃~1000℃ for 1 h~5 h in a pyrolysis atmosphere of nitrogen or argon or a mixture of the two in any ratio, and then cool to room temperature to obtain a carbon material;

[0010] S4: treating the carbon material with an acidic solution or an alkaline solution, or sequentially treating with an acidic solution and an alkaline solution, or sequentially treating with an alkaline solution and an acidic solution; or treating with a mixture of an organic solvent and an alkaline solution, and washing to neutrality; the filtered product is vacuum dried at a temperature of 80°C to 120°C for 6 h to 10 h to obtain a waste rubber-based carbon negative electrode material, i.e., a negative electrode material for lithium / sodium / potassium ion batteries.

[0011] The beneficial effects of the present invention are:

[0012] 1. The embodiment of the present invention uses waste rubber as a carbon source, starting from the distribution and cross-linking mode between zinc sulfide and waste rubber carbon material particles, step by step reduces the agglomeration and coating between particles, regulates the zinc sulfide in the waste rubber, improves the impurity removal effect, and does not lose the electrochemical properties of the carbon material. The prepared negative electrode material can be applied to lithium / sodium / potassium ion batteries, and improves the electrochemical performance, thereby realizing high value-added applications of waste rubber.

[0013] 2. Compared with the traditional waste rubber treatment method, the embodiment of the present invention realizes waste utilization and is more environmentally friendly; the produced carbon negative electrode material has a short process flow and low overall cost, and has broad development space.

[0014] 3. The embodiments of the present invention improve the utilization rate of waste rubber. With the improvement of rubber performance, the recycling of rubber products after scrapping is becoming more and more difficult. For example, waste tires have complex components, which makes recycling difficult and has a low recycling rate. The present invention recycles waste rubber, improves its utilization rate, reduces environmental pollution and resource waste, and promotes the development of a circular economy. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 This is the XRD spectrum of the rubber powder after cleaning in Example 5.

[0017] Figure 2 This is the XRD spectrum of the waste rubber-based carbon material after cleaning in Example 11.

[0018] Figure 3a This is the EDS spectrum of the waste rubber-based carbon material prepared in Comparative Example 1.

[0019] Figure 3b This is the SEM image of the waste rubber-based carbon material prepared in Comparative Example 1.

[0020] Figure 4 The waste rubber-based carbon material prepared in Example 11 was assembled into a lithium-ion battery at 0.2 A g -1 Cycling performance diagram at different current densities.

[0021] Figure 5 The waste rubber-based carbon material prepared in Example 12 was assembled into a lithium-ion battery at 0.2 A g -1 Cycling performance diagram at different current densities.

[0022] Figure 6 The waste rubber-based carbon material prepared in Example 12 was assembled into a sodium ion battery at 0.05 A g -1 Cycling performance diagram at different current densities.

[0023] Figure 7 The waste rubber-based carbon material prepared in Example 12 was assembled into a potassium ion battery at 0.1 A g -1 Cycling performance diagram at different current densities.

[0024] Figure 8 This is the XRD spectrum of the waste rubber-based carbon material after cleaning in Example 12.

[0025] Fig. 9 It is a comparison diagram between Example 12 and Comparative Example 2. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] The basic concept of the embodiment of the present invention is as follows:

[0028] The zinc oxide in waste rubber is converted into zinc sulfide (ZnS) during high-temperature pyrolysis. ZnS has a high theoretical capacity, but it has poor conductivity and large electrochemical volume change. Poor conductivity and slow ion transfer rate make the material's irreversible specific capacity serious and the electrochemical performance is not ideal during high-rate charge and discharge.

[0029] ;

[0030] Secondly, during the charge and discharge process, ZnS will undergo severe volume expansion, causing the intrinsic material to split or even pulverize, and the contact between the active material and the electrode sheet to decrease, resulting in a rapid decrease in the reversible specific capacity of ZnS. When waste rubber is used as the raw material, the zinc sulfide impurities obtained have a high degree of cross-linking with carbon and are buried between carbon particles, making it difficult to remove the zinc sulfide impurities without losing the electrochemical properties of the carbon material.

[0031] The present invention provides a method for preparing an ion battery negative electrode material using waste rubber as a raw material, which is specifically carried out according to the following steps:

[0032] S1: Cut the rubber part of the waste rubber products and crush them into rubber powder with a particle size of 30-100 mesh; waste rubber products include waste tires, etc.; the methods for crushing waste rubber are: normal temperature (25℃) crushing method, low temperature (-120℃) crushing method, wet method or solution method.

[0033] S2: Wash the rubber powder with detergent at a temperature of 30℃~60℃ for 2 h~4 h, filter it after washing, and vacuum dry the filtered product at a temperature of 60℃~120℃ for 5 h~12 h.

[0034] The rubber powder contains impurities such as ZnO, SiO2, CaCO3, and a large amount of sulfur-containing organic matter. The washing liquid in step S2 is an organic solution, which is any one or more of acetonitrile, pyridine, methanol, ethanol, acetone, isopropanol, dichloromethane, toluene, ether, cyclohexane, N-methylpyrrolidone or N,N-dimethylformamide mixed in any proportion. The rubber powder can be swollen better, and organic and inorganic impurities in the rubber powder can be removed by washing.

[0035] S3: The washed rubber powder is pyrolyzed at high temperature in a lower tube furnace, and the carbon material is obtained after cooling to room temperature. The high temperature pyrolysis temperature is 700℃~1000℃, the high temperature pyrolysis time is 1 h~5 h, the high temperature pyrolysis heating rate is 1℃ / min~10℃ / min, and the high temperature pyrolysis atmosphere is one of nitrogen or argon or a mixture of the two in any ratio.

[0036] S4: The prepared carbon material is washed with a washing liquid at 30°C~200°C for 2 h~10 h, and the washing method is one or more of stirring washing, high-pressure washing or ultrasonic washing; after cleaning, it is washed with ultrapure water until neutral, filtered, and the filtered product is vacuum dried at a temperature of 80°C~120°C for 6 h~10 h to obtain a waste rubber-based carbon negative electrode material, i.e., a lithium / sodium / potassium ion battery negative electrode material.

[0037] In step S4, the washing liquid is an inorganic solution or an organic solution, and the inorganic solution includes any one or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, hydrochloric acid, nitric acid, phosphoric acid, sulfuric acid, boric acid, hydrogen peroxide, ultrapure water, etc. The organic solution includes any one or more of acetonitrile, pyridine, methanol, ethanol, acetone, isopropanol, dichloromethane, toluene, ether, cyclohexane, etc.

[0038] The carbon material in the embodiment of the present invention contains inorganic and organic impurities such as SiO2, ZnS, CaCO3, CaMg(CO3)2, MgSiO3 and iron-zinc sulfide. The ZnS content is regulated during the impurity removal process by using multiple solvents in combination with different physical diffusion, filling and chemical reaction methods.

[0039] Example 1

[0040] A method for preparing an ion battery negative electrode material using waste rubber as a raw material comprises the following steps:

[0041] S1: Crushing the rubber parts of waste tires into rubber powder with a particle size of 30-100 meshes;

[0042] S2: The rubber powder was washed with N-methylpyrrolidone solution at 60°C for 2 h, filtered after washing, and the filtered product was vacuum dried at 100°C for 10 h;

[0043] S3: The washed rubber powder was pyrolyzed at 850°C in a lower tube furnace for 3 h at a heating rate of 5°C / min in a nitrogen atmosphere; the carbon material was obtained after cooling to room temperature;

[0044] S4: The carbon material was stirred and cleaned with a hydrogen peroxide solution at 50 °C for 3 h, and then washed and filtered with ultrapure water until neutral; the filtered product was vacuum dried at 100 °C for 8 h to obtain a waste rubber-based carbon negative electrode material, i.e., a negative electrode material for lithium / sodium / potassium ion batteries. When used as a negative electrode material for lithium ion batteries, the specific capacity is 335 mA h g -1 , after 100 cycles, the capacity retention rate is about 82%.

[0045] Example 2

[0046] A method for preparing an ion battery negative electrode material using waste rubber as a raw material, except that in step S2, the rubber powder is washed with an N,N-dimethylformamide solution at a temperature of 30°C for 4 hours, and the filtered product is vacuum dried for 5 hours at a temperature of 120°C; except that in step S4, the prepared carbon material is ultrasonically washed with an ethanol solution at 80°C for 2 hours; the rest is the same as in Example 1.

[0047] The rubber powder contains impurities such as ZnO, SiO2, CaCO3 and a large amount of sulfur-containing organic matter. In step S2 of embodiments 1 and 2, washing with N-methylpyrrolidone solution and N,N-dimethylformamide solution can better swell the rubber powder, and the sulfur-containing organic matter impurities in the rubber powder can be removed by washing.

[0048] The negative electrode material prepared in Example 2 has a specific capacity of 352 mA hg when used as a negative electrode material for lithium ion batteries. -1 , after 100 cycles, the capacity retention rate is about 65%.

[0049] Example 3

[0050] A method for preparing negative electrode materials for lithium-ion batteries using waste rubber as raw materials, except that in step S3, the washed rubber powder is pyrolyzed at 1000°C in a tube furnace (argon atmosphere), the high-temperature pyrolysis time is 1 h, and the carbon material is obtained after cooling to room temperature, and the high-temperature pyrolysis heating rate is 1°C / min. The remaining steps are the same as those in Example 1. The obtained negative electrode material has a specific capacity of 319 mA hg when used as a negative electrode material for lithium-ion batteries. -1 , after 100 cycles, the capacity retention rate is about 63%.

[0051] Example 4

[0052] A method for preparing negative electrode materials for lithium-ion batteries using waste rubber as raw materials, except that the cleaned rubber powder is pyrolyzed in a tubular furnace at 700°C in step S3, the pyrolysis atmosphere is a mixture of argon and argon in a volume ratio of 1:1; the high-temperature pyrolysis time is 5 hours, and the carbon material is obtained after cooling to room temperature, and the high-temperature pyrolysis heating rate is 10°C / min. The remaining steps are the same as those in Example 1. The obtained negative electrode material has a specific capacity of 336 mA hg when used as a negative electrode material for lithium-ion batteries -1 , after 100 cycles, the capacity retention rate is about 64%.

[0053] Examples 3 and 4 investigate the effects of pyrolysis conditions on the morphology and properties of carbon materials, and produce carbon materials with excellent performance. When the temperature is too low (the lower limit of the temperature is 700°C), the material is partially pyrolyzed incompletely and contains many impurities, which affects the performance of the carbon as a negative electrode. When the temperature is too high (the upper limit of the temperature is 1000°C), the carbon material has a high degree of graphitization and the alkali metal ion storage sites are reduced.

[0054] Example 5

[0055] A method for preparing negative electrode materials for ion batteries using waste rubber as raw materials, except that in step S2, the rubber powder is washed with cyclohexane solution (mass concentration ≥ 99%) and anhydrous ethanol solution (mass concentration ≥ 99%) at 40°C for 3 h in sequence; after washing, the filtered product is vacuum dried at 60°C for 12 h; except that in step S4, the prepared carbon material is stirred and washed with 2 mol / L nitric acid solution at 30°C for 4 h, and after washing, it is washed and filtered with ultrapure water until neutral; the rest is the same as in Example 1. If the concentration of the cyclohexane solution and the anhydrous ethanol solution is too low, the washing effect is not good; if the concentration of the nitric acid solution is too low, the washing effect cannot be achieved; if the concentration is too high, the corrosiveness is too strong, the danger increases sharply, and the cost increases at the same time.

[0056] Example 5 The XRD spectrum of the rubber powder after cleaning is as follows: Figure 1 As shown, according to Figure 1 It can be seen that the rubber powder contains fewer impurities. By comparing with the standard card (PDF card: 75-1526), ​​the main impurity contained in the cleaned rubber powder is ZnO, which shows that the impurity removal effect of this embodiment is better.

[0057] Two or more molecules or ions containing lone pairs of electrons (or π bonds) are used as ligands to combine with central atoms or ions with empty valence electron orbitals to form structural units. In this embodiment, cyclohexane solution and anhydrous ethanol solution are used to wash the rubber powder in turn. Cyclohexane reacts with metal ions such as iron, copper, aluminum, calcium, and magnesium in the rubber powder to separate these metal ions from other substances and remove impurities. Ethanol is a very good solvent that can dissolve many inorganic substances and many organic substances, so that both organic and inorganic substances can be dissolved, increasing the contact area between the solvent and the rubber powder and increasing the reaction rate. The carbon material is treated with a strong oxidizing acid, and the carbon material is oxidized to generate hydrophilic functional groups such as hydroxyl, carbonyl, and carboxyl. First, this carrier has good hydrophilicity and can be infiltrated with metal precursors (i.e., metal ions such as iron, copper, aluminum, calcium, and magnesium). Second, the loaded metal is stably present under the anchoring effect of these functional groups without agglomeration.

[0058] If only cyclohexane solution is used for treatment, the other steps are the same as those in Example 5, and the specific capacity of the waste rubber-based carbon negative electrode material as the negative electrode material of lithium-ion battery is 327 mA h g -1 , after 100 cycles, the capacity retention rate is about 66%.

[0059] Example 6

[0060] A method for preparing negative electrode materials for ion batteries using waste rubber as raw materials, except that in step S2, the rubber powder is washed with acetonitrile solution (mass concentration ≥ 99%) and toluene solution (mass concentration ≥ 99%) at 40°C for 3 h; except that in step S4, the prepared carbon material is stirred and washed with 4 mol / L sulfuric acid solution at 60°C for 2 h, and then washed and filtered with ultrapure water until neutral; the rest is the same as in Example 1. The specific capacity of the prepared negative electrode material as a negative electrode material for lithium ion batteries is 361 mA hg -1 , after 100 cycles, the capacity retention rate is about 79%.

[0061] Acetonitrile can dissolve a variety of organic, inorganic and gaseous substances (such as sulfur-containing organic matter, ZnO, SiO2, CaCO3 and other impurities), and toluene can be used as a solvent in large quantities; sulfuric acid is one of the most active binary inorganic strong acids and can react with many metals. Sulfuric acid will also cause structural disorder and increase porosity.

[0062] The concentrations of acetonitrile solution and toluene solution are lower than their corresponding ranges, and the cleaning effect is poor; the concentration of sulfuric acid solution is too low to achieve the cleaning effect, and the concentration is too high and the corrosiveness is too strong, the danger increases dramatically, and the cost increases.

[0063] Example 7

[0064] A method for preparing negative electrode materials for lithium ion batteries using waste rubber as raw materials, except that in step S4, the prepared carbon material is stirred and washed with 8 mol / L sulfuric acid solution and 3 mol / L sodium hydroxide solution at 40°C for 3 h, and then washed and filtered with ultrapure water until neutral; the filtered product is vacuum dried at 80°C for 8 h; the rest is the same as in Example 1. The specific capacity of the obtained negative electrode material as a negative electrode material for lithium ion batteries is 375 mA hg -1 , after 100 cycles, the capacity retention rate is about 83%.

[0065] Sodium hydroxide is a strong alkali with strong corrosiveness. It is easily soluble in water (releases heat when dissolved in water) and forms an alkaline solution. It is also deliquescent and easily absorbs water vapor and carbon dioxide in the air. It undergoes disproportionate reactions with halogens such as chlorine, bromine, and iodine, and neutralizes with acids to generate salt and water. The concentration of sulfuric acid solution is 7 mol / L~9 mol / L, and the concentration of sodium hydroxide solution is 2 mol / L~4 mol / L. If the concentration of sulfuric acid solution and sodium hydroxide solution is too low, the cleaning effect cannot be achieved. If the concentration is too high, the corrosion is too strong, the danger increases dramatically, and the cost increases at the same time. ZnS+H2SO4=ZnSO4+H2S↑, using strong acid to make weak acid, reducing zinc sulfide, but there is still obvious residue. The residual impurities are brought into the negative electrode material, which will cause the negative electrode material to expand too much during the insertion and removal process, affecting its electrochemical performance.

[0066] Example 8

[0067] A method for preparing negative electrode materials for lithium-ion batteries using waste rubber as raw materials, except that in step S4, the prepared carbon material is sequentially stirred and washed with 1 mol / L sodium hydroxide solution and 3 mol / L hydrochloric acid solution at 40°C for 3 h, and then washed and filtered with ultrapure water until neutral; the filtered product is vacuum dried at 120°C for 6 h; the rest is the same as in Example 1. The obtained negative electrode material has a specific capacity of 379 mA hg when used as a negative electrode material for lithium-ion batteries. -1 , after 100 cycles, the capacity retention rate is about 84%.

[0068] Hydrochloric acid is a strong acid that reacts with certain metals, metal oxides, metal hydroxides, and most metal salts (iron, copper, aluminum, calcium, magnesium and other metal ions and their oxides and hydroxides) to form hydrochlorides. The concentration of sodium hydroxide solution is 1 mol / L~2 mol / L, and the concentration of hydrochloric acid solution is 3 mol / L~6 mol / L. If the concentration is too low, the cleaning effect cannot be achieved. If the concentration is too high, the corrosion is too strong, the danger increases dramatically, and the cost increases.

[0069] Example 9

[0070] A method for preparing negative electrode materials for lithium-ion batteries using waste rubber as raw materials, except that in step S4, the prepared carbon material is ultrasonically washed with a 2 mol / L sodium hydroxide alcohol solution at 50°C for 2 h, washed and filtered with ultrapure water until neutral; the filtered product is vacuum dried at 80°C for 9 h; the rest is the same as in Example 2. The prepared negative electrode material has a specific capacity of 381 mAh g when used as a negative electrode material for lithium-ion batteries. -1 , after 100 cycles, the capacity retention rate is about 84%. The sodium hydroxide alcohol solution is an ethanol solution of sodium hydroxide, and the mass fraction of sodium hydroxide in the 2 mol / L~4 mol / L sodium hydroxide alcohol solution is 8%~12% in the ethanol solution of sodium hydroxide.

[0071] Some substances (such as sulfur-containing organic matter) are insoluble in water but soluble in ethanol, so an ethanol solution of sodium hydroxide is used for the reaction, the reaction temperature is 40℃~60℃, and the ultrasonic time is 1 h~3 h; the concentration of the ethanol solution of sodium hydroxide is too low, and the cleaning effect is not good. Example 9 can adjust the ZnS content, and the effect is better than that of Example 5; Example 9 uses an organic solvent as a medium. Compared with water, the organic solvent has a smaller contact angle with the carbon material, which can better infiltrate and contact the carbon material, thereby making the regulation effect better.

[0072] Example 10

[0073] A method for preparing negative electrode materials for lithium ion batteries using waste rubber as raw materials, except that in step S4, the prepared carbon material is stirred and washed with toluene solution (mass concentration ≥ 99%), 2 mol / L potassium hydroxide solution, and 5 mol / L phosphoric acid solution at 30°C for 3 h; after washing, it is washed and filtered with ultrapure water until neutral; the filtered product is vacuum dried at a temperature of 120°C for 6 h; the rest is the same as in Example 1. The prepared negative electrode material has a specific capacity of 378 mA hg when used as a negative electrode material for lithium ion batteries. -1 , after 100 cycles, the capacity retention rate is about 81%.

[0074] Phosphoric acid is a tribasic acid and a medium-strong acid. Phosphate ions have a strong coordination ability and can form soluble complexes with many metal ions (such as iron, copper, aluminum, calcium, magnesium and other metal ions). In the embodiment, the concentration of phosphoric acid is 3 mol / L~6 mol / L, the concentration of potassium hydroxide solution is 2 mol / L~4 mol / L, the reaction temperature is 30°C~60°C, and the reaction time is 1 h~3 h.

[0075] In Examples 6-10, in step S4, acidic and alkaline solutions are used respectively, and acidic and alkaline solutions are used in sequence, or alkaline and acidic solutions are used in sequence for treatment, which can effectively regulate the zinc sulfide in the shallow layer and on the surface. Among them, Examples 6 and 10 explore the influence of non-strong oxidizing acids and medium-strong acids. Acids with excessively strong oxidizing properties may oxidize carbon materials, and the use of non-strong acid cleaning can effectively remove residual alkali. The principle of regulating zinc sulfide in Examples 6 and 10 is that zinc sulfide can react with strong acids and strong bases, but strong oxidizing acids will cause certain oxidation to carbon materials, affecting the performance of carbon materials. At the same time, the residual acid will also affect the performance of carbon materials. By exploring the regulating role and effect of non-strong oxidizing acids and medium-strong acids, the regulation efficiency can be improved.

[0076] Examples 7 and 9 explore the effects of using different acid and alkaline solutions in different orders to form partial zinc hydroxide colloids on regulation. In a weakly alkaline environment, zinc sulfide will be partially converted into zinc hydroxide colloids, which can be converted into zincate and dissolved and washed away by acid washing after alkali washing. Example 9 explores the effects of organic solvents on the contact angle of carbon particles in materials. Aqueous solutions cannot achieve good infiltration and contact with rubber powder carbon materials, while organic solvents can improve the infiltration effect.

[0077] Embodiment 11

[0078] A method for preparing an ion battery negative electrode material using waste rubber as a raw material, except that in step S2, the rubber powder is washed with a pyridine solution (mass concentration ≥ 99) and an isopropanol solution (mass concentration ≥ 99%) at 40°C for 3 h in sequence; except that in step S4, the prepared carbon material is washed with a 3 mol / L sodium hydroxide alcohol solution at 120°C by a solvent thermal method for 8 h, then washed with a 4 mol / L hydrochloric acid solution at 30°C for 2 h with stirring, and washed with ultrapure water and filtered until neutral; the filtered product is vacuum dried at 100°C for 10 h; the rest is the same as Example 1.

[0079] The XRD spectrum of the waste rubber-based carbon material obtained in Example 11 is as follows: Figure 2 As shown, it can be seen that the waste rubber-based carbon material contains two obvious carbon peaks, 2θ=24° and 43°, which correspond to the diffraction peaks of the (002) and (100) crystal planes, respectively, and only a small amount of ZnS diffraction peaks, indicating that this embodiment has a good cleaning and impurity removal effect on the waste rubber-based carbon material and a good regulation effect on zinc sulfide.

[0080] The cycle performance of the lithium / sodium / potassium ion battery assembled from the waste rubber-based carbon material prepared in Example 11 is as follows: Figure 4 As shown in the figure, it can be seen that when used as a negative electrode material for lithium-ion batteries, the specific capacity is maintained at 380 mAh g -1 It is about 2.5 times higher than commercial graphite, and also has excellent electrochemical performance when used as anode materials for sodium / potassium ion batteries.

[0081] In this embodiment, the solvent thermal method is to use 2 mol / L~4 mol / L of sodium hydroxide alcohol solution to clean by solvent thermal method at 100℃~140℃ for 6 h~10 h. The solvent thermal method can control the formation of carbon material phase, particle size and morphology, and the product has good dispersibility. Under solvent thermal conditions, the properties of the solvent (density, viscosity, dispersion) affect each other, and its properties are very different from those under normal conditions. The dissolution, dispersion and chemical reaction activity of the reactants are greatly improved or enhanced, which enables the cleaning with 3 mol / L~5 mol / L hydrochloric acid in step S4 to be carried out at a lower temperature (40℃~60℃) and the cleaning time is 1 h~3 h.

[0082] Example 12

[0083] A method for preparing negative electrode materials for ion batteries using waste rubber as raw material, except that in step S3, the cleaned rubber powder is pyrolyzed at high temperature in a tubular furnace (nitrogen atmosphere) at a temperature of 900°C for 3 hours, and the carbon material is obtained after cooling to room temperature. Except that in step S4, the prepared carbon material is hydrothermally cleaned with an ultrapure aqueous solution at 120°C for 14 hours, and then ultrasonically cleaned with a 4 mol / L sodium hydroxide alcohol solution at 50°C for 2 hours, with an ultrasonic frequency of 20-130 KHz; filtered and separated, added to a 4 mol / L hydrochloric acid solution, cleaned for 3 hours, washed with ultrapure water and filtered until neutral; the filtered product is vacuum dried at a temperature of 120°C for 7 hours; the rest is the same as Example 2. The obtained negative electrode material has excellent performance in lithium-ion batteries, sodium-ion batteries, and potassium-ion batteries, among which the specific capacity of the negative electrode material used in lithium-ion batteries is maintained at 410 mA hg -1 Applied in sodium ion batteries, the specific capacity is maintained at 210 mA hg -1 Applied in potassium ion batteries, the specific capacity is maintained at 180 mA hg -1 After 100 cycles, the capacity retention rate is above 90%. Figure 5 , Figure 6 and Figure 7 shown.

[0084] The XRD spectrum of the waste rubber-based carbon material obtained in Example 12 is as follows: Figure 8 As shown, it can be seen that the waste rubber-based carbon material contains only two obvious carbon peaks, 2θ=24° and 43°, which correspond to the diffraction peaks of the (002) and (100) crystal planes, respectively, and no other impurity peaks, indicating that this embodiment has a good cleaning and impurity removal effect on the waste rubber-based carbon material and a good regulation effect on zinc sulfide.

[0085] Zinc sulfide expands during the charge and discharge cycle, which can cause the collapse of the electrode material structure and a decrease in battery performance. The excellent regulatory effect of zinc sulfide can be reflected in the battery cycle performance and capacity retention rate.

[0086] In this embodiment, ultrapure water is first used for hydrothermal cleaning at 100°C~140°C for 12 h~15 h to remove some water-soluble impurities and reduce the agglomeration degree of the carbon powder particles. Then, high-energy ultrasound is used with an ultrasonic frequency of 20~130 KHz, and an ethanol solution of sodium hydroxide is used for ultrasonic washing at 40°C~60°C for 1 h~3 h to further depolymerize and dissolve the stripped zinc sulfide impurities. Finally, 3 mol / L~5 mol / L hydrochloric acid is used for washing to remove residual sulfide ions. Ultrapure water is used for washing until neutral to obtain a high-performance carbon negative electrode material, which significantly reduces the zinc sulfide impurity content and obtains amorphous carbon with good electrochemical properties.

[0087] Comparative Example 1

[0088] A method for preparing an ion battery negative electrode material using waste rubber as a raw material is specifically carried out according to the following steps:

[0089] S1: Under normal temperature conditions, use a wire bead stripping machine to remove the tire bead and a magnetic separator to remove iron impurities, and then use a crusher to crush the waste tire into 90 mesh rubber powder.

[0090] S2: Wash the rubber powder with ethanol solution at 30°C for 3 h, filter it after washing, and dry the filtered product in vacuum at 100°C for 10 h.

[0091] S3: The washed rubber powder was pyrolyzed at 850°C in a tubular furnace (nitrogen atmosphere) for 3 hours, and the carbon material was obtained after cooling to room temperature.

[0092] S4: The carbon material is hydrothermally cleaned with an ultrapure aqueous solution at 120°C for 10 h, filtered after cleaning, and the filtered product is vacuum dried at 120°C for 12 h to obtain a waste rubber-based carbon material, i.e., a negative electrode material for lithium / sodium / potassium ion batteries.

[0093] The SEM images and EDS spectra of the prepared waste rubber-based carbon materials are as follows: Figure 3a-3b As shown, it means that waste rubber-based carbon materials contain some sulfur and zinc elements. Zinc sulfide negative electrode materials have a higher specific capacity, but they will produce certain expansion during the cycle, resulting in unstable performance of the negative electrode material, which is one of the main impurities for regulation.

[0094] Comparative Example 2

[0095] A method for preparing an ion battery negative electrode material using waste rubber as a raw material is specifically carried out according to the following steps:

[0096] S1: Under normal temperature conditions, use a wire bead stripping machine to remove the tire bead and a magnetic separator to remove iron impurities, and then use a crusher to crush the waste tire into 90 mesh rubber powder.

[0097] S2: The washed rubber powder was pyrolyzed at 850°C in a tubular furnace (nitrogen atmosphere) for 3 hours, and the carbon material was obtained after cooling to room temperature.

[0098] In this embodiment, the rubber powder is directly pyrolyzed without any impurity removal process; Fig. 9 As shown, when the prepared carbon material is used as a negative electrode material for a lithium-ion battery, the cycle performance of the battery is significantly lower than that of Example 12.

[0099] Comparative Example 3

[0100] A method for preparing negative electrode materials for ion batteries using waste rubber as raw material, except that in step S4, the prepared carbon material is stirred and washed with an alcohol solution at 30°C for 2 h, and dried at 80°C for 6 h to obtain a waste rubber-based carbon material, and the rest is the same as Example 11. Only part of the organic impurities can be washed away, and the ZnS content cannot be effectively regulated, resulting in unsatisfactory cycle performance of the obtained negative electrode material. The initial specific capacity of the obtained negative electrode material is 380 mA h g -1 However, after 50 cycles, the specific capacity dropped to 300 mA h g -1 After 100 cycles, the capacity retention rate dropped to less than 30%, indicating that simple alcohol solution cleaning cannot regulate the zinc sulfide with a certain degree of cross-linking coating with the carbon material.

[0101] Comparative Example 4

[0102] A method for preparing negative electrode materials for ion batteries using waste rubber as raw materials, except that in step S4, the prepared carbon material is ultrasonically cleaned with ether solution (mass concentration ≥ 99%) at 20°C for 2 h; the rest is the same as Example 2. Ether can be oxidized into peroxides, aldehydes and acetic acid under the action of air, and exposure to light can promote its oxidation. Only part of the organic impurities can be washed away, and the ZnS content cannot be effectively regulated, resulting in unsatisfactory cycle performance of the obtained negative electrode material. The initial specific capacity of the obtained negative electrode material is 380 mA h g -1 However, after 50 cycles, the specific capacity dropped to 300 mA h g -1 Below, the capacity retention rate drops below 30% after 100 cycles.

[0103] Compared with Comparative Examples 1-3, the initial specific capacity of the negative electrode material prepared in the present invention is 360-380 mA h g -1 , the capacity retention rate is above 80% after about 100 cycles.

[0104] The embodiment of the present invention starts from the distribution and cross-linking mode between zinc sulfide and waste rubber carbon material particles, gradually reduces the agglomeration and coating between particles, and then utilizes the difference in chemical properties of impurities between different solvents, selects different solutions for physical means and chemical reaction impurity regulation, uses multiple solvents, combines different physical diffusion, filling and chemical reaction methods, and adjusts appropriate temperature and pressure at the same time, ultimately achieving the purpose of reducing zinc sulfide impurities, deeply regulating the impurity content and microstructure of waste rubber-based carbon materials, and regulating zinc sulfide without affecting the electrochemical properties of waste rubber-based carbon materials. A variety of inorganic and organic impurities are removed. The obtained waste rubber-based carbon negative electrode material is successfully used in three alkali metal ion battery negative electrode materials of lithium, sodium and potassium, and improves its electrochemical performance as an ion negative electrode material; it can not only solve the environmental pollution problem caused by waste tires, but also turn waste into treasure and improve the utilization rate of waste tires.

[0105] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing negative electrode materials for ion batteries using waste rubber as raw materials, characterized in that: The following steps are involved: S1: crushing the rubber parts of waste rubber products into rubber powder; S2: at a temperature of 30°C to 60°C, wash the rubber powder with an organic solution for 2 h to 4 h, filter it after washing, and vacuum dry the filtered product at a temperature of 60°C to 120°C for 5 h to 12 h; S3: Pyrolyze the rubber powder at 700℃~1000℃ for 1 h~5 h in a pyrolysis atmosphere of nitrogen or argon or a mixture of the two in any ratio, and then cool to room temperature to obtain a carbon material; S4: The prepared carbon material is hydrothermally cleaned with an ultrapure aqueous solution at 100°C~140°C for 12 h~15 h, and then ultrasonically cleaned with a 2 mol / L~4 mol / L sodium hydroxide alcohol solution at 40°C~60°C for 1 h~3 h, with an ultrasonic frequency of 20~130KHz; filtered and separated, added to a 3 mol / L~5 mol / L hydrochloric acid solution, cleaned for 1 h~3 h, and washed with water and filtered until neutral; the filtered product is vacuum dried at a temperature of 80°C~120°C for 7 h~9 h to obtain a waste rubber-based carbon negative electrode material, i.e., a negative electrode material for lithium / sodium / potassium ion batteries; In S2, the organic solution is any one or more of acetonitrile, pyridine, methanol, ethanol, acetone, isopropanol, dichloromethane, toluene, ether, cyclohexane, N-methylpyrrolidone or N,N-dimethylformamide mixed in any proportion.

2. The method for preparing negative electrode materials for ion batteries using waste rubber as raw materials according to claim 1, characterized in that: In the S4, the prepared carbon material is cleaned by a solvent thermal method at 100°C to 140°C with a 2 mol / L to 4 mol / L sodium hydroxide alcohol solution for 6 h to 10 h, then cleaned by stirring with a 3 mol / L to 5 mol / L hydrochloric acid solution at 40°C to 60°C for 1 h to 3 h, and then washed with water and filtered until neutral; the filtered product is vacuum dried at a temperature of 80°C to 120°C for 6 h to 10 h to obtain a waste rubber-based carbon negative electrode material, i.e., a lithium / sodium / potassium ion battery negative electrode material.

3. The method for preparing negative electrode materials for ion batteries using waste rubber as raw materials according to claim 1, characterized in that: In S1, the method for crushing the waste rubber is: crushing method, wet method or solution method, and the particle size of the rubber powder is 30 mesh to 100 mesh.

4. The method for preparing negative electrode materials for ion batteries using waste rubber as raw materials according to claim 1, characterized in that: In S2, the rubber powder is washed with a cyclohexane solution with a mass concentration of ≥99% and an anhydrous ethanol solution with a mass concentration of ≥99% at a temperature of 30° C. to 60° C. for 2 h to 4 h.

5. The method for preparing negative electrode materials for ion batteries using waste rubber as raw materials according to claim 1, characterized in that: In S3, the high temperature pyrolysis heating rate is 1°C / min to 10°C / min.