Method for synthesizing amorphous silicon oxide coated nickel powder with assistance of chemical precipitation and atomization granulation
By coating amorphous silicon oxide onto the surface of Ni powder through chemical precipitation and atomization granulation, core/shell structured Ni@SiO2 particles are formed, which solves the problem of mismatch between oxidation and sintering shrinkage rate of Ni internal electrodes and improves the electrode performance and service life of MLCCs.
Patent Information
- Application Number
- CN202411016818.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies for preparing Ni internal electrodes for MLCCs suffer from problems such as easy oxidation of Ni powder, mismatch between Ni powder and ceramic sintering shrinkage, and interpenetration and reaction at the interface with dielectric ceramics, which limit the lifespan and performance of capacitors.
A chemical precipitation and atomization granulation method was adopted, using silicate as the Si source and inorganic acid as the precipitant to prepare a mixture of silica gel colloid and nano/submicron Ni powder. Amorphous silicon oxide was coated on the surface of Ni powder by spray drying to form core/shell structured Ni@SiO2 particles, thereby controlling the particle size and distribution.
This improved the oxidation resistance and sintering performance of Ni powder, enhanced the interfacial bonding between the Ni electrode and the ceramic dielectric layer, reduced internal stress, and improved electrode continuity and product qualification rate.
Smart Images

Figure CN118926523A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal powder material preparation, and relates to a method for synthesizing amorphous silicon oxide-coated nickel powder assisted by chemical precipitation and atomization granulation. The prepared metal powder has good oxidation resistance and sintering performance. Background Art
[0002] Multilayer ceramic capacitors (MLCC, Multilayer Ceramic Capacitors) are made of ceramic dielectric diaphragms with printed electrodes (inner electrodes) stacked in a staggered manner, and then sintered at high temperature once to form a ceramic chip, and then sealed with a metal layer (outer electrode) at both ends of the chip to form a monolithic structure, so it is also called a monolithic capacitor. MLCC is one of the most common and widely used electronic components in electronic equipment. It is widely used in bypass, filtering, tuning circuit, DC isolation, coupling, energy conversion, control circuit and other circuits. The output accounts for more than 40% of the total electronic components. It has great application value in information, military, mobile communications, electronic appliances, aviation, oil exploration and other industries, and has promoted the research on miniaturization, high performance, high reliability and low power consumption of electronic components. It has become an important electronic control component in my country's electronic information components. Initially, in order to perform high-temperature sintering in air, components such as MLCC, MLVC and PTCR used pure platinum (Pt) or pure palladium (Pd) as the inner electrode because they are not easy to oxidize at high temperatures and have stable performance. However, with the development of the electronics industry, the demand for higher performance of electronic components has been increasing, and the number of layers of multilayer chip components has gradually increased, resulting in a surge in the use of precious metals in production and an increase in the proportion of electrode costs. This has prompted people to study cheaper internal electrode materials to replace expensive pure platinum or pure palladium, and the research and application of base metal electrodes has emerged.
[0003] Ni powder has the characteristics of low cost, high conductivity, low electrical mobility, good corrosion resistance and heat resistance to solder, and high sintering temperature. It is currently the most widely used electrode material in MLCC. Therefore, the preparation of Ni powder is the key technology for the preparation of Ni internal electrode slurry for MLCC. However, in actual application, Ni internal electrodes have key problems such as easy oxidation, mismatch with the sintering shrinkage rate of ceramics, and interpenetration and reaction with the dielectric ceramic interface, which seriously affect the service life and performance of capacitors.
[0004] At present, there are two main methods to improve the performance of metal Ni powder. One is to improve the microstructure (crystallinity, particle size, etc.) of Ni powder. Ni powder with high crystallinity has good oxidation resistance, while Ni powder with smaller particle size can form dense and smooth Ni electrodes at lower sintering temperatures, which is more suitable for MLCC internal electrode slurry. The other is to modify the surface of Ni powder. A common method is to form a coating layer on its surface, such as CaZrO3, SrZrO3, ZrO2, Bi2O3, CaCO3, BaO, Cr2O3, TiO2, SiO2, etc., to improve its oxidation resistance and solve the problem of mismatch with the sintering shrinkage rate of ceramics. This method is currently the most widely used and most effective method. In patent JP2004183027A, a layer of BaTiO3 ceramic dielectric material is coated on the surface of Ni powder by chemical method, which improves its antioxidant performance and sintering performance to a certain extent, but its operation process is complicated and the coating effect is poor; patent CN103508736 A discloses a two-step method for modifying the surface of Ni powder, using two methods of normal pressure coating hydrothermal crystallization and normal pressure coating crystallization to coat the surface of nickel powder particles with a barium titanate layer, and the antioxidant and sintering properties are effectively improved, but the addition of too many chemicals increases its production cost and is not suitable for large-scale production. Patent CN117583598A uses a DC plasma arc method to coat a layer of amorphous silicon oxide on the surface of Ni, which greatly improves the shrinkage performance of Ni electrodes, but its preparation process has low yield and high energy consumption. Patent CN116516384A uses organic polysilazane as a silicon source to prepare a silicon dioxide shell on the surface of metals such as Ni and Cu, but the large-scale use of organic matter will cause certain pollution to the environment. In the process of preparing composite materials, core-shell structures, etc., the synthesis method is crucial. Common synthesis methods such as chemical vapor deposition, sol-gel method, hydrothermal method, etc., all have certain limitations, are complex to operate, involve many chemicals, and are not suitable for large-scale production.
[0005] As a versatile tool, spray drying has shown the potential to expand to an industrial scale. The technology was first used in the pharmaceutical field to produce pure APIs. It has a simple operating process, can be scalable, has a high yield, and has little impact on the environment. Subsequently, its application areas quickly expanded to other industries such as cosmetics, fabrics, electronic materials, microcapsules, controlled-release particles, composite particles, nanoparticles, and liposomes. Spray drying technology has gradually developed into a technology with high efficiency, simple procedures, convenience, simple structure, small volume, and excellent product quality. Spray drying technology can adjust the microstructure, particle distribution, and performance of the powder by controlling process parameters such as air inlet temperature, feed rate, gas flow rate, and gas medium. The productivity is high, the obtained particles have good dispersibility, and the thickness uniformity of the coating layer can be controlled. In patent CN106684346A, the electrode material C coating is prepared by spray drying, which effectively realizes the preparation of the C coating layer. In CN117317218 A, after intermittent ball milling by solid phase ball milling, a carbon source is added, spray drying is performed, and high temperature sintering is performed to obtain a carbon-coated lithium iron manganese phosphate positive electrode material. The obtained carbon-coated lithium iron manganese phosphate positive electrode material has a stable structure, perfect particles, and secondary particles are evenly arranged on the surface of primary particles, so that carbon is evenly coated on the surface of the positive electrode material. Compared with other oxides, silicon dioxide has higher anti-oxidation and corrosion resistance stability, and its shell layer has the advantages of non-toxicity, high inertness, easy to combine with various functional groups, and good coupling with nanoparticles, and can better realize the combination with the dielectric ceramic layer. In the subsequent preparation of Ni slurry, SiO2 itself is added to the Ni slurry as an inorganic binder, and no new impurities or additives are introduced, so as to avoid a series of sintering problems that may be caused by new components in the subsequent sintering process. In addition, amorphous silicon dioxide is used as an additive component of the glass phase or dielectric ceramic layer, and its sintering temperature is also similar to BaTiO3 ceramics. In addition, there are a large number of silicates in nature. Using them as Si sources can reduce the cost of manufacturing and therefore has broad application prospects in theory.
[0006] The present invention combines spray drying technology, uses silicate as Si source and inorganic acid as precipitant, prepares a mixed solution of silica gel colloid and nano / submicron Ni powder, uses spray drying method to homogenize and granulate the silicon oxide-coated Ni powder, and obtains core-shell Ni@SiO2 particles after low-temperature heating and decomposition. Summary of the invention
[0007] The present invention provides a method for synthesizing amorphous silicon oxide-coated nickel powder assisted by chemical precipitation and atomization granulation to solve the key problems of easy oxidation of Ni inner electrodes for MLCC during preparation, mismatch with the sintering shrinkage rate of ceramics, interpenetration and reaction with dielectric ceramic interfaces, etc. The method uses silicate as Si source and inorganic acid as precipitant, and mixes with nano / submicron Ni powder to prepare a mixed solution of silica colloid and nano / submicron Ni powder, and uses a spray drying device to perform surface modification treatment on Ni powder particles to prepare Ni@SiO2 particles. The prepared powder material is a spherical "core-shell structure", thereby controlling the sintering shrinkage rate of the MLCC inner electrode and the dielectric layer, reducing internal stress to prevent the generation of defects such as cracks and delamination, and improving electrode continuity and product qualification rate.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is:
[0009] A method for synthesizing amorphous silicon oxide coated nickel powder assisted by chemical precipitation and atomization granulation, wherein the method is used to coat Ni powder to obtain amorphous silicon oxide coated modified Ni powder material Ni@SiO2, wherein the particles are of a core / shell microstructure, wherein the core is metal Ni, the shell is a silicon oxide coating layer, the shell thickness is in the range of 10 to 15 nm, and the particle size is between 80 and 150 nm. The finished powder has good sphericity, crystallinity and purity.
[0010] The presence of the silicon oxide coating layer improves the oxidation resistance and sintering performance of the powder, improves the continuity of the electrode, and thus improves the qualified rate and service life of the product.
[0011] The core / shell microstructure, particle size and distribution of the particles can be regulated by controlling the ratio of silicate to raw material, the concentration of inorganic acid, the type and amount of dispersant added and parameters related to the spray drying process.
[0012] A method for synthesizing amorphous silicon oxide-coated nickel powder assisted by chemical precipitation and atomization granulation, firstly, using silicate as Si source and inorganic acid as precipitant to prepare silica gel colloid, and then mixing with nano / submicron Ni powder to prepare a mixed solution of colloid and Ni powder; secondly, synthesizing a silica gel-coated Ni powder intermediate based on the obtained mixed solution by spray drying; finally, washing, filtering, sintering in a tubular furnace and then decomposing to form silicon oxide-coated Ni powder. The method comprises the following steps:
[0013] The first step is to prepare a suspension for spray drying;
[0014] At room temperature, the raw material Ni powder and dispersant are added to the solvent, dispersed with a homogenizer for 10 minutes, and then ultrasonically treated for 10 to 30 minutes to obtain a suspension A; at room temperature, acid is added to the silicate, and ultrasonic dispersion vibration is performed for 30 minutes to obtain a colloid B; at room temperature, colloid B is added to the suspension A, mechanically stirred for 6 to 12 hours, and fully mixed to obtain a suspension C for spray drying.
[0015] Furthermore, the solvent in the suspension A includes deionized water solvent, ethanol, ethylene glycol and other organic solvents or their mixed solvents, preferably deionized water; the dispersant includes polyvinyl pyrrolidone (PVP), polyethylene glycol, citric acid, sodium citrate and the like or one or more mixtures thereof; the silicate includes one or more mixtures of sodium silicate, calcium silicate, potassium silicate and the like; the acid includes inorganic acid and organic acid, wherein the inorganic acid includes hydrochloric acid, nitric acid and sulfuric acid, and from the perspective of production cost and operational safety, dilute hydrochloric acid is preferred, and the organic acid includes citric acid, oxalic acid, acetic acid and the like or one or more mixtures thereof, preferably oxalic acid.
[0016] Furthermore, in the suspension A, the mass ratio of Ni powder to dispersant is 4:(1-3), and the concentration of Ni powder is 4 g / 1L.
[0017] Furthermore, in the colloid B, the molar ratio of silicate to acid is 1:1 to 1:2, and the concentration of silicate is 1 g / L to 4 g / L.
[0018] Furthermore, in the suspension C, the mass ratio of Ni powder to silicate is 4:(1-4).
[0019] The second step is to prepare the silicon oxide coated Ni powder intermediate by spray drying;
[0020] The silica-coated Ni powder is prepared by using the spray drying equipment and the suspension prepared in the first step as the formal liquid material. The specific process steps are: setting the circulating air volume and air inlet temperature of the central fan of the spray drying equipment, the outlet pressure of the air compressor, the high-pressure gas flow rate, and the speed of the peristaltic pump. When the air inlet temperature display is the same as the set temperature display or the outlet temperature display exceeds 90°C, and it is determined that the spray drying equipment has reached various preset indicators and is operating normally and stably, the spray drying process of the formal liquid material (the suspension prepared in the first step) can be entered.
[0021] Furthermore, the circulating air volume of the circulating fan can be set arbitrarily within the range of 85% to 95%.
[0022] Furthermore, the air inlet temperature ranges from 110 to 120°C.
[0023] Furthermore, the outlet pressure of the air compressor is set to 6Kg.
[0024] Furthermore, the high-pressure gas flow rate is set to 8-10 L / min.
[0025] Furthermore, the peristaltic pump speed is 25% to 35%.
[0026] The third step is to collect, wash and filter the powder.
[0027] After the spray drying process is completed, stop heating and turn off the equipment after the outlet temperature drops. After the machine cools to room temperature, unscrew the main collecting bottle from the lower port of the cyclone separator to collect the powder. Add a certain amount of deionized water to the collected powder, ultrasonically vibrate, centrifuge and remove the supernatant, wash repeatedly and filter to remove impurities.
[0028] Step 4: Heat and decompose the powder to prepare the finished product
[0029] The filtered powder is placed in a tubular furnace, the equipment is vacuumed, and heated and decomposed at 150-200°C for 4-6 hours. After the tubular furnace is cooled to room temperature, the final powder product is collected.
[0030] The specific working principle and innovation of the present invention are:
[0031] First, the dispersant is mixed with Ni powder to improve the dispersibility of Ni powder in the solution. Then, silicate reacts with inorganic acid to form silica gel colloid. Taking calcium silicate and hydrochloric acid as an example, the following reaction occurs: CaSiO3+2HCl=CaCl2+H2SiO3. The two are mixed together to form a stable suspension. The changes achieved in the spray drying method can be divided into two steps: spraying and drying.
[0032] The feed solution / suspension is pumped into the drying chamber through a nozzle. Compressed air is ejected from the air inlet pipe at a very high speed. At this time, the liquid material with a lower flow rate is ejected from the feed pipe. There will be a high relative speed between the two, which will cause friction and shear force between the gas and liquid. Under the action of the force, the liquid is pulled into a thin line, and the thin line breaks at a thinner point to form tiny droplets. Each small droplet contains one or more Ni powder particles wrapped in silica gel colloid. DLVO theory shows that adding free electrolytes to well-dispersed sols will reduce the potential energy barrier between aggregated particles, and a slow aggregation process will begin above the critical electrolyte concentration. During the spray drying process of this metastable sol, the ionic strength in the atomized droplets increases rapidly as water evaporates from the surface. This process further reduces the barrier to aggregation in the droplets accordingly. After the water evaporates to a certain extent, the ionic strength reaches the critical concentration. At this time, there is no repulsive barrier for aggregation. The colloid in the droplet quickly flocculates and the droplet gels. At the nozzle outlet, the droplet is atomized and contacts the drying fluid inside the drying chamber, that is, hot gas (usually air). In the process of passing through the drying chamber, energy-mass transfer occurs on the surface of the dynamic droplet, and the solvent is evaporated. Finally, the dried material is separated from the drying medium by a cyclone separator and collected in a collection device. The collected powder product is silica gel coated Ni powder, which is then washed, centrifuged, filtered, and impurities such as salts are removed. This process will not destroy the coating structure formed by silica gel on the Ni surface. Subsequently, it is heated and decomposed in a tubular furnace, and the reaction occurs: H2SiO3=SiO2+H2O. The silica gel coated on the surface of the Ni powder decomposes to form silicon oxide and water. After the water evaporates, silicon oxide coated Ni powder with a core-shell structure is formed. The parameter setting of spray drying has a great influence on the coating effect of powder. The injection speed of feed directly affects the size, movement trajectory and movement speed of droplets. At the same time, the increase of liquid feed per unit time also means that more solvent needs to be vaporized in the same time. Usually, a lower solution feed rate can obtain better atomization effect and smaller droplet size. Drying is the stage of converting droplets into dry particles. At this stage, the higher the drying temperature, the faster the solvent loss on the surface of droplets, which can not only lead to fewer undried particles attached to the wall of the drying chamber and increase the output, but also affect the speed of solute shrinkage and change the particle morphology. From this point of view, the higher the inlet temperature, the better. However, in practical applications, due to reasons such as thermal stability of materials, energy consumption of equipment and possible blockage of passages, the drying temperature should still be controlled within a reasonable range. The innovation of the present invention is: combining spray drying with chemical precipitation method, proposing a novel low-cost, green and environmentally friendly method for preparing nano / submicron Ni@SiO2 NCs metal powder. By adjusting parameters such as spray drying process parameters, type of dispersant, concentration of silicate, etc., the shortcomings of the single chemical precipitation method are solved: the coating thickness is difficult to control, it is not suitable for large-scale production, and the powder dispersibility is poor.Secondly, silicates that are widely found in nature are used as raw materials, which has low production costs and little pollution to the environment.
[0033] The beneficial effects of the present invention are:
[0034] (1) The present invention provides a process combining traditional chemical method and spray drying method for preparing nano-scale / submicron metal powder coating materials. Compared with the traditional chemical method, the powder prepared by the method of the present invention has the following advantages: the composition and microstructure are easy to control, with high sphericity and dispersibility, high density and good repeatability. By adjusting the process parameters, the particle size and its distribution can be changed, and it has the characteristics of being environmentally friendly and easy to mass produce.
[0035] (2) Silica itself is used as a glass phase or inorganic binder added to MLCC, making full use of the material properties of silica non-metallic oxides and introducing it onto the surface of Ni powder particles in the form of a coating layer without introducing new phase material components that do not belong to this system. This promotes the affinity between the silica-coated Ni powder for the internal electrode and the ceramic dielectric layer. In addition, silica can also be used as a sintering aid to increase the rate of the combustion reaction, increase the heat release of combustion, improve combustion stability, and control the generation of combustion products.
[0036] (3) The surface of the metal Ni particles is coated with an amorphous silicon dioxide layer. First, the dispersion of the Ni powder is effectively improved, reducing agglomeration. Second, it protects the metal Ni core, making it less susceptible to oxidation and improving its oxidation resistance. At the same time, it achieves a good interface bonding with the ceramic dielectric layer, thereby alleviating key issues such as volume shrinkage mismatch and easy cracking at the interlayer interface during the sintering process. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is the X-ray diffraction spectra of the pure Ni powder prepared in Comparative Example 1 and the amorphous silicon dioxide-coated Ni powder prepared in Examples 1-3.
[0038] Figure 2 This is a transmission electron micrograph of the amorphous silicon dioxide-coated Ni powder prepared in Example 2.
[0039] Figure 3 It is a transmission electron microscopic image of the amorphous silicon dioxide-coated Ni powder prepared in Example 2 (Figure a), and the corresponding Ni (Figure b), Si (Figure c), and O (Figure d) element distribution diagrams.
[0040] Figure 4 This is a detailed X-ray photoelectron spectrum of the amorphous silicon dioxide-coated Ni powder prepared in Example 2. (a) Si2p electron spectrum; (b) O1s electron spectrum.
[0041] Figure 5 These are the TGA-DSC curves of the pure Ni powder prepared in Comparative Example 1 (Figure a) and the amorphous silicon dioxide-coated Ni powder prepared in Example 2 (Figure b).
[0042] Figure 6 It is the volume shrinkage rate of the amorphous silicon dioxide-coated Ni powder prepared in Example 1 compared with the pure Ni powder prepared in Example 1.
[0043] Figure 7 It is the volume shrinkage rate of the amorphous silicon dioxide-coated Ni powder prepared in Example 2 compared with the pure Ni powder prepared in Example 1.
[0044] Figure 8 It is the volume shrinkage rate of the amorphous silicon dioxide-coated Ni powder prepared in Example 3 compared with the pure Ni powder prepared in Example 1.
[0045] Fig. 9 It is the volume shrinkage rate of the amorphous silicon dioxide coated Ni powder prepared in Example 4 compared with the pure Ni powder prepared in Example 1. DETAILED DESCRIPTION
[0046] The above contents of the present invention will be further described in detail below in conjunction with specific implementation modes, but the scope of the present invention is not limited to the following examples:
[0047] Comparative Example 1:
[0048] 1. Preparation process
[0049] Pure Ni powder without silica coating was prepared as a comparative example and compared with the Ni powder coated with silica (Example 1).
[0050] 1. The first step is to prepare Ni suspension for spray drying
[0051] At room temperature of 25°C, take 2 g of nano / submicron Ni powder as raw material, add 500 ml of deionized water, disperse it with a homogenizer for 10 min, add 0.5 citric acid, homogenize and disperse it for 10 min, then ultrasonically disperse it for 10 min, and stir it mechanically for 6 h.
[0052] 2. The second step is to prepare pure Ni powder by spray drying
[0053] Pure Ni powder is prepared by spray drying equipment. The specific process steps are: setting the circulating air volume of the circulating fan, the air inlet temperature, the outlet pressure of the air compressor, the high-pressure gas flow rate, the peristaltic pump speed, and when the air inlet temperature display is the same as the set temperature display or the outlet temperature display has exceeded 90°C, and confirming that the spray dryer system has reached the preset various indicators and is operating normally and stably, the spray drying process of the formal liquid material (the suspension prepared in the first step) can be entered.
[0054] Furthermore, the circulating air volume of the circulating fan is set to 85%.
[0055] Furthermore, the air inlet temperature is 110°C.
[0056] Furthermore, the outlet pressure of the air compressor is set to 6Kg.
[0057] Furthermore, the high-pressure gas flow rate is set to 8 L / min.
[0058] Furthermore, the peristaltic pump speed is 25%
[0059] Since the spray drying process is carried out in a hot air field, the dried powder may be adsorbed on the wall of the glassware due to static electricity. This phenomenon is normal.
[0060] 2. Results Analysis and Characterization
[0061] As attached Figure 1 The following is the XRD diffraction pattern of pure Ni powder. Pure Ni powder has a high degree of crystallinity. Figure 5 (a) shows the TGA-DSC results of the pure Ni powder comparative example. The initial oxidation temperature of the pure Ni powder is 315°C and the most intense oxidation temperature is 441°C. Figure 6 As shown, it is the volume shrinkage curve of pure Ni powder. During the sintering process in the range of 50 to 1200°C, the final volume shrinkage is 25.25%, and the volume shrinkage change is significantly greater than that of BaTiO3 powder.
[0062] Example 1
[0063] 1. Preparation process
[0064] 1. The first step is to prepare the Ni@SiO2 mixed solution for spray drying
[0065] At room temperature, 2 g of Ni powder was added to 500 ml of deionized water, dispersed with a homogenizer for 10 min, 0.5 g of citric acid was added, homogenized and dispersed for 10 min, and then ultrasonically treated for 10 min to obtain suspension A; at room temperature, 0.5 g of calcium silicate was added to 5.74 ml of hydrochloric acid (concentration of 1.5 mol / l), and ultrasonically dispersed and vibrated for 30 min to obtain colloid B; at room temperature, suspension A and suspension B were mixed, mechanically stirred for 6 h, and suspension C for spray drying was obtained after sufficient mixing.
[0066] Furthermore, in the suspension A, the added amounts of Ni powder and dispersant are 2 g and 0.5 g, respectively.
[0067] Furthermore, in the colloid B, the molar ratio of calcium silicate to hydrochloric acid is 1:2.
[0068] Furthermore, in the suspended C, the added amounts of Ni powder and calcium silicate are 2 g and 0.5 g, respectively.
[0069] 2. The second step is to prepare the silicon oxide coated Ni powder intermediate by spray drying
[0070] The silicon oxide coated Ni powder was prepared by spray drying equipment. The specific process steps are: setting the circulating air volume of the circulating fan, the air inlet temperature, the outlet pressure of the air compressor, the high-pressure gas flow, the peristaltic pump speed, when the air inlet temperature display is the same as the set temperature display or the outlet temperature display has exceeded 90°C, and after confirming that the spray dryer system has reached the preset various indicators and is operating normally and stably, the spray drying process of the formal liquid material (the suspension prepared in the first step) can be entered.
[0071] Furthermore, the circulating air volume of the circulating fan is set to 85%.
[0072] Furthermore, the air inlet temperature is 110°C.
[0073] Furthermore, the outlet pressure of the air compressor is set to 6Kg.
[0074] Furthermore, the high-pressure gas flow rate is set to 8 L / min.
[0075] Furthermore, the peristaltic pump speed is 25%
[0076] Since the spray drying process is carried out in a hot air field, the dried powder may be adsorbed on the wall of the glass instrument due to static electricity. This phenomenon is normal.
[0077] 3. The third step is to collect, wash and filter the powder
[0078] After the spray drying experiment is over, stop heating, and turn off other switches of the equipment after the outlet temperature drops. After the machine cools down to room temperature, collect the powder. Add a certain amount of deionized water to the collected powder, ultrasonically vibrate, centrifuge and remove the supernatant, wash repeatedly and filter to remove impurities.
[0079] 4. The fourth step is to heat and decompose the powder to prepare the finished product
[0080] The filtered powder was placed in a tubular furnace, the equipment was vacuumed, and heated and decomposed at 150°C for 4 hours. After the tubular furnace was cooled to room temperature, the final powder product was collected.
[0081] 2. Results Analysis and Characterization
[0082] As attached Figure 1As shown in the figure, it is the XRD diffraction pattern of Ni@SiO2 powder. According to the standard PDF card, there is an obvious Ni phase diffraction peak, indicating that the Ni core particles in the powder have a high degree of crystallinity; there is no diffraction peak of silicon dioxide in the X-ray diffraction spectrum, and the silicon dioxide coating layer exists in an amorphous non-crystalline form. Figure 6 As shown in the figure, compared with the volume shrinkage curve of pure Ni powder in comparative example 1, the final volume shrinkage is 25.25% during the sintering process in the range of 50-1200°C, and the volume shrinkage change is significantly greater than that of BaTiO3 powder. The sintering shrinkage of Ni@SiO2 powder in Example 1 is greatly reduced to 13.01%, which indicates that SiO2-coated Ni powder can greatly increase the shrinkage resistance of Ni powder between 1000 and 1200°C.
[0083] Example 2
[0084] 1. Preparation process
[0085] 1. The first step is to prepare the Ni@SiO2 mixed solution for spray drying
[0086] At room temperature, 2 g of Ni powder was added to 500 ml of ethanol, dispersed with a homogenizer for 10 min, 1 g of PVP was added, homogenized and dispersed for 20 min, and then ultrasonically treated for 20 min to obtain suspension A; at room temperature, 1 g of sodium silicate was added to 5.46 ml of hydrochloric acid (concentration of 1.5 mol / l), and ultrasonically dispersed and vibrated for 30 min to obtain colloid B; at room temperature, suspension A and suspension B were mixed, mechanically stirred for 9 h, and after sufficient mixing, suspension C for spray drying was obtained.
[0087] Furthermore, in the suspension A, the added amounts of Ni powder and dispersant are 2 g and 1 g, respectively.
[0088] Furthermore, in the colloid B, the molar ratio of sodium silicate to hydrochloric acid is 1:1.
[0089] Furthermore, in the suspension C, the added amounts of Ni powder and sodium silicate are 2 g and 1 g respectively.
[0090] 2. The second step is to prepare the silicon oxide coated Ni powder intermediate by spray drying
[0091] The silicon oxide coated Ni powder was prepared by spray drying equipment. The specific process steps are: setting the circulating air volume of the circulating fan, the air inlet temperature, the outlet pressure of the air compressor, the high-pressure gas flow, the peristaltic pump speed, when the air inlet temperature display is the same as the set temperature display or the outlet temperature display has exceeded 90°C, and after confirming that the spray dryer system has reached the preset various indicators and is operating normally and stably, the spray drying process of the formal liquid material (the suspension prepared in the first step) can be entered.
[0092] Furthermore, the circulating air volume of the circulating fan is set to 90%.
[0093] Furthermore, the air inlet temperature is 115°C.
[0094] Furthermore, the outlet pressure of the air compressor is set to 6Kg.
[0095] Furthermore, the high-pressure gas flow rate is set to 9 L / min.
[0096] Furthermore, the peristaltic pump speed is 30%
[0097] 3. The third step is to collect, wash and filter the powder
[0098] After the spray drying experiment is over, stop heating, and turn off other switches of the equipment after the outlet temperature drops. After the machine cools down to room temperature, collect the powder. Add a certain amount of deionized water to the collected powder, ultrasonically vibrate, centrifuge and remove the supernatant, wash repeatedly and filter to remove impurities.
[0099] 4. The fourth step is to heat and decompose the powder to prepare the finished product
[0100] The filtered powder was placed in a tubular furnace, the equipment was vacuumed, and heated and decomposed at 175°C for 5 hours. After the tubular furnace was cooled to room temperature, the final powder product was collected.
[0101] 2. Results Analysis and Characterization
[0102] As attached Figure 1 As shown, it is the XRD diffraction pattern of Ni@SiO2 powder. According to the standard PDF card, there is an obvious Ni phase diffraction peak, indicating that the Ni core particles in the powder have a high degree of crystallinity; there is no diffraction peak of silica in the X-ray diffraction spectrum, and the silica coating layer exists in an amorphous non-crystalline form.
[0103] As attached Figure 2 As shown, it is a transmission electron micrograph of silicon dioxide coated Ni powder particles, forming a clear amorphous SiO2 coating layer (shell), with Ni particles as the core, and this core / shell structure particle has good sphericity. In addition, the thickness of the SiO2 coating layer is about 10nm.
[0104] Attached Figure 3 As shown, this is the energy spectrum of NI@SiO2, from which the distribution of cleaned elements can be seen.
[0105] Attached Figure 4 The figure shows the X-ray photoelectron spectroscopy test of Ni powder particles coated with silicon dioxide (5wt.%). Figure 4(a) is the detailed XPS spectrum of Si2p electrons. The peak at 103.14 eV corresponds to the binding energy of Si2p electrons in SiO2. Figure 4 (b) is the detailed XPS spectrum of O1s electrons. The Si-O bond originates from the SiO2 coating layer. In addition, Ni-O bond signals from trace amounts of oxidized Ni oxide layer also appear.
[0106] As attached Figure 5 (b) shows the TG-DSC analysis results of the silica-coated Ni powder particles. Compared with the TGA of pure Ni powder (Comparative Example 1), the initial oxidation temperature of the silica-coated Ni powder was delayed by 52°C; compared with the DSC curve, the most intense oxidation temperature of the silica-coated Ni powder was delayed by 36.68°C.
[0107] As attached Figure 7 As shown in the volume shrinkage curve of pure Ni powder, the final volume shrinkage is 25.25% during the sintering process in the range of 50-1200°C, and the volume shrinkage change is significantly greater than that of BaTiO3 powder. The sintering shrinkage of Ni@SiO2 powder in Example 2 is greatly reduced to 8.91%, and its anti-sintering performance is significantly improved.
[0108] Example 3
[0109] 1. Preparation process
[0110] 1. The first step is to prepare the Ni@SiO2 mixed solution for spray drying
[0111] At room temperature, 2 g of Ni powder was added to 500 ml of ethylene glycol, dispersed with a homogenizer for 10 min, 1.5 g of polyethylene glycol was added, homogenized and dispersed for 30 min, and then ultrasonically treated for 30 min to obtain suspension A; at room temperature, 2 g of potassium silicate was added to 13.3 ml of oxalic acid (concentration of 1.5 mol / l), and ultrasonically dispersed and vibrated for 30 min to obtain colloid B; at room temperature, suspension A and suspension B were mixed, mechanically stirred for 12 h, and after sufficient mixing, suspension C for spray drying was obtained.
[0112] Furthermore, in the suspension A, the added amounts of Ni powder and dispersant are 2 g and 1.5 g, respectively.
[0113] Furthermore, in the colloid B, the molar ratio of potassium silicate to oxalic acid is 1:1.
[0114] Furthermore, in the suspension C, the mass ratio of Ni powder to sodium silicate added is 2g and 2g respectively.
[0115] 2. The second step is to prepare the silicon oxide coated Ni powder intermediate by spray drying
[0116] The silicon oxide coated Ni powder was prepared by spray drying equipment. The specific process steps are: setting the circulating air volume of the circulating fan, the air inlet temperature, the outlet pressure of the air compressor, the high-pressure gas flow, the peristaltic pump speed, when the air inlet temperature display is the same as the set temperature display or the outlet temperature display has exceeded 90°C, and after confirming that the spray dryer system has reached the preset various indicators and is operating normally and stably, the spray drying process of the formal liquid material (the suspension prepared in the first step) can be entered.
[0117] Furthermore, the circulating air volume of the circulating fan is set to 95%.
[0118] Furthermore, the air inlet temperature is 120°C.
[0119] Furthermore, the outlet pressure of the air compressor is set to 6Kg.
[0120] Furthermore, the high-pressure gas flow rate is set to 10 L / min.
[0121] Furthermore, the peristaltic pump speed is 35%
[0122] 3. The third step is to collect, wash and filter the powder
[0123] After the spray drying experiment is over, stop heating, and turn off other switches of the equipment after the outlet temperature drops. After the machine cools down to room temperature, collect the powder. Add a certain amount of deionized water to the collected powder, ultrasonically vibrate, centrifuge and remove the supernatant, wash repeatedly and filter to remove impurities.
[0124] 4. The fourth step is to heat and decompose the powder to prepare the finished product
[0125] The filtered powder was placed in a tubular furnace, the equipment was vacuumed, and heated and decomposed at 180°C for 6 hours. After the tubular furnace was cooled to room temperature, the final powder product was collected.
[0126] 2. Results Analysis and Characterization
[0127] As attached Figure 1 As shown, it is the XRD diffraction pattern of Ni@SiO2 powder. According to the standard PDF card, there is an obvious Ni phase diffraction peak, indicating that the Ni core particles in the powder have a high degree of crystallinity; there is no diffraction peak of silica in the X-ray diffraction spectrum, and the silica coating layer exists in an amorphous non-crystalline form.
[0128] As attached Figure 8 As shown in the volume shrinkage curve of pure Ni powder, the final volume shrinkage is 25.25% during the sintering process in the range of 50-1200°C. The sintering shrinkage of Ni@SiO2 powder in Example 3 is reduced to a certain extent, which is 22.33%.
[0129] Example 4
[0130] 1. Preparation process
[0131] 1. The first step is to prepare the Ni@SiO2 mixed solution for spray drying
[0132] At room temperature, 2 g of Ni powder was added to a mixture of 500 ml of water and ethanol (volume ratio of 1:1), dispersed with a homogenizer for 10 mi, 1.5 g of sodium citrate was added, homogenized and dispersed for 30 min, and then ultrasonically treated for 30 min to obtain suspension A; at room temperature, 2 g of calcium silicate was added to 11.49 ml of hydrochloric acid (concentration of 1.5 mol / l), and ultrasonically dispersed and vibrated for 30 min to obtain colloid B; at room temperature, suspension A and suspension B were mixed, mechanically stirred for 12 h, and suspension C for spray drying was obtained after sufficient mixing.
[0133] Furthermore, in the suspension A, the added amounts of Ni powder and dispersant are 2 g and 1.5 g, respectively.
[0134] Furthermore, in the colloid B, the molar ratio of calcium silicate to hydrochloric acid is 1:2.
[0135] Furthermore, in the suspended C, the added amounts of Ni powder and calcium silicate are 2 g and 2 g respectively.
[0136] 2. The second step is to prepare the silicon oxide coated Ni powder intermediate by spray drying
[0137] The silicon oxide coated Ni powder was prepared by spray drying equipment. The specific process steps are: setting the circulating air volume of the circulating fan, the air inlet temperature, the outlet pressure of the air compressor, the high-pressure gas flow, the peristaltic pump speed, when the air inlet temperature display is the same as the set temperature display or the outlet temperature display has exceeded 90°C, and after confirming that the spray dryer system has reached the preset various indicators and is operating normally and stably, the spray drying process of the formal liquid material (the suspension prepared in the first step) can be entered.
[0138] Furthermore, the circulating air volume of the circulating fan is set to 95%.
[0139] Furthermore, the air inlet temperature is 120°C.
[0140] Furthermore, the outlet pressure of the air compressor is set to 6Kg.
[0141] Furthermore, the high-pressure gas flow rate is set to 10 L / min.
[0142] Furthermore, the peristaltic pump speed is 35%
[0143] 3. The third step is to collect, wash and filter the powder
[0144] After the spray drying experiment is over, stop heating, and turn off other switches of the equipment after the outlet temperature drops. After the machine cools down to room temperature, collect the powder. Add a certain amount of deionized water to the collected powder, ultrasonically vibrate, centrifuge and remove the supernatant, wash repeatedly and filter to remove impurities.
[0145] 4. The fourth step is to heat and decompose the powder to prepare the finished product
[0146] The filtered powder was placed in a tubular furnace, the equipment was vacuumed, and heated and decomposed at 200°C for 6 hours. After the tubular furnace was cooled to room temperature, the final powder product was collected.
[0147] 2. Results Analysis and Characterization
[0148] As attached Fig. 9 As shown in the volume shrinkage curve of pure Ni powder, the final volume shrinkage is 25.25% during the sintering process in the range of 50-1200°C, and the volume shrinkage change is significantly greater than that of BaTiO3 powder. The sintering shrinkage of Ni@SiO2 powder in Example 4 first increases and then decreases to 3.79%.
[0149] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for synthesizing amorphous silicon oxide-coated nickel powder by chemical precipitation and atomization granulation, characterized in that: The amorphous silicon oxide coated nickel powder Ni@SiO2 has a core / shell microstructure, wherein the core is metal Ni and the shell is a silicon oxide coating layer.
2. The method of synthesizing amorphous silicon oxide-coated nickel powder by chemical precipitation and atomization granulation according to claim 1, characterized in that: The particle size of the amorphous silicon oxide-coated nickel powder particles is between 80 and 150 nm.
3. A method for synthesizing amorphous silicon oxide-coated nickel powder assisted by chemical precipitation and atomization granulation according to claim 1 or 2, characterized in that: The method firstly uses silicate as Si source and inorganic acid as precipitant to prepare silica gel colloid, and then mixes it with nano / submicron Ni powder to prepare a mixed solution of colloid and Ni powder; secondly, based on the obtained mixed solution, a silica gel-coated Ni powder intermediate is synthesized by spray drying method; finally, after washing, filtering, and sintering in a tubular furnace, it is decomposed to form silicon oxide-coated Ni powder.
4. The method for synthesizing amorphous silicon oxide-coated nickel powder by chemical precipitation and atomization granulation according to claim 3, characterized in that: The following steps are involved: The first step is to prepare a suspension for spray drying; At room temperature, raw Ni powder and dispersant are added to a solvent, dispersed, and ultrasonically treated to obtain suspension A; at room temperature, acid is added to silicate, and ultrasonically dispersed to obtain colloid B; at room temperature, colloid B is added to suspension A, mechanically stirred, and fully mixed to obtain suspension C for spray drying; In the second step, the suspension prepared in the first step is used as the formal liquid material, and a spray drying device is used to prepare silicon oxide-coated Ni powder; The third step is to collect, wash and filter the powder. After the spray drying process is completed, the collected powder is added to deionized water, ultrasonically vibrated, centrifuged and the supernatant is removed, and the powder is filtered after repeated washing; Step 4: Heat and decompose the powder to prepare the finished product The powder obtained in the third step is placed in a tubular furnace, the equipment is vacuumed, and heated and decomposed at 150-200°C for 4-6 hours. After the tubular furnace is cooled to room temperature, the product is obtained.
5. The method for synthesizing amorphous silicon oxide-coated nickel powder by chemical precipitation and atomization granulation according to claim 4, characterized in that: The core / shell microstructure, particle size and distribution of the particles can be regulated by controlling the ratio of silicate to raw material, the concentration of inorganic acid, the type and amount of dispersant added, and parameters related to the spray drying process.
6. The method for synthesizing amorphous silicon oxide-coated nickel powder by chemical precipitation and atomization granulation as claimed in claim 4, characterized in that: In the first step, the mechanical stirring time is 6 to 12 hours at room temperature.
7. The method for synthesizing amorphous silicon oxide-coated nickel powder assisted by chemical precipitation and atomization granulation according to claim 4, characterized in that: In the first step described: The solvent in the suspension A includes deionized water, ethanol, ethylene glycol or other organic solvents, or a mixed solvent thereof; the dispersant includes polyvinyl pyrrolidone, polyethylene glycol, citric acid, sodium citrate or a mixture of one or more thereof; the silicate includes a mixture of one or more of sodium silicate, calcium silicate and potassium silicate; the acid includes an inorganic acid and an organic acid, wherein the inorganic acid includes hydrochloric acid, nitric acid and sulfuric acid; the organic acid includes citric acid, oxalic acid, acetic acid and the like or a mixture of one or more thereof; In the suspension A, the mass ratio of Ni powder to dispersant is 4:(1-3), wherein the concentration of Ni powder is 4 g / 1L; in the colloid B, the molar ratio of silicate to acid is 1:1-1:2, wherein the concentration of silicate is 1 g / L-4 g / L; in the suspension C, the mass ratio of Ni powder to silicate is 4:(1-4).
8. The method for synthesizing amorphous silicon oxide-coated nickel powder by chemical precipitation and atomization granulation as claimed in claim 7, characterized in that: The suspension A is preferably deionized water; the acid is preferably dilute hydrochloric acid; and the organic acid is preferably oxalic acid.
9. The method for synthesizing amorphous silicon oxide-coated nickel powder assisted by chemical precipitation and atomization granulation according to claim 4, characterized in that: The specific steps of the second step are: setting the circulating air volume, air inlet temperature, outlet pressure, high-pressure gas flow rate and peristaltic pump speed of the central fan of the spray drying equipment; when the air inlet temperature display is the same as the set temperature display or the outlet temperature display has exceeded 90°C, and after determining that the spray drying equipment has reached various preset indicators and is operating normally and stably, the formal liquid spray drying process is carried out.
10. The method for synthesizing amorphous silicon oxide-coated nickel powder assisted by chemical precipitation and atomization granulation according to claim 9, characterized in that: The process parameters of the second step are set as follows: The circulating air volume of the circulating fan can be set arbitrarily within the range of 85% to 95%; The air inlet temperature range is 110-120°C; The outlet pressure of the air compressor is set to 6Kg; The high pressure gas flow rate is set to 8-10 L / min; The rotation speed of the peristaltic pump is 25% to 35%.
Citation Information
Cited By
Barium titanate coated Ni particle material synthesized with assistance of spray drying technology and method of barium titanate coated Ni particle material
CN119634725A
Noctilucent glass bead brocade ammonia air coated yarn and preparation method thereof
CN120866986A