Superhydrophobic SERS substrate with multi-level micro-nanostructure coupling amplification and its preparation and application

By using a superhydrophobic SERS substrate with multi-level micro-nano structure coupling and amplification in SERS detection, the problem of the inability of noble metal nanoparticles to be fixed during the evaporation process of liquid droplets is solved, the repeatability of detection and signal stability are improved, and the problem of Coffee ring effect.

CN115598104BActive Publication Date: 2024-10-01HANGZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211159582.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-22
Publication Date
2024-10-01
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

In existing SERS detection, noble metal nanoparticles cannot be fixed during the evaporation process of liquid droplets, resulting in the coffee ring effect, resulting in poor detection repeatability and large signal fluctuations, which limits its practical application.

Method used

A superhydrophobic SERS substrate with multi-level micro-nano structure coupling and amplification is used. By using SiO2 nanospheres as the basic unit to build a patterned surface and combining it with a two-dimensional film of hydrophobic noble metal nanoparticles, a micro-nano rough structure is formed, eliminating the coffee ring effect and realizing nanoparticles. of fixed.

Benefits of technology

It improves the hydrophobicity of the two-dimensional film of precious metal nanoparticles, enhances the density of hot spots, ensures the fixation of nanoparticles, and significantly improves the repeatability and signal stability of SERS detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115598104B_ABST
    Figure CN115598104B_ABST
Patent Text Reader

Abstract

The present invention provides a multi-level micro-nano structure coupled amplified super-hydrophobic SERS substrate and its preparation and application, with SiO 2 Nanospheres as basic units for preparing hydrophobic SiO 2 Regular array, with noble metal nanoparticles as the basic unit, using the low surface energy of perfluorinated molecules to prepare a hydrophobic noble metal nanoparticle two-dimensional film, and then transferring the hydrophobic nanoparticle two-dimensional film to the hydrophobic SiO 2 The array can be prepared. The present invention enhances the hydrophobicity of the nanoparticle two-dimensional film, prepares a super-hydrophobic substrate, and achieves a droplet concentration effect; when in use, the dye to be tested is mixed with the gold ball and then dropped on the substrate together, and the gold ball in the droplet and the nanoparticle film are mirror-coupled under laser irradiation, which not only provides hot spots in the nanoparticle two-dimensional film layer, but also the mirror effect of the gold ball and the two-dimensional film will produce interlayer hot spots, further achieving the SERS enhancement effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of nanomaterials and SERS detection technology, and in particular to a multi-level micro-nano structure coupled amplified super-hydrophobic SERS substrate and preparation and application thereof. Background Art

[0002] Surface enhanced Raman scattering (SERS) is a commonly used sensing technology. In this technology, when the molecules to be detected are adsorbed on the surface of metal nanostructures, the Raman scattering intensity caused by the interaction with the metal surface due to the plasma resonance (SPR) is enhanced. So far, silver and gold are the most frequently used metals in SERS. SERS applications are very extensive and are widely used in real life, such as food safety and art authentication. Regarding the preparation of SERS substrates, a lot of work has been done in the study of hydrophobic substrates. For example, Shikuan Yang et al. reported a SERS platform based on Nepenthes-inspired slippery liquid injection porous surface, which provides an almost pin-free matrix for enriching analytes in aqueous and most importantly non-aqueous liquids and delivering them to specific SERS detection areas to achieve ultra-sensitive detection. However, this does not maximize the coupling of nanoparticles, so the preparation of a super-hydrophobic substrate that can be coupled in three dimensions is currently a difficult problem to overcome in SERS detection.

[0003] The inventor proposed Chinese patent CN113714499A earlier, which disclosed a two-dimensional film of precious metal nanoparticles with low surface energy, which can capture and enrich dye molecules and can serve as a SERS substrate. However, in actual application, the nanoparticles contained in the detection liquid droplets during the evaporation process cannot be fixed, resulting in a coffee ring effect. Coffee rings are a phenomenon often encountered in SERS spectral detection, that is, when precious metal nanoparticle sol drops are dropped on a planar substrate such as Si or SiO2, as the solvent evaporates, more nanoparticles in the droplets are deposited on the edge of the droplets, forming a ring-shaped nanoparticle distribution similar to a coffee ring. This distribution is uneven, which will lead to poor SERS detection repeatability and large signal fluctuations, limiting its actual detection application. Summary of the invention

[0004] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a method for preparing a super-hydrophobic SERS substrate with multi-level micro-nano structure coupling amplification, with SiO2 nanospheres as the basic unit. The spherical structure of SiO2 will form grooves on the surface, which is called a patterned surface. This method combines the patterned surface with a two-dimensional film of hydrophobic precious metal nanoparticles, thereby increasing the hot spots. The micro-nano rough structure increases the hydrophobicity of the two-dimensional film, achieves super-hydrophobic performance, and eliminates the coffee ring effect.

[0005] The method specifically adopts the following technical solutions:

[0006] (1) Preparation of hydrophobic SiO2 self-assembled structures

[0007] Taking SiO2 nanospheres as basic units, a compact and regular SiO2 self-assembled structure was constructed by utilizing ethanol-assisted self-assembly at the air / water interface; the SiO2 array was chemically deposited to modify hydrophobic molecules to obtain a hydrophobic SiO2 self-assembled structure.

[0008] (2) Preparation of hydrophobic noble metal nanoparticle two-dimensional films

[0009] A n-hexane-ethanol solution of perfluorinated molecules is injected into the precious metal nanoparticles, and the oil phase n-hexane is completely volatilized at 25-50° C. to obtain a hydrophobic two-dimensional film of precious metal nanoparticles at the water-oil interface; the precious metal nanoparticles are nanogold balls, nanogold rods, and gold triangle sheets; and the volume ratio of the precious metal nanoparticles to the n-hexane-ethanol solution of perfluorinated molecules is 5-7:10.

[0010] (3) Preparation of super-hydrophobic SERS substrate with multi-level micro-nanostructure coupling amplification

[0011] The hydrophobic SiO2 array is placed downward in contact with the two-dimensional film of noble metal nanoparticles. After the two-dimensional film of noble metal nanoparticles covers the entire surface of the hydrophobic SiO2 regular array, it is rinsed with deionized water to obtain a superhydrophobic SERS substrate.

[0012] Preferably, in step (1), the size of the SiO2 nanospheres is 2 μm.

[0013] Preferably, in step (1), the hydrophobic molecule is 1H,1H,2H,2H-perfluorodecyltrichlorosilane.

[0014] Preferably, in step (1), the chemical deposition environment is a vacuum environment, and the chemical deposition time is 12 hours.

[0015] Preferably, in step (2), the noble metal nanoparticles are gold rod films, and the gold rods are 90 to 100 nm in length and 20 to 25 nm in width.

[0016] Preferably, in step (2), the perfluoro molecule is perfluorodecyl mercaptan, and the concentration is 10 mM; and the volume ratio of n-hexane to ethanol in the n-hexane-ethanol solution of the perfluoro molecule is 1:2.

[0017] Preferably, in step (2), the gold nanospheres are prepared from sodium citrate, chloroauric acid and tris(hydroxymethyl)aminomethane solution as raw materials; the gold nanorods are prepared from hexadecyltrimethylammonium bromide (CTAB), sodium borohydride, chloroauric acid, sodium oleate, silver nitrate, hydrochloric acid and ascorbic acid as raw materials; and the triangular sheets are prepared from hexadecyltrimethylammonium chloride (CTAC), sodium borohydride, chloroauric acid, potassium iodide, ascorbic acid and sodium chloride as raw materials.

[0018] The second object of the present invention is to provide a super-hydrophobic SERS substrate obtained by the above method.

[0019] The third object of the present invention is to provide the application of the super-hydrophobic SERS substrate in SERS detection, specifically:

[0020] The object to be tested is mixed with noble metal nanoparticles to form a liquid droplet of the object to be tested; the liquid droplet of the object to be tested is dropped on the super-hydrophobic SERS substrate, and after the droplet is evaporated, the SERS is detected under a Raman instrument.

[0021] The noble metal nanoparticles mixed with the analyte produce a mirror coupling effect with the two-dimensional film of the noble metal nanoparticles in the substrate. Under laser irradiation, a magnetic effect is induced between the noble metal nanoparticles in the upper part and the imaging of the two-dimensional film of the noble metal nanoparticles, further realizing dual coupling in the lateral and longitudinal directions, and achieving the SERS enhancement effect.

[0022] Preferably, the noble metal nanoparticles are gold nanospheres, gold nanorods or gold triangle sheets, more preferably gold nanospheres.

[0023] Preferably, the analyte is methylene blue.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention improves the hydrophobicity of the two-dimensional film of the noble metal nanoparticles by combining the hydrophobic SiO2 with the hydrophobic noble metal nanoparticle two-dimensional film. Since the noble metal nanoparticles modified with perfluorodecyl mercaptan have extremely strong hydrophobicity, the macroscopic large-area assembly of the two-dimensional film of the hydrophobic noble metal nanoparticles can be achieved, and the assembly utilization rate of the noble metal nanoparticles is close to 100%.

[0026] The SiO2 array groove structure in the lower layer of the substrate increases the density of the upper layer of the noble metal nanoparticle two-dimensional film and increases the hot spots. The noble metal nanoparticle two-dimensional film combines with the silicon dioxide substrate to form a micro-nano rough structure. During the evaporation of the droplet of the test object, the nanoparticles contained in the droplet can be fixed, thereby eliminating the coffee ring effect.

[0027] The present invention mixes the dye to be tested with noble metal nanoparticles and then drops them together on a substrate. The noble metal nanoparticles in the droplets and the two-dimensional film of the noble metal nanoparticles are mirror-coupled under laser irradiation, which not only provides hot spots within the two-dimensional film layer of the noble metal nanoparticles, but the mirror effect between the noble metal nanoparticles and the two-dimensional film of the noble metal nanoparticles also produces interlayer hot spots. Coupling amplification is performed based on a multi-level micro-nano structure, and good detection performance is achieved in dye molecule detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the SEM image of the gold nanorod two-dimensional film in Example 2, with a scale of 200 nm.

[0029] Figure 2 This is the SEM image of the gold nanospheres in Example 3, with a scale of 100 nm.

[0030] Figure 3 This is a SEM image of the golden triangle piece in Example 4, with a scale of 200 nm.

[0031] Figure 4 This is the SEM picture of the hydrophobic SiO2 array in Example 5, with a scale of 2 μm.

[0032] Figure 5 This is a SEM image of the super-hydrophobic SERS substrate based on multi-level micro-nanostructure coupling amplification in Example 6, with a scale of 2 μm.

[0033] Figure 6 This is a comparison of the hydrophobicity of a simple gold rod two-dimensional membrane and a micro-nanostructured gold rod two-dimensional membrane.

[0034] Figure 7 This is a schematic diagram of the results of verifying the optimal SERS conditions of the gold triangle sheet, gold sphere and gold rod film by mixing the gold rod with the test object in Application Example 1.

[0035] Figure 8 This is a schematic diagram of the results of the optimal SERS conditions of different nanoparticle triangles, gold balls and gold rods mixed with the test object under the optimal substrate gold rod film of Application Example 1 in Application Example 2.

[0036] Fig. 9 This is a comparison chart of the SERS intensities of four different substrates in Application Example 3.

[0037] Fig.10 This is the SERS image of detecting different concentrations of methylene blue in Application Example 4.

[0038] Fig.11 In the figure, (a) is the microscopic result of the sample droplet on the simple hydrophobic gold rod two-dimensional film of Application Example 5, and (b) is the microscopic result of the sample droplet on the super-hydrophobic SERS substrate based on multi-level micro-nanostructure coupling amplification of Application Example 5. DETAILED DESCRIPTION

[0039] As mentioned above, in view of the shortcomings of the prior art, the inventor of this case proposed the technical solution of the present invention after long-term research and extensive practice, which is mainly based on at least:

[0040] The present invention combines hydrophobic SiO2 with a hydrophobic noble metal nanoparticle two-dimensional film to achieve super-hydrophobic performance. When used, the object to be tested is mixed with the noble metal nanoparticles, and the noble metal nanoparticles and the hydrophobic noble metal nanoparticle two-dimensional film substrate produce a mirror coupling effect. Under laser irradiation, a magnetic effect is induced between the upper part of the noble metal nanoparticles and the imaging of the hydrophobic noble metal nanoparticle two-dimensional film, thereby further achieving coupling in the two-dimensional direction and realizing a SERS enhancement effect. It has been verified that the detection performance is good in dye molecule detection.

[0041] The method for preparing a super-hydrophobic SERS substrate with multi-level micro-nano structure coupling amplification of the present invention comprises the following steps:

[0042] (1) Preparation of hydrophobic SiO2 regular array

[0043] Using SiO2 nanospheres with a size of 2 μm as the basic unit, an ITO glass sheet with a thickness of 2 mm (10*10 cm) was washed with acetone, ethanol and deionized water in an ultrasonic bath. 2 ), then washed and dried in 98% H2SO4 / H2O2 (volume ratio 3:1), H2O / NH3·H2O / H2O2 (volume ratio 5:1:1), and after thorough cleaning, the surface of the glass slide was fully hydrophilic. The mixed suspension was then diluted in the same volume of ethanol and sonicated to obtain absolute homogeneity;

[0044] The preparation of large-area SiO2 arrays is as follows: First, a clean ITO glass slide is placed on a flat plate and deionized water of about 2 mm thickness is dropped on it to form a water film covering the entire surface of the slide. Secondly, the mixed suspension diluted with ethanol (volume is about 100 μL) is taken with a micropipette and continuously and slowly injected into the water at the edge of the preformed water film for about 5 minutes. After injection, it is kept for 5 minutes to allow the SiO2 spheres to self-assemble at the air / water interface. Finally, after the liquid evaporates, a large-area SiO2 array is formed on the slide by a gentle airflow at 30°C.

[0045] The prepared SiO2 array was modified with hydrophobic molecules 1H,1H,2H,2H-perfluorodecyltrichlorosilane and chemically deposited for 12 h in a vacuum environment.

[0046] (2) Preparation of hydrophobic noble metal nanoparticle two-dimensional film

[0047] Inject 10 mL of a 10 mM hexane-ethanol solution of perfluorodecyl mercaptan into 5 to 7 mL of precious metal nanoparticles, and completely volatilize the oil phase hexane at 25 to 50° C. to obtain a hydrophobic two-dimensional film of precious metal nanoparticles at the water-oil interface; the precious metal nanoparticles are gold nanospheres, gold nanorods, or gold triangle sheets, preferably a gold rod film, with a gold rod length of 90 to 100 nm and a width of 20 to 25 nm; and the volume ratio of hexane to ethanol is 1:2.

[0048] (3) Preparation of super-hydrophobic SERS substrate with multi-level micro-nanostructure coupling amplification

[0049] Use tweezers to hold the ITO glass slide loaded with the hydrophobic SiO2 array, with the side loaded with the hydrophobic SiO2 array facing down, and vertically extend it into the quartz beaker to reach the water-oil interface. After the two-dimensional film of hydrophobic noble metal nanoparticles covers the entire surface of the SiO2 regular array, take out the glass slide, and then rinse the loaded surface to obtain a super-hydrophobic SERS substrate.

[0050] The present invention will be further described below in conjunction with the accompanying drawings and embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0051] Example 1

[0052] (1) Preparation of gold nanorod seed solution

[0053] Prepare 5 mL of 0.2 M CTAB aqueous solution, dissolve at 50 ° C for 30 minutes, wait for the solution to cool to room temperature, add 5 mL of 0.5 mM chloroauric acid solution, gently stir and mix for 1 minute. Quickly add 0.6 mL of 0.01 M sodium borohydride solution prepared with ice water, stir vigorously for 2 minutes, and stand at 30 ° C for 30-40 minutes to prepare the gold nanorod seed solution.

[0054] (2) Preparation of gold nanorod solution

[0055] Add 3.5g CTAB and 0.617g sodium oleate to 125mL warm water, cool to 30℃ after complete dissolution, then add 9mL 4mM silver nitrate and 125mL 1mM chloroauric acid in turn, stir at 700rpm for 90min at room temperature, then add 0.9mL hydrochloric acid (37%, 12M) to adjust the aspect ratio of the gold rod. After slowly stirring at 400rpm for 15min, add 0.625mL 0.064M ascorbic acid solution and stir vigorously for 30s. Finally, add 0.2mL of nano-gold rod seed solution, stir vigorously for 30s, and let stand at 30℃ for more than 12h. Centrifuge the resulting nano-gold rod original solution at 8500rpm for 10min, and then redisperse it in deionized water at the original concentration for subsequent perfluorinated film formation.

[0056] Example 2

[0057] Preparation of hydrophobic gold rod two-dimensional film: After adding 7 mL of nano-gold rod solution into a quartz beaker, add 10 mL of a mixed solution of perfluorodecyl mercaptan in n-hexane / ethanol (10 mM, the volume ratio of n-hexane to ethanol is 1:2) to the gold rod solution, and gently shake it by hand for 5 seconds to obtain a hydrophobic nano-gold rod two-dimensional film at the interface of n-hexane and water. After the n-hexane is completely volatilized, a transferable hydrophobic nano-gold rod two-dimensional film is prepared.

[0058] The SEM image of the hydrophobic gold rod two-dimensional membrane is shown in Figure 1 As shown, the length is 90-100 nm and the width is 20-25 nm.

[0059] Example 3

[0060] Preparation of gold nanosphere solution: Add 140mL of deionized water to a three-necked flask, set up a condenser, heat to 137°C, add 10mL of 0.1g sodium citrate solution; add 1mL of 25mM chloroauric acid after 15min, add 5mL of 0.1M tris(hydroxymethyl)aminomethane after 60s, the solution turns to peach pink, keep the temperature for 15min; adjust the temperature of the heating stage to 100°C, cool for 15min; add 1mL of 25mM chloroauric acid, add it again every 20min, keep the temperature for 20min and cool it naturally to obtain a gold nanosphere solution. Centrifuge at 8000rpm for 10min, concentrate 5 times and then disperse it again in deionized water.

[0061] The SEM image of the gold nanoparticles is shown in Figure 2 As shown, the diameter is 30 to 40 nm.

[0062] Example 4

[0063] (1) Preparation of Au-NTs seed solution

[0064] 100 μL of 20 mM HAuCl4 was thoroughly mixed with 9.3 ml of 0.1 M CTAC solution, and after stirring for 1 min, 450 μL of freshly prepared glacial NaBH4 solution (0.01 M) was added to the resulting solution, stirred vigorously for 2 min, and allowed to stand at 30°C for 2 h.

[0065] (2) Synthesis of Au-NTs

[0066] The following two solutions were prepared: HAuCl4 (100 μL, 20 mM) and KI solution (25 μL, 0.01 M) were added to 9.7 mL 0.1 M CTAC solution, mixed until the solution was clear and translucent, and labeled as solution A. In addition, HAuCl4 (300 μL, 20 mM) and KI solution (90 μL 0.01 M) were added to 29.1 mL 0.1 M CTAC solution, mixed until the solution was clear and transparent, and the solution was labeled as solution B. Before synthesis, 185 μL and 500 μL 0.04 M AA were added to solutions A and B, respectively, shaken and manually mixed until the solution changed from light yellow to colorless, indicating Au 3+ Reduction to Au + . In addition, the seeds were diluted 10 times with 0.1 M CTAC, and then 250 μL was added to solution A under stirring. After 5 s (room temperature was 20 °C), the color changed to light pink-purple, and then 150 μL of solution A was quickly added to solution B and manually shaken for 10 s to mix evenly. Within 10 minutes, it can be observed that the solution slowly showed light blue and gradually turned dark blue, and the synthesis was completed.

[0067] (3) Purification of Au-NTs

[0068] The synthesized solution was centrifuged at 3700rpm for 2min. At this time, golden bright spots were deposited on the wall of the centrifuge tube, and there were pink suspended substances around the bright spots and in the supernatant, forming spherical impurities. Gently shake the centrifuge tube to redissolve the pink substance, and quickly pour out the supernatant. Under ultrasonic conditions, redisperse in 15ml CTAC (0.1M), and add 0.15ml NaCl solution (5M) to it, further shake, let stand for 1h to slowly absorb the supernatant, repeat the process until the impurity peak in the UV absorption spectrum is the smallest, and finally redisperse with 0.01M CTAC. The SEM picture of the golden triangle piece is shown below. Figure 3 shown.

[0069] Example 5

[0070] Preparation of hydrophobic SiO2: 100 μL of deionized water was spread horizontally on a 10×10 cm 2 After the ITO glass sheet is formed, the SiO2 aqueous solution and ethanol are mixed in equal volumes by ultrasound to form a SiO2 suspension. 100 μL of the suspension is slowly injected into the deionized water on the ITO glass sheet with a syringe, so that SiO2 is assembled at the water-ethanol interface. After the ethanol is evaporated, a hydrophilic SiO2 substrate is obtained. The hydrophilic SiO2 substrate and the hydrophobic molecule 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane are placed in a vacuum oven for chemical deposition for 12 hours to obtain a hydrophobic SiO2 array.

[0071] The SEM image of the hydrophobic SiO2 array is shown in Figure 4 As shown, the diameter is 2 μm.

[0072] Example 6

[0073] Preparation of super-hydrophobic SERS substrate SiO2@Au NRs based on multi-level micro-nanostructure coupling amplification: Use tweezers to clamp the ITO glass slide loaded with the hydrophobic SiO2 array, with the side loaded with the hydrophobic SiO2 array facing down, and extend it vertically into the quartz beaker to reach the water-oil interface. After the two-dimensional film of hydrophobic noble metal nanoparticles covers the entire surface of the SiO2 regular array, take out the glass slide, and then rinse the loaded surface to obtain the super-hydrophobic SERS substrate SiO2@Au NRs.

[0074] The SEM image of the super-hydrophobic SERS substrate based on multi-level micro-nanostructure coupling amplification is shown in Figure 2. Figure 5 shown.

[0075] The hydrophobicity of the hydrophobic gold rod two-dimensional film prepared in Example 2 and the multi-level micro-nanostructured gold rod two-dimensional film obtained in this example was compared. Figure 6 As shown, the hydrophobic properties of the two-dimensional membrane combined with multi-level micro-nanostructures are improved.

[0076] Application Example 1

[0077] Gold triangles, gold balls, and gold rods were used as SERS substrates, respectively, and methylene blue (10 -4 M) The hybrid nanoparticles all use gold rods. Under the excitation wavelength of 785nm, the coupling enhancement of the gold rod film-gold rod system is most obvious, and the SERS enhancement effect is the best.

[0078] Comparison of SERS intensity of three nanoparticles Figure 7 shown.

[0079] Application Example 2

[0080] In the gold rod film with the strongest enhancement effect, different nanoparticles of gold triangles, gold balls, and gold rods were used to mix with methylene blue (10 -4 M) mixing, the gold rod film-gold sphere system has the strongest coupling effect, which verifies that the best system at the excitation wavelength of 785nm is the gold rod film-gold sphere system.

[0081] Comparison of SERS intensity of three nanoparticle two-dimensional films Figure 8 shown.

[0082] Application Example 3

[0083] Take 10 -5 Methylene blue was used as the dye to be tested, and four samples were made to test the enhancement effect:

[0084] a. Directly drop 8 μL of methylene blue onto the superhydrophobic SiO2;

[0085] b. Drop 8 μL of a mixed solution of methylene blue and gold balls onto the super-hydrophobic SiO2;

[0086] c. Directly drop 8 μL of methylene blue onto the super-hydrophobic substrate SiO2@AuNRs;

[0087] d. 8 μL of the mixed solution of methylene blue and gold balls was dropped onto the superhydrophobic substrate SiO2@Au NRs.

[0088] Comparison of SERS intensity of four samples Fig. 9 As shown, it is proved that the dual coupling effect between the hydrophobic gold rod film and the gold sphere particles is enhanced.

[0089] Application Example 4

[0090] Detection of different concentrations of methylene blue using superhydrophobic substrate (SiO2@AuNRs).

[0091] 10 μL of methylene blue of different concentrations was mixed with 10 μL of gold ball solution, and after oscillation for 3 seconds, 8 μL was taken out and dropped on the super-hydrophobic substrate (SiO2@AuNRs). After the droplet evaporated, SERS was detected.

[0092] The intensity of methylene blue at different concentrations Fig.10 shown.

[0093] Application Example 5

[0094] A common hydrophobic SERS substrate was prepared using a hydrophobic gold rod two-dimensional film. A mixed solution consisting of methylene blue and gold balls was dropped on the common hydrophobic SERS substrate and the super-hydrophobic substrate SiO2@AuNRs, respectively. After the droplets evaporated, the two substrates were placed under a microscope for observation. The results are shown in Figure 2. Fig.11 The two-dimensional film of noble metal nanoparticles in the super-hydrophobic substrate SiO2@Au NRs is combined with the silica substrate to form a micro-nano rough structure, eliminating the coffee ring effect, which cannot be eliminated by a simple hydrophobic gold rod two-dimensional film.

Claims

1. A method for preparing a multi-level micro-nanostructure coupled amplified super-hydrophobic SERS substrate, characterized in that: The steps include: Step (1), preparation of a hydrophobic SiO2 regular array Taking SiO2 nanospheres as the basic unit, a compact and regular SiO2 self-assembled structure was constructed by using ethanol-assisted self-assembly at the air / water interface; the SiO2 array was chemically deposited to modify hydrophobic molecules to obtain a hydrophobic SiO2 self-assembled structure; Step (2), preparation of a hydrophobic noble metal nanoparticle two-dimensional film Placing the noble metal nanoparticles in a reaction container, injecting a n-hexane-ethanol solution of perfluorinated molecules, and completely volatilizing the oil phase n-hexane at 25-50° C. to obtain a hydrophobic two-dimensional film of the noble metal nanoparticles at the water-oil interface; the noble metal nanoparticles are nanogold balls, nanogold rods or gold triangle sheets; and the volume ratio of the noble metal nanoparticles to the n-hexane-ethanol solution of perfluorinated molecules is 5-7:10; Step (3), preparing a super-hydrophobic SERS substrate with multi-level micro-nanostructure coupling amplification The entire hydrophobic SiO2 self-assembled structure surface was covered with a two-dimensional film of noble metal nanoparticles and then rinsed with deionized water to obtain a super-hydrophobic SERS substrate.

2. The method for preparing a multi-level micro-nanostructure coupled amplified super-hydrophobic SERS substrate according to claim 1, characterized in that: The size of the SiO2 nanospheres in step (1) is 2 μm, and the hydrophobic molecule is 1H,1H,2H,2H-perfluorodecyltrichlorosilane.

3. The method for preparing a multi-level micro-nanostructure coupled amplified super-hydrophobic SERS substrate according to claim 1, characterized in that: The chemical deposition environment in step (1) is a vacuum environment, and the chemical deposition time is 12 h.

4. The method for preparing a multi-level micro-nanostructure coupled amplified super-hydrophobic SERS substrate according to claim 1, characterized in that: The noble metal nanoparticles described in step (2) are gold nanorods with a length of 90-100 nm and a width of 20-25 nm.

5. The method for preparing a multi-level micro-nanostructure coupled amplified super-hydrophobic SERS substrate according to claim 1, characterized in that: The perfluorinated molecule in step (2) is perfluorodecyl mercaptan, and the concentration is 10 mM; the volume ratio of n-hexane to ethanol in the n-hexane-ethanol solution of the perfluorinated molecule is 1:

2.

6. The method for preparing a multi-level micro-nanostructure coupled amplified super-hydrophobic SERS substrate according to claim 1, characterized in that: In step (2), the gold nanospheres are prepared from sodium citrate, chloroauric acid and tris(hydroxymethyl)aminomethane solution as raw materials; the gold nanorods are prepared from hexadecyltrimethylammonium bromide (CTAB), sodium borohydride, chloroauric acid, sodium oleate, silver nitrate, hydrochloric acid and ascorbic acid as raw materials; and the gold triangle sheets are prepared from hexadecyltrimethylammonium chloride (CTAC), sodium borohydride, chloroauric acid, potassium iodide, ascorbic acid and sodium chloride as raw materials.

7. A super-hydrophobic SERS substrate prepared by the preparation method according to any one of claims 1 to 6.

8. The use of the super-hydrophobic SERS substrate as claimed in claim 7 in SERS detection, characterized in that Specifically, the test object is mixed with noble metal nanoparticles and then dropped on a super-hydrophobic SERS substrate to form droplets. After the droplets evaporate, SERS is detected under a Raman instrument.

9. The use according to claim 8, characterized in that: The noble metal nanoparticles are one of nanogold balls, nanogold rods or gold triangle sheets; and the object to be detected is a dye.

10. The use according to claim 9, characterized in that: The noble metal nanoparticles are gold nanospheres; and the object to be detected is methylene blue.