A Ni2P / TiO2 S-type heterojunction photoanode material and its application

Through the construction of Ni2P/TiO2 S-type heterojunction photoanode material, the problem of low photogenerated cathodic protection efficiency in marine environment is solved, efficient photoelectric conversion and cathodic protection effects are achieved, and the photogenerated cathodic protection performance is significantly improved.

CN115613037BActive Publication Date: 2024-10-29INST OF OCEANOLOGY - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211188737.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-28
Publication Date
2024-10-29
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

The existing photo-generated cathodic protection technology has low efficiency in the marine environment, and the carriers of a single semiconductor material are small, resulting in low light utilization and easy recombination of carriers, which limits the development of photo-generated cathodic protection.

Method used

Ni2P/TiO2 S-type heterojunction photoanode material is used, and the TiO2 nanotube array is loaded with Ni2P nanoparticles to construct an S-type heterojunction, forming a built-in electric field, improving the photocurrent response and light absorption range, and enhancing the reduction ability of electrons .

Benefits of technology

It significantly improves the photoelectric conversion efficiency, reduces the carrier recombination efficiency, retains holes and electrons with stronger oxidation and reduction capabilities, achieves more effective photogenerated cathode protection, and improves the protective effect of semiconductors on metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115613037B_ABST
    Figure CN115613037B_ABST
Patent Text Reader

Abstract

The present invention relates to a nanocomposite film photoanode material for photogenerated cathode protection, and specifically to a Ni2P / TiO2S-type heterojunction photoanode material and its application. The Ni2P / TiO2S-type heterojunction photoanode material is a TiO2 nanotube array; Ni2P nanoparticles are loaded on the TiO2 nanotube array; and an S-type heterojunction, wherein the Ni2P nanoparticles are dispersedly distributed on the surface of the TiO2 nanotube array. In the material of the present invention, a built-in electric field is constructed between Ni2P and TiO2. Compared with pure TiO2, the Ni2P / TiO2S-type heterojunction photoanode material improves the photoelectric conversion efficiency, reduces the carrier recombination efficiency, retains holes and electrons with stronger oxidation and reduction capabilities, and forms an excellent photogenerated cathode protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a nano composite film photoanode material for photogenerated cathode protection, in particular to a Ni2P / TiO2 S-type heterojunction photoanode material and application thereof. Background Art

[0002] Metal corrosion is a spontaneous process, and its essence is the transformation of single metal into compounds. This is the reverse process of metal smelting. Metal smelting requires a lot of energy and resources and is a consumption process. Corrosion is a spontaneous process of releasing energy. This will cause huge consumption of energy and resources. At present, the problem of energy resources is becoming more and more serious, which is extremely unfavorable to human development. According to a survey, the global average corrosion loss value accounts for as much as 3.4% of the global gross national product (GNP). my country's marine industry is also booming, but it also faces many challenges accordingly. Among them, the problem of corrosion protection in the marine environment is self-evident. Seawater is a complex and highly corrosive electrolyte solution, which contains a large amount of salts and dissolved oxygen of various types, and the conductivity, pH value, temperature, dissolved substances, seawater flow rate and a large number of marine organisms in the ocean are all factors affecting the corrosion of metal substances in seawater. Therefore, the problem of marine corrosion is very complex and serious. Various types of ships, marine exploration equipment, drilling platforms, oil pipelines, offshore wind power equipment, etc. in the marine environment, most of the structures are made of various metal materials such as carbon steel, low alloy steel, stainless steel, etc. These materials are easily damaged by corrosion, which will bring huge economic losses and waste of resources, and even cause serious environmental pollution, trigger catastrophic engineering accidents, and endanger the personal and property safety of ordinary people. To a certain extent, the impact on the economy, resources, and environment caused by material corrosion is much greater than the loss of the material itself. Among them, stainless steel is widely used in marine engineering due to its good corrosion resistance. However, it is also easily corroded in marine environments with high salt, high temperature and high Cl- concentration. In this environment, not only stress corrosion failure will occur, the proportion of which is as high as about 45%, but also severe pitting and pitting corrosion will occur. The main principle is that chloride ions, as active anions, are easily adsorbed, squeeze out oxygen atoms, and react with cations in the passivation film to generate soluble chlorides, destroying the passivation film on the surface of stainless steel, forming small pits, forming closed circuits, and current corrosion, which ultimately leads to severe corrosion.

[0003] At present, the main corrosion protection methods in marine engineering are: coating protection, corrosion inhibitor protection, anodic protection and cathodic protection. Among them, cathodic protection is the most commonly used corrosion protection method in marine engineering, mainly including external power protection method and sacrificial anode protection method. The sacrificial anode cathode protection method is to connect the protected metal with a piece of metal that is more likely to lose electrons than it, forming a macroscopic galvanic cell provided by the metal with a more negative potential, thereby realizing the protection of the metal. This method has relatively low equipment requirements and does not require external power supply, but its limited protection potential difference, limited current that can be provided, current cannot be adjusted and large anode consumption greatly limit its application scope. Impressed current cathodic protection is a protection method that uses an additional DC power supply to directly cathodically polarize the metal to place it in the thermodynamically stable zone. It is widely used because the current is adjustable. However, this protection method requires long-term maintenance and management, requires external power equipment, and consumes a lot of electricity, especially in the current situation where energy and resources are facing depletion. This disadvantage is particularly prominent. In addition, this method is not suitable for use in offshore environments where there is a lack of power systems.

[0004] The marine environment is not only a harsh corrosive environment, but also the place with the most solar energy. This special environment also brings new opportunities for corrosion protection. In recent years, researchers in the field of corrosion protection have developed photogenerated cathodic protection using the photoelectric effect of semiconductors. The main principle of photogenerated cathodic protection is that semiconductors generate photoelectrons under light conditions, and transmit them to the surface of the protected metal through external wires under the action of potential difference, thereby forming cathodic polarization on the metal to achieve protection. Its advantage is that it can utilize solar energy and has no material consumption. It can not only play the role of cathodic protection, but also achieve clean energy and pollution corrosion protection.

[0005] The cathodic protection of semiconductor materials depends on the size of photogenerated carriers. The more carriers there are, the better the cathodic protection effect is, and the fewer carriers there are, the worse the protection effect is. At present, most single semiconductors have small carriers. The main reason is that the band gap is large, only ultraviolet light can be absorbed, and carriers are easy to recombine. This greatly limits the development of its photogenerated cathodic protection.

[0006] The construction of heterojunctions by combining different semiconductors is an effective way to solve the problems of low light utilization and easy recombination of carriers. Traditionally, there are three types of heterojunctions formed by the combination of two semiconductors: nested (type I), staggered (type II), and disconnected (type III). In type I, photogenerated carriers are all transferred to the same semiconductor. If they cannot be removed in time, recombination is easily induced. In type III, due to the effect of energy barriers, the transfer of carriers between the two semiconductors cannot be completed, and the electron-hole pairs cannot be effectively separated. Only in type II can the electrons and holes generated by light excitation be transferred to two different semiconductors respectively, completing the effective separation of carriers and increasing the photoelectric properties of a single semiconductor material. However, the efficiency of type II photogenerated electron-hole separation is at the expense of reducing the redox ability of the two semiconductor photocatalysts, which is unfavorable for the cathode.

[0007] In recent years, researchers have discovered an S-type heterojunction system that is more conducive to photoelectric conversion. The S-type heterojunction is constructed in a staggered manner by a reduced semiconductor with a small work function and a high Fermi level and an oxidized semiconductor with a large work function and a low Fermi level, which can effectively separate electron-hole pairs with strong redox ability. At present, a large number of studies have been conducted on the application of type II heterojunctions in photogenerated cathode protection, while there are still no related reports on S-type heterojunctions. Therefore, it is very necessary to construct an S-type inhibitor and explore its application in photogenerated cathode protection. Summary of the invention

[0008] The present invention aims to provide a Ni2P / TiO2 S-type heterojunction photoanode material and its application.

[0009] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0010] A Ni2P / TiO2 S-type heterojunction photoanode material:

[0011] TiO2 nanotube array;

[0012] Ni2P nanoparticles loaded on the TiO2 nanotube array;

[0013] The S-type heterojunction is composed of Ni2P nanoparticles dispersedly distributed on the surface of the TiO2 nanotube array.

[0014] The Ni2P nanoparticles and the TiO2 nanotube array form a built-in electric field.

[0015] Compared with pure TiO2, the photocurrent response of the Ni2P / TiO2 S-type heterojunction photoanode material is improved by at least 8 times.

[0016] The sheet resistance of the Ni2P / TiO2 S-type heterojunction photoanode material is reduced by no less than 3.0 E5Ω.

[0017] The bandgap width of the Ni2P / TiO2 S-type heterojunction photoanode material is reduced by 0.128 eV.

[0018] A method for preparing a Ni2P / TiO2 S-type heterojunction photoanode material,

[0019] Obtaining TiO2 nanotube arrays;

[0020] Ni2P nanoparticles are loaded on the TiO2 nanotube array by a hydrothermal method to form an S-type heterojunction photoanode material.

[0021] Specifically:

[0022] (a) NiCl2·6H2O, red phosphorus, ascorbic acid and polyvinyl pyrrolidone (PVP) were selected as raw materials, ultrapure water was used as solvent, and magnetic stirring was used to dissolve each substance in water to form a uniform precursor solution for standby use; wherein Ni in the precursor solution 2+ The final concentration is 1-30 mmol / L; the mass ratios of NiCl2·6H2O: red phosphorus, ascorbic acid and polyvinylpyrrolidone (PVP) are: (1.89-3.78): (1.39-2.78): (2-3): (1-1.5);

[0023] (b) transferring the precursor solution into a hydrothermal reactor, and placing the TiO2 nanotube array in an inclined manner in the hydrothermal reactor;

[0024] (c) placing the reactor in a forced air drying oven at 140-160° C. for 12-15 h, cooling naturally and washing with deionized water and anhydrous ethanol for several times, and finally vacuum drying at 60-80° C. for 12-15 h to obtain a Ni2P / TiO2 S-type heterojunction photoanode material.

[0025] The TiO2 nanotube array is obtained by an anodic oxidation method using a platinum sheet as a cathode and a titanium plate as an anode, and ethylene glycol containing ammonium fluoride as an electrolyte; wherein the mass ratio of ammonium fluoride to ethylene glycol is 1:150-1:200.

[0026] The anodizing method comprises the following steps: providing a DC voltage of 20 to 40 V by a DC power supply, the anodizing time being 1 to 2 hours, calcining at 450 to 600° C. for 120 to 200 minutes in a muffle furnace, and obtaining a TiO2 nanotube array after natural cooling.

[0027] An application of a Ni2P / TiO2 S-type heterojunction photoanode material, and an application of the Ni2P / TiO2 S-type heterojunction photoanode material in photogenerated cathode protection.

[0028] The basic principle of the present invention is that the nanoparticle Ni2P and the TiO2 nanotube array are combined to construct an S-type heterojunction. The excellent nanoparticles and tubular structure are conducive to the capture of light. The S-type heterojunction constructed by Ni2P and TiO2 reduces the bandgap width of the composite photoanode and enhances the light absorption range. The Ni2P / TiO2S-type heterojunction forms a built-in electric field, realizes the effective transfer of photogenerated carriers under illumination conditions, and retains photogenerated electrons with stronger reducibility. Finally, the photogenerated electrons are transferred to the stainless steel electrode with a lower potential, causing the potential of the stainless steel electrode to shift negatively, thereby placing it in a cathodic protection state, thereby achieving the purpose of slowing down corrosion. Therefore, the Ni2P / TiO2 S-type heterojunction photoanode material can effectively improve the photogenerated cathodic protection effect of semiconductors on metals.

[0029] The advantages of the present invention are:

[0030] The present invention obtains an S-type heterojunction photoanode material with high light absorption, low carrier recombination rate and strong electron reduction energy by matching the semiconductor energy band structure and rationally optimizing the structure of the heterojunction material, thereby effectively improving the photoelectric performance of the photoanode material and solving the problem of low photogenerated cathode protection performance; specifically:

[0031] 1. A built-in electric field is constructed between Ni2P and TiO2 in the Ni2P / TiO2 S-type heterojunction photoanode material obtained by the present invention. Compared with pure TiO2, the Ni2P / TiO2 S-type heterojunction photoanode material improves the photoelectric conversion efficiency, reduces the carrier recombination efficiency, retains holes and electrons with stronger oxidation and reduction capabilities, and forms excellent photogenerated cathode protection.

[0032] 2. The material obtained by the present invention has strong light absorption and energy absorption, which significantly increases the light absorption range.

[0033] 3. The material obtained by the present invention reduces the film resistance, is beneficial to the photoelectric effect, and improves the photocurrent response

[0034] 4. The material obtained by the present invention reduces the carrier recombination efficiency, retains holes and electrons with stronger oxidation and reduction capabilities, and is conducive to generating more electrons with stronger reduction capabilities.

[0035] 5. The material obtained by the present invention can effectively improve the photo-induced cathode protection effect of semiconductors on metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1This is an X-ray diffraction (XRD) diagram of the Ni2P / TiO2 S-type heterojunction photoanode material provided in Example 1 of the present invention.

[0037] Figure 2 Scanning electron microscope (SEM) images of (a) pure TiO2 and (b) Ni2P / TiO2 S-type heterojunction photoanode materials provided in Example 1 of the present invention.

[0038] Figure 3 The 304L stainless steel provided in Example 1 of the present invention is coupled with pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in a 3.5% NaCl solution, and the electrode potential changes with time before and after illumination. The horizontal axis is time (s), and the vertical axis is the electrode potential (V vs. SCE). On means illumination, and off means turning off the light source.

[0039] Figure 4 The photocurrent variation curve of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials provided in Example 1 of the present invention before and after illumination, where the horizontal axis is time (s) and the vertical axis is current density (μA / cm 2 ).

[0040] Figure 5 Curve a is a graph of the ultraviolet visible absorption spectrum (UV-DRS) of pure TiO2 and curve b is a graph of the Ni2P / TiO2 S-type heterojunction photoanode material provided in Example 1 of the present invention.

[0041] Figure 6 Nyquist plots of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials provided in Example 1 of the present invention.

[0042] Figure 7 Schematic diagram of the S-type energy band structure and IEF formation of the Ni2P / TiO2 S-type heterojunction photoanode material provided in Example 1 of the present invention.

[0043] Figure 8 This is a diagram of the S-type electron transfer path of the Ni2P / TiO2 S-type heterojunction photoanode material provided in Example 1 of the present invention.

[0044] Fig. 9 The 304L stainless steel provided in Example 2 of the present invention is coupled with pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in a 3.5% NaCl solution, and the electrode potential changes with time before and after illumination. The horizontal axis is time (s), and the vertical axis is the electrode potential (V vs. SCE). On means illumination, and off means turning off the light source.

[0045] Fig.10The photocurrent variation curve of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials provided in Example 2 of the present invention before and after illumination, where the horizontal axis is time (s) and the vertical axis is current density (μA / cm 2 ).

[0046] Fig.11 Curve a, pure TiO2, and curve b, Ni2P / TiO2 S-type heterojunction photoanode materials provided in Example 2 of the present invention are ultraviolet visible absorption spectra (UV-DRS) graphs.

[0047] Fig.12 Nyquist diagram of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials provided in Example 2 of the present invention. DETAILED DESCRIPTION

[0048] The specific implementation modes of the present invention are further described below in conjunction with examples. It should be noted that the specific implementation modes described here are only for illustrating and explaining the present invention, and are not limited to the present invention.

[0049] The Ni2P / TiO2 S-type heterojunction photoanode material of the present invention is composed of Ni2P nanoparticles dispersedly distributed on the surface of a TiO2 nanotube array. The construction of the S heterojunction can improve the structural state of TiO2 and enhance its photoelectric conversion performance, thereby further improving its photogenerated cathode protection effect. In addition, Ni2P has metal-like properties and exhibits good electronic conductivity, which is conducive to the rapid transfer of photogenerated electrons. It can also improve the overall photoelectric effect of the Ni2P / TiO2 S heterojunction, thereby further improving its photogenerated cathode protection effect.

[0050] The photocathodic protection effect of the Ni2P / TiO2 S-type heterojunction photoanode material prepared as described below was tested, specifically using a dual electrolytic cell system consisting of a photoelectrolytic cell and a corrosion electrolytic cell. In the photoelectrolytic cell, the Ni2P / TiO2 S-type heterojunction photoanode material is used as the anode in an electrolyte of 0.1M Na2S and 0.2M NaOH solution. The corrosion electrolytic cell is a three-electrode system, the working electrode is the protected metal (316L stainless steel), the counter electrode is a Pt electrode, the reference electrode is a saturated calomel electrode (SCE), and the corrosion medium is a NaCl solution with a mass concentration of 3.5%. The photoanode and the protected metal electrode are connected by a wire as the working electrode, and the photoelectrolytic cell and the corrosion electrolytic cell are connected by a salt bridge (agar containing saturated KCl). A 300W high-pressure xenon lamp with a wavelength of ≥400nm is used as a visible light source to directly irradiate the surface of the nanotube composite film in the photoelectrolytic cell, and the potential change of the stainless steel electrode before and after illumination is tested using an electrochemical workstation.

[0051] The photocurrent of the Ni2P / TiO2 S-type heterojunction photoanode material prepared as described below was tested, specifically using a dual electrolytic cell system consisting of a photoelectrolytic cell and a corrosion electrolytic cell. In the photoelectrolytic cell, the Ni2P / TiO2 S-type heterojunction photoanode material was used as the anode and placed in an electrolyte of 0.1M Na2S and 0.2M NaOH solution. To avoid the influence of polarization on the photocurrent test, the 304ss electrode was connected to the ground interface of the chemical workstation (GNE), and the reference electrode (RE) interface of the chemical workstation was short-circuited with the counter electrode (CE) interface.

[0052] The light absorption performance of the Ni2P / TiO2 S-type heterojunction photoanode material prepared below was tested, and the bandgap width of the prepared sample was obtained by converting it using the Tauc plot method. The wavelength range of the test process was 200-800nm, with barium sulfate as the reference.

[0053] The electrochemical impedance spectroscopy test was performed on the Ni2P / TiO2 S-type heterojunction photoanode material prepared as follows. The system used was a three-electrode system, in which the Pt electrode was the counter electrode, the saturated calomel electrode (SCE) was the reference electrode, the Ni2P / TiO2 S-type heterojunction photoanode material was the working electrode, and the solution used was a 0.1 mol / L Na2SO4 solution. The electrochemical workstation was CHI760E, the test amplitude was 10mV, the frequency range was 10-2~105Hz, and it was carried out under no light conditions.

[0054] The Vienna Ab-initio Simulation Package (VASP) was used to analyze the structure and electronic properties, and density functional theory (DFT) calculations were performed on Ni2P / TiO2.

[0055] Example 1

[0056] 1) Cut a commercially available titanium plate (purity of 99.9%) into samples of 0.3 mm × 10 mm × 20 mm, and ultrasonically clean them several times with pure water and acetone for 20 minutes each time to remove inorganic or organic impurities on the surface of the sample, and dry them at room temperature for later use.

[0057] 2) First, dissolve 0.9g of ammonium fluoride (NH4F) in 5mL of pure water, then add 12mL of hydrogen peroxide (H2O2) and 12mL of nitric acid (65% HNO3) in turn and stir evenly with a magnetic stirrer to obtain a polishing solution. Immerse the titanium plate sample after the above treatment in the polishing solution and chemically polish until the surface of the sample is uniform, smooth and free of impurities. Then take it out and ultrasonically clean it twice with pure water and anhydrous ethanol alternately, each time for 10 minutes, to obtain a clean titanium plate sample. Finally, store it in anhydrous ethanol for later use.

[0058] 3) The method for preparing TiO2 nanotube array on the surface of the titanium plate sample after the above polishing treatment is as follows:

[0059] (1) 0.44 g NH4F was dissolved in 8 mL pure water, and then 80 mL ethylene glycol was added and stirred evenly using a magnetic stirrer to obtain an electrolyte for preparing TiO2 nanotube arrays.

[0060] (2) Pour 80 mL of the above electrolyte into a 200 mL beaker, connect the above polished and cleaned titanium plate sample to the positive electrode of the DC power supply, and connect the platinum foil (20 mm × 20 mm) to the negative electrode of the DC power supply to build a two-electrode system. Set the voltage to +20 V and the reaction time to 1 h. After the reaction is completed, rinse the sample alternately with pure water and anhydrous ethanol several times. After drying at room temperature, place the sample in a muffle furnace, set the heating rate to 5 ° C / min, calcine at 450 ° C for 120 minutes, and obtain a TiO2 nanotube array after natural cooling. The surface morphology of the TiO2 nanotube array is as follows Figure 2 As shown in (a), it can be seen that the nanotubes in the nanotube array are relatively uniform, with tube diameters ranging from 60 to 80 nanometers.

[0061] 4) Preparation of Ni2P / TiO2 S-type heterojunction photoanode materials

[0062] (1) First, 29.6 mg NiCl2·6H2O, 21.8 mg red phosphorus, 31.2 mg ascorbic acid, and 15.6 mg polyvinylpyrrolidone (PVP) were weighed and placed in a beaker containing 60 mL ultrapure water and stirred with a magnetic stirrer for 1 h to fully form a uniform precursor solution.

[0063] (2) The above precursor solution was transferred to a 100 mL hydrothermal reactor, and the TiO2 nanotube array was placed tilted in the hydrothermal reactor. The reactor was then placed in a forced air drying oven at 140°C for 12 h, and after natural cooling, it was alternately washed with deionized water and anhydrous ethanol for several times, and finally vacuum dried at 60°C for 12 h to obtain the Ni2P / TiO2 S-type heterojunction photoanode material.

[0064] The Ni2P / TiO2 S-type heterojunction photoanode material obtained in Example 1 was subjected to crystal analysis.

[0065] Figure 1The XRD patterns of the sample NPTs-15 nanostructured material are compared with the standard PDF card. The diffraction peaks of Ti in the Ti substrate at 2θ = 35.0°, 38.4°, 40.1°, 53.0°, 70.6° and 76.2° are (JCPDS No. 44–1294). The peaks at 2θ of 25.3°, 48.1° and 82.6° are attributed to the anatase TiO2 (101), (200) and (224) crystal planes (JCPDS No. 21–1272). This indicates that anatase TiO2 can be successfully formed on the Ti substrate after anodization and high temperature calcination annealing at 450°C. In addition, 2θ=40.7°, 44.5°, 47.3°, 54.2°, and 54.9° correspond to Ni2P (111), (201), (210), (300), and (211) crystal planes (JCPDS No.03-0953), respectively. This indicates that the Ni2P / TiO2 S-type heterojunction photoanode material was successfully obtained by the above preparation method.

[0066] The pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials obtained in Example 1 were analyzed by scanning electron microscope. Figure 2 .pass Figure 2 (a) It can be seen that the nanotube array in the TiO2 nanotube array is relatively uniform, with an average inner diameter of about 60-80nm, a characterization deviation of about 6nm, a wall thickness of 10-15nm, and a length of 650-700nm. Figure 2 (b) It can be seen that only round block-shaped nanoparticles are distributed at the mouth of the TiO2 nanotube, indicating that the Ni2P nanoparticles exist in the form of nanoparticles on the surface of the TiO2 nanotube, and together construct the Ni2P / TiO2 S-type heterojunction photoanode material.

[0067] The pure TiO2 nanotube array and the Ni2P / TiO2 S-type heterojunction photoanode material obtained in the above Example 1 were coupled to 304 stainless steel, respectively, and the electrode potential of the 304 stainless steel in simulated seawater was tested over time.

[0068] Depend on Figure 3 It can be seen that the electrode potential of 304 stainless steel coupled with TiO2 nanotube array under intermittent illumination drops to about -460mV, which has a certain photogenerated cathode protection effect. When coupled with Ni2P / TiO2 S-type heterojunction photoanode material, the potential of 304 stainless steel can be reduced to about -830mV, which is significantly lower than its self-corrosion potential. When the light source is cut off, the electrode potential of stainless steel begins to rise, but at this time the electrode potential of 304 stainless steel is still far lower than its self-corrosion potential. When the light is irradiated again, the electrode potential of stainless steel connected to the composite film drops rapidly again, indicating that the composite film has a good photogenerated cathode protection effect and good stability.

[0069] In order to characterize the photogenerated carrier separation ability and recombination rate of the pure TiO2 nanotube array and Ni2P / TiO2 S-type heterojunction photoanode material obtained in Example 1, the transient photocurrent spectrum of the sample was tested. Figure 4 It can be seen that when the sample is pure TiO2, the maximum transient photocurrent density under light on is 6.9μA / cm 2 The steady-state current is 6.6 μA / cm 2 When the sample is a Ni2P / TiO2 S-type heterojunction photoanode material, the maximum transient photocurrent under light on is 209.4μA / cm 2 , which is about 30.3 times that of pure TiO2 nanotube arrays. The transient photocurrent of Ni2P / TiO2 S-type heterojunction photoanode material finally stabilized at 29.9μA / cm 2 The photocurrent intensity of Ni2P / TiO2 S-type heterojunction photoanode material is significantly enhanced, which is about 4.53 times that of pure TiO2 nanotubes, and far exceeds the transient photocurrent of pure TiO2 nanotube arrays. This result shows that the photocurrent intensity of Ni2P / TiO2 S-type heterojunction photoanode material is significantly enhanced. This is mainly because Ni2P / TiO2 S-type heterojunction photoanode material can reduce the recombination of photogenerated electron-hole pairs and effectively improve the utilization rate of light.

[0070] The UV-visible absorption spectra of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in Example 1 are analyzed. Figure 5 . The test results show that the light absorption range of pure TiO2 nanotube arrays is mainly in the ultraviolet region, and its spectral absorption edge is about 380nm. The absorption intensity of the nano Ni2P / TiO2 S-type heterojunction photoanode material in both the ultraviolet and visible light regions increased significantly, indicating that the Ni2P / TiO2 S-type heterojunction photoanode material effectively improves the absorption capacity of the TiO2 nanotube array for ultraviolet and visible light. In addition, the bandgap width of the sample can be obtained by plotting after conversion with the Kubelka-Munk equation. From Figure 5 (b) The band gaps of pure TiO2 and NPTs-15 are 3.28 eV and 3.1 eV, respectively. These data indicate that loading Ni2P onto TiO2 can effectively broaden its light absorption range and enhance its light absorption.

[0071] The pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in Example 1 were subjected to AC impedance test analysis. The results showed that the impedance of the Ni2P / TiO2 S-type heterojunction photoanode material (Figure (6) b) was much smaller than that of pure TiO2, as shown in Table 1. ct ) is 1.063E4 Ω·cm 2, pure TiO2 charge transfer resistance (R ct ) is 3.827E5Ω·cm 2 That is, the conductivity of Ni2P / TiO2 S-type heterojunction photoanode material is lower than that of pure TiO2, which is beneficial to the separation of semiconductor photogenerated carriers and the photoelectric effect.

[0072] Table 1 AC impedance test of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials

[0073]

[0074] The electron energy band and density inverse function calculations of the pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in Example 1 revealed that their work functions were 5.1 and 3.46 eV ( Figure 7 ). When the two come into contact with each other, electrons are transferred from Ni2P with a smaller work function to TiO2 with a larger work function, forming a band bending and a built-in electric field from Ni2P to TiO2, which helps to quickly separate the photogenerated carriers, form more photogenerated electrons, and improve the photoelectric effect.

[0075] The photoinduced cathode protection mechanism of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in Example 1 was analyzed. Figure 8 It was found that under illumination, the TiO2 conduction band photoelectrons in the Ni2P / TiO2 S-type heterojunction photoanode material recombined with the Ni2P valence band under the action of the built-in electric field, and at the same time, the electrons with stronger oxidation and reduction were retained in the TiO2 valence band and Ni2P conduction band, respectively, thus forming an S-type heterojunction. The electrons with stronger reduction were transferred to the 304 stainless steel through the external circuit under the action of the potential difference, thereby forming cathodic protection for the 304.

[0076] Example 2

[0077] 1) Cut a commercially available titanium plate (purity of 99.9%) into samples of 0.3 mm × 10 mm × 20 mm, and ultrasonically clean them several times with pure water and acetone for 20 minutes each time to remove inorganic or organic impurities on the surface of the sample, and dry them at room temperature for later use.

[0078] 2) First, dissolve 0.9g of ammonium fluoride (NH4F) in 5mL of pure water, then add 12mL of hydrogen peroxide (H2O2) and 12mL of nitric acid (65% HNO3) in turn and stir evenly with a magnetic stirrer to obtain a polishing solution. Immerse the titanium plate sample in the polishing solution and chemically polish until the surface of the sample is uniform, smooth and free of impurities. After taking it out, alternately ultrasonically clean it with pure water and anhydrous ethanol for 2 times, each time for 10 minutes, to obtain a clean titanium plate sample. Finally, store it in anhydrous ethanol for later use.

[0079] 3) The method for preparing TiO2 nanotube array on the surface of titanium plate sample is as follows:

[0080] (1) 0.44 g NH4F was dissolved in 8 mL pure water, and then 80 mL ethylene glycol was added and stirred evenly using a magnetic stirrer to obtain an electrolyte for preparing TiO2 nanotube arrays.

[0081] (2) 80 mL of the above electrolyte was placed in a 200 mL beaker, the clean titanium plate sample was connected to the positive electrode of the DC power supply, and the platinum foil (20 mm × 20 mm) was connected to the negative electrode of the DC power supply to build a two-electrode system. The voltage was set to +20 V and the reaction time was 1 h. After the reaction was completed, the sample was rinsed alternately with pure water and anhydrous ethanol for several times. After drying at room temperature, the sample was placed in a muffle furnace, the heating rate was set to 5 ° C / min, and calcined at 450 ° C for 120 minutes. After natural cooling, the TiO2 nanotube array was obtained.

[0082] 4) Preparation of Ni2P / TiO2 S-type heterojunction photoanode materials

[0083] (1) First, 59.2 mg NiCl2·6H2O, 43.6 mg red phosphorus, 62.4 mg ascorbic acid, and 31.2 mg polyvinylpyrrolidone (PVP) were weighed and placed in a beaker containing 60 mL ultrapure water and stirred with a magnetic stirrer for 1 h to fully form a uniform precursor solution.

[0084] (2) The above precursor solution was transferred to a 100 mL hydrothermal reactor, and the TiO2 nanotube array was placed tilted in the hydrothermal reactor. The reactor was then placed in a forced air drying oven at 140°C for 12 h, and after natural cooling, it was alternately washed with deionized water and anhydrous ethanol for several times, and finally vacuum dried at 60°C for 12 h to obtain the Ni2P / TiO2 S-type heterojunction photoanode material.

[0085] The pure TiO2 nanotube array and the Ni2P / TiO2 S-type heterojunction photoanode material obtained in Example 2 were coupled to 304 stainless steel, and the electrode potential of 304 stainless steel in simulated seawater was tested over time. Fig. 9It can be seen that the electrode potential of 304 stainless steel coupled with TiO2 nanotube array under intermittent illumination drops to about -460mV, which has a certain photogenerated cathode protection effect. When coupled with Ni2P / TiO2 S-type heterojunction photoanode material, the potential of 304 stainless steel can be reduced to about -780mV, which is significantly lower than its self-corrosion potential. When the light source is cut off, the electrode potential of stainless steel begins to rise, but at this time the electrode potential of 304 stainless steel is still far lower than its self-corrosion potential. When the light is irradiated again, the electrode potential of stainless steel connected to the composite film drops rapidly again, indicating that the composite film has a good photogenerated cathode protection effect and good stability.

[0086] In order to characterize the photogenerated carrier separation ability and recombination rate of the pure TiO2 nanotube array and Ni2P / TiO2 S-type heterojunction photoanode material obtained in Example 2, the transient photocurrent spectrum of the sample was tested. Fig.10 It can be seen that when the sample is pure TiO2, the maximum transient photocurrent density under light on is 6.9μA / cm 2 The steady-state current is 6.6 μA / cm 2 When the sample is a Ni2P / TiO2 S-type heterojunction photoanode material, the maximum transient photocurrent under light on is 104.6μA / cm 2 , which is about 15 times that of pure TiO2 nanotube arrays. The transient photocurrent of the Ni2P / TiO2 S-type heterojunction photoanode material finally stabilized at 20.7μA / cm 2 The photocurrent intensity of Ni2P / TiO2 S-type heterojunction photoanode material is significantly enhanced, which is mainly due to the fact that Ni2P / TiO2 S-type heterojunction photoanode material can reduce the recombination of photogenerated electron-hole pairs and effectively improve the utilization rate of light.

[0087] The UV-visible absorption spectra of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in Example 2 are analyzed. Fig.11 The test results show that the light absorption range of pure TiO2 nanotube array is mainly in the ultraviolet region. The absorption intensity of nano Ni2P / TiO2 S-type heterojunction photoanode material in both ultraviolet and visible light regions increased significantly, indicating that Ni2P / TiO2 S-type heterojunction photoanode material effectively improves the absorption capacity of TiO2 nanotube array to ultraviolet and visible light.

[0088] The pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials in Example 2 were subjected to AC impedance test analysis. The results showed that the impedance of the Ni2P / TiO2 S-type heterojunction photoanode material (Figure (12) b) was much smaller than that of pure TiO2, as shown in Table 2. ct ) is 2.947E4 Ω·cm 2 , pure TiO2 charge transfer resistance (R ct ) is 3.827E5Ω·cm 2 That is, the conductivity of Ni2P / TiO2 S-type heterojunction photoanode material is lower than that of pure TiO2, which is beneficial to the separation of semiconductor photogenerated carriers and the photoelectric effect.

[0089] Table 2 AC impedance test of pure TiO2 and Ni2P / TiO2 S-type heterojunction photoanode materials

[0090]

[0091] The Ni2P / TiO2 S-type heterojunction photoanode material described in the present invention can inhibit metal corrosion, has an excellent photoelectric conversion effect, and can play a good photoinduced cathode protection effect on 304 stainless steel as a photoanode.

[0092] Other preparation methods not exemplified can be easily implemented under the guidance of the above two preparation methods and will not be described in detail here.

[0093] It should be understood that, under the guidance of the present invention, ordinary technicians in this field can also make various variations such as replacement, modification, combination, etc. without departing from the scope of protection of the claims of the present invention. The scope of protection of the rights of the present invention shall be based on the claims.

Claims

1. A Ni 2 P / TiO 2 S-type heterojunction photoanode materials, Features: TiO 2 Nanotube arrays; Ni 2 P nanocrystalline particles, which are loaded on the TiO 2 Nanotube arrays; S-type heterojunction, wherein the Ni 2 P nanocrystal particles are dispersed in the TiO 2 The surface of the nanotube array is composed of 2 P nanoparticles and the TiO 2 The nanotube array creates a built-in electric field.

2. A Ni according to claim 1 2 P / TiO 2 Preparation method of S-type heterojunction photoanode material, Features: Obtaining TiO 2 Nanotube arrays; The TiO 2 Ni loaded on nanotube array 2 P nanoparticles form S-type heterojunction photoanode materials; Ni 2 P / TiO 2 The specific preparation method of S-type heterojunction photoanode material is as follows: (a) Select NiCl 2 6H 2 O, red phosphorus, ascorbic acid and polyvinyl pyrrolidone (PVP) were used as raw materials, ultrapure water was used as solvent, and magnetic stirring was used to dissolve each substance in water to form a uniform precursor solution for standby use; among them, Ni 2+ The final concentration of NiCl is 1-30 mmol / L; 2 6H 2 O: The mass ratio of red phosphorus, ascorbic acid and polyvinylpyrrolidone (PVP) is: (1.89-3.78): (1.39-2.78): (2-3): (1-1.5); (b) transferring the precursor solution to a hydrothermal reactor and adding the TiO 2 The nanotube array is placed tilted in a hydrothermal reactor; (c) placing the reactor in a forced air drying oven at 140-160°C for 12-15 hours, cooling naturally and washing with deionized water and anhydrous ethanol alternately for several times, and finally drying under vacuum at 60-80°C for 12-15 hours to obtain Ni 2 P / TiO 2 S-type heterojunction photoanode materials.

3. Ni according to claim 2 2 P / TiO 2 Preparation method of S-type heterojunction photoanode material, Features: The TiO 2 The nanotube array uses a platinum sheet as cathode, a titanium plate as anode, and ethylene glycol containing ammonium fluoride as electrolyte to obtain TiO by anodic oxidation. 2 Nanotube array; wherein the mass ratio of ammonium fluoride to ethylene glycol is 1:150-1:

200.

4. Ni according to claim 3 2 P / TiO 2 Preparation method of S-type heterojunction photoanode material, Features: The anodizing method comprises the following steps: providing a DC voltage of 20 to 40 V by a DC power supply, the anodizing time being 1 to 2 h, calcining in a muffle furnace at 450 to 600° C. for 120 to 200 minutes, and naturally cooling to obtain TiO 2 Nanotube arrays.

5. The Ni according to claim 1 2 P / TiO 2 Application of S-type heterojunction photoanode materials, Features: The Ni 2 P / TiO 2 Application of S-type heterojunction photoanode materials in photogenerated cathodic protection.