Preparation method of anti-pollution oxide film on pure titanium surface
By performing anodizing and vacuum annealing treatment in an oxygen-rich environment, the amorphous TiO2 is converted into anatase structure TiO2, which solves the problem of insufficient catalytic activity caused by insufficient oxygen in the prior art, and achieves efficient photocatalysis and resistance Oil stain performance, suitable for photocatalysis and material self-cleaning.
Patent Information
- Application Number
- CN202211262661.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-10-14
AI Technical Summary
The oxide film prepared by electrochemical anodizing/microar oxidation method on the surface of existing titanium alloys is mainly composed of hypoxic titanium oxide, amorphous TiO2 and nanocrystalline anatase phases, lacking photocatalytic and anti-oil stain characteristics, and due to insufficient oxygen The formed hypoxic oxide leads to insufficient catalytic activity.
Anodized in an oxygen-rich environment, an electrolyte containing 0.3% NH4F and 2% H2O was used, and the amorphous TiO2 was converted into anatase structure TiO2 by constant current anodization and vacuum annealing. Avoid the formation of hypoxic oxides.
Anatase structure TiO2 oxide film with high photocatalytic activity and oil-resistant properties was prepared, which can quickly degrade oil-stained and organic pollutants under ultraviolet light, prevent microbial contamination, and is used in the fields of photocatalysis, antibacterial and self-cleaning of materials.
Smart Images

Figure BDA0003891855470000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material surface treatment, and in particular relates to a method for preparing an anti-pollution oxide film on the surface of pure titanium. Background Art
[0002] TiO prepared on titanium alloy surface by electrochemical anodic oxidation / micro-arc oxidation 2 Thin films are widely used in corrosion protection, photocatalysis, bioengineering and other fields due to their simple preparation method, low cost, strong load capacity and long service life. However, the oxide film generated by anodic oxidation / micro-arc oxidation is mainly composed of oxygen-deficient titanium oxide, amorphous TiO 2 and partly nanocrystalline anatase phase. Oxygen-deficient and amorphous TiO 2 It does not have photocatalytic and anti-oil properties. Compared with non-stoichiometric titanium oxide and amorphous TiO 2 , crystalline TiO 2 It has higher photocatalytic activity. Among them, the anatase structure TiO 2 The band gap is 3.2eV, and the rutile structure of TiO 2 The band gap is 3.0 eV, and the anatase structure of TiO 2 Because the lattice contains more defects and dislocations, more oxygen vacancies are generated to capture electrons, which has stronger catalytic activity. Therefore, the anatase structure of TiO 2 It can quickly degrade a variety of organic solutes and has good photocatalytic, antibacterial and anti-oil properties. Summary of the invention
[0003] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to prepare an oxide film with strong anti-oil performance on the surface of pure titanium, which adopts a specific electrolyte and performs anodization in an oxygen-rich environment, which greatly reduces the amount of oxygen-deficient oxides generated and increases the stoichiometric TiO 2 The amount of production; then through a specific heat treatment process to make amorphous TiO 2 , and is converted into anatase TiO2 with strong photocatalytic and oil-reducing properties. 2 The technical problem of oxygen-deficient oxides formed by insufficient oxygen in the prior art is solved. Under ultraviolet light, anatase TiO 2 It can quickly degrade oil stains on its surface and prevent microbial contamination.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing an anti-pollution oxide film on the surface of pure titanium, comprising the following steps:
[0005] ① The titanium sample was polished with 600-mesh, 800-mesh and 1200-mesh sandpapers in turn; then the titanium sample was immersed in a solution containing 1% HF and 2% HNO 3The titanium sample was chemically polished in a solution of 5-10s; the polished titanium sample was then ultrasonically cleaned in acetone for 20min, washed with distilled water for multiple times and dried for later use.
[0006] ② Prepare the electrolyte and introduce high-purity oxygen into the bottom of the electrolyte for 10-30 minutes before anodization. The electrolyte has a mass content of 0.3% NH 4 F and 2% H 2 O ethylene glycol mixed electrolyte, the use of fluorinated ethylene glycol solution can improve the geometric characteristics of pure titanium surface oxides, which has a very important influence on the specific surface area and photocatalytic performance; the electrolyte solution contains 2% H 2 O can increase the migration rate of ions. The concentration of high-purity oxygen in step ② is ≥99%, and the electrolyte is always in an oxygen-rich environment. Anodizing under oxygen-rich conditions can avoid the formation of oxygen-deficient oxides due to insufficient oxygen, thereby increasing the stoichiometric TiO 2 The amount of generation.
[0007] ③ The sample in step ① is subjected to anodizing treatment. The oxygen is continuously supplied during the entire anodizing process to keep the oxygen content in the electrolyte in a supersaturated state. Ultrasonic waves are used to stir the solution during the anodizing process. The ultrasonic frequency is 50-100KHz. After the anodizing process is completed, the sample is rinsed with distilled water for multiple times and dried with cold air. The anodizing method in step ③ is constant current anodizing; the anodizing current is 1-3A / dm 2 The anodizing time is 10-30 minutes, so that the pure titanium surface is fully oxidized during the anodizing process.
[0008] ④ Perform vacuum annealing on the sample dried in step ③, with a vacuum degree of ≥10 -2 Pa, the holding time is 30-80min, and then cooled to room temperature with the furnace. The vacuum annealing holding temperature in step ④ is 400℃-500℃, and the holding time is preferably 40-60min. If the annealing temperature is too low, it is easy to transform into brookite structure TiO 2 If the temperature is too high, it will transform into rutile structure TiO 2 .
[0009] A pure titanium surface anti-pollution oxide film prepared by the method described above and its application, under the condition of continuous natural light / ultraviolet irradiation, the oxide film formed on the surface of the sample can quickly degrade the oil and other organic pollutants on the surface.
[0010] In the above technical solution, preferably, the anodic oxidation treatment adopts a constant current method, and the anodic oxidation current is preferably 3A / dm 2 , the anodizing time is 30min.
[0011] In the above technical solution, preferably, the vacuum annealing treatment is carried out at a holding temperature of 500°C, a holding time of 60 minutes, and a vacuum degree of 10 -2 Pa.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] The present invention adopts anodizing and vacuum annealing method to prepare anatase structure TiO on the surface of pure titanium 2 The anti-pollution oxide film is anodized under oxygen-rich conditions to avoid the formation of oxygen-deficient oxides due to insufficient oxygen and improve the stoichiometric TiO 2 The preparation method is simple, the cost is low, the service life is long, the carrier concentration is high, it has strong catalytic activity, can quickly degrade various organic pollutants on the surface of the material, and prevent microbial contamination. It has important application prospects in daily life, material self-cleaning and titanium industry. DETAILED DESCRIPTION
[0014] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. The titanium sample in the examples is industrial pure titanium TA1, and is made into a sample with a specification of 100×50×0.6 mm; the chemical reagents are all commercially available analytically pure.
[0015] Example 1
[0016] The method for preparing an anti-pollution oxide film on the surface of pure titanium comprises the following steps:
[0017] ① The titanium samples were polished with 600-mesh, 800-mesh and 1200-mesh sandpapers in turn; the polished titanium samples were then immersed in a solution containing 1% HF and 2% HNO 3 The titanium sample was chemically polished in a solution of 10 s; the polished titanium sample was then ultrasonically cleaned in acetone for 20 min, washed with distilled water for several times, and dried with cold air for later use.
[0018] ②Prepare 0.3% NH 4 F and 2% H 2 O-ethylene glycol mixed electrolyte, and high-purity oxygen with an oxygen concentration of 99% was continuously introduced into the bottom of the electrolyte for 30 minutes before anodization.
[0019] ③ The sample in step ① is subjected to anodization treatment. The oxygen is continuously supplied during the entire anodization process to keep the oxygen content in the electrolyte in a supersaturated state. Ultrasonic waves are used to stir the solution during the anodization process. The ultrasonic frequency is 100KHz. After the anodization is completed, the sample is rinsed with distilled water for multiple times and dried with cold air. The anodization method described in step ③ is constant current anodization; the anodization current is 3A / dm 2The anodizing time is 30 min, so that the pure titanium surface is fully oxidized during the anodizing process.
[0020] ④ Perform vacuum annealing on the sample dried in step ③, with the holding temperature at 500℃ and the vacuum degree ≥10 -2 Pa, the holding time is 60 min, and then cooled to room temperature with the furnace.
[0021] Under 365nm (300W light efficiency) ultraviolet light irradiation, the photocurrent density of the sample was tested, and the test results are shown in Table 1. Organic pollutants are rapidly degraded through photocatalytic oxidation reactions to generate clean CO 2 , H 2 O and other inorganic small molecules, thereby achieving the purpose of anti-pollution.
[0022] Example 2
[0023] The method for preparing an anti-pollution oxide film on the surface of pure titanium comprises the following steps:
[0024] ① The titanium samples were polished with 600-mesh, 800-mesh and 1200-mesh sandpapers in turn; the polished titanium samples were then immersed in a solution containing 1% HF and 2% HNO 3 The titanium sample was chemically polished in a solution of 10 s; the polished titanium sample was then ultrasonically cleaned in acetone for 20 min, washed with distilled water for several times, and dried with cold air for later use.
[0025] ②Prepare 0.3% NH 4 F and 2% H 2 O-ethylene glycol mixed electrolyte, and high-purity oxygen with an oxygen concentration of 99% was continuously introduced into the bottom of the electrolyte for 30 minutes before anodization.
[0026] ③ The sample in step ① is subjected to anodization treatment. The oxygen is continuously supplied during the entire anodization process to keep the oxygen content in the electrolyte in a supersaturated state. Ultrasonic waves are used to stir the solution during the anodization process. The ultrasonic frequency is 100KHz. After the anodization is completed, the sample is rinsed with distilled water for multiple times and dried with cold air. The anodization method described in step ③ is constant current anodization; the anodization current is 3A / dm 2 The anodizing time is 20 min, so that the pure titanium surface is fully oxidized during the anodizing process.
[0027] ④ Perform vacuum annealing on the sample dried in step ③, with the holding temperature at 450℃ and the vacuum degree ≥10 -2 Pa, the holding time is 60 min, and then cooled to room temperature with the furnace.
[0028] Under 365nm (300W light efficiency) ultraviolet light irradiation, the photocurrent density of the sample was tested. The test results are shown in Table 1.
[0029] Table 1 Test results of photocurrent density of samples in the embodiment uv ( / A·m -2 )
[0030]
[0031] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.
Claims
1. Preparation method of anti-pollution oxide film on pure titanium surface, It is characterized in that The method comprises the following steps: ① The titanium sample was polished with 600-mesh, 800-mesh and 1200-mesh sandpapers in turn; then the titanium sample was immersed in a solution containing 1% HF and 2% HNO 3 Chemical polishing treatment is performed in a solution of 5-10s; The polished titanium sample was then ultrasonically cleaned in acetone for 20 min, rinsed with distilled water and dried for later use; ② Prepare the electrolyte, and introduce high-purity oxygen into the bottom of the electrolyte for 10-30 minutes before anodizing, wherein the concentration of the high-purity oxygen is ≥99%; ③ Perform anodizing treatment on the sample in step ①, and keep oxygen flowing throughout the anodizing process so that the oxygen content in the electrolyte is always in a supersaturated state; ultrasonic waves are used to stir the solution during the anodizing process, and the ultrasonic frequency is 50-100kHz; after the anodizing is completed, the sample is rinsed with distilled water for multiple times and dried with cold air; The anodization method is constant current anodization; the anodization current is 3A / dm 2 , anodizing time is 10-30min; ④ Perform vacuum annealing on the sample dried in step ③, with a vacuum degree of ≥10 -2 Pa, the holding time is 30-80min, and then cooled to room temperature with the furnace; The anti-pollution oxide film on the surface of pure titanium prepared by the above method was tested under 365nm ultraviolet light. The photocurrent density of the sample was uv Up to 100A / m 2 .
2. The method for preparing the anti-pollution oxide film on the surface of pure titanium according to claim 1, It is characterized in that The electrolyte described in step ② is 0.3% NH 4 F and 2% H 2 O ethylene glycol mixed electrolyte.
3. The method for preparing the anti-pollution oxide film on the surface of pure titanium according to claim 1, It is characterized in that The vacuum annealing holding temperature in step ④ is 400°C-500°C, and the holding time is 40-60min.
4. An application of an anti-pollution oxide film on the surface of pure titanium prepared by the method as claimed in claim 1.
Citation Information
Patent Citations
Dye wastewater treatment method
CN102424466A
Titanium dioxide nanocomposite and one-step preparation method by utilizing anodic oxidation device
CN102534727A
Method for preparing biomedical titanium and titanium alloy surface antibacterial coatings
CN102758202A
Tungsten oxide substrate with surface reinforced Raman scattering function and preparation method thereof
CN106756853A
Carbon nano tube doped titanium dioxide nanotube photocatalytic material and preparation method thereof
CN109382083A