A LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent and aluminizing method

Through the LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent and the optimized aluminizing method, the problem of uneven distribution of coating components and large thickness changes of the aluminizing agent at high temperatures is solved, achieving uniform aluminum-chromium-silicon coating at high temperatures. Improved performance and corrosion resistance, extending coating life.

CN115627440BActive Publication Date: 2024-10-25CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211295607.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-10-25
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Existing aluminizing agents have defects such as uneven distribution of coating components, large thickness changes, oxidation inclusions and cracks at high temperatures, and are prone to environmental pollution, making it difficult to effectively improve the high-temperature oxidation resistance and corrosion resistance of metals.

Method used

LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent is used. Through the mixing and heat treatment of component A and component B, a multi-layer structural coating is formed. The aluminizing method is optimized to improve the uniformity and thickness stability of the coating, and Heat treatment is performed under an inert atmosphere to reduce oxidative inclusions.

Benefits of technology

It achieves the refinement and uniformity of composition distribution of the coating, reduces the risk of oxidation and corrosion at high temperatures, improves the high-temperature oxidation and corrosion resistance of the aluminum-chromium-silicon coating, extends the life of the coating, and reduces The occurrence of localized corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115627440B_ABST
    Figure CN115627440B_ABST
Patent Text Reader

Abstract

The present invention discloses a LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent and an aluminizing method. The LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent comprises, by mass fraction, 50-71% of Al2O3, 17-22% of Al, 1.1-4.5% of Cr, 8-16% of Si, 2-6% of LaB6 and 1.2-1.5% of NH4Cl. The present invention uses LaB6 as a reinforcing agent to refine the grains of the aluminized layer and evenly distribute the components; at the same time, the aluminizing method is optimized, and the problems of large variations in the components and thickness of the coating prepared by the traditional aluminizing agent, oxide inclusions, etc. are improved, thereby reducing the formation probability of pitting and stress corrosion, preventing the uniform passivation film on the surface from being destroyed at high temperature, inhibiting the occurrence of local corrosion to a certain extent, enhancing the high-temperature oxidation resistance, corrosion resistance and foreign body intrusion resistance of the aluminum-chromium-silicon coating, and improving the coating efficiency and life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface treatment, and in particular relates to a LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent and an aluminizing method. Background Art

[0002] With the rapid development of science and technology, more and more extreme and complex application scenarios have emerged in the fields of aerospace, national defense and military industry, which puts more stringent requirements on the comprehensive performance of materials. The turbine blades of aerospace engines work in a high temperature environment above 1000°C for a long time, and at the same time withstand the high centripetal force caused by high-speed rotation. This requires the blade material to have excellent high-temperature mechanical properties, high-temperature oxidation resistance and corrosion resistance. In addition to optimizing the alloy composition, preparation process and cooling process of the material, we also need further protection measures.

[0003] Oxidation and corrosion of metals at high temperatures are the main factors that cause their performance to deteriorate, so surface treatment can significantly increase the working temperature and extend the working time. At present, how to prepare coatings that can further improve the mechanical and chemical properties of metals at high temperatures has become a hot topic of common concern for researchers around the world.

[0004] The Al2O3 with excellent stability generated by aluminum at high temperature can protect the metal matrix very well; the discrete SiO2 in the oxide layer can further reduce the oxidation rate and improve the oxidation resistance of the metal; Cr can promote the formation of the Al2O3 layer on the metal surface; the addition of rare earth elements can make the surface particles of the coating smaller, more uniform and denser. Therefore, Al, Si and Cr become common elements of high-temperature oxidation-resistant and corrosion-resistant coatings, and rare earth oxides such as Y2O3, La2O3 and CeO2 can be used for coating modification. At present, the commonly used diffusion methods are: hot dip plating, cold spraying and embedding; diffusion aluminizing agents are in the form of slurry aluminizing agents and solid aluminizing agents. Slurry aluminizing has very high requirements on slurry viscosity and pH, and the product is prone to nodules and local unevenness. The coating produced by solid aluminizing agents has uneven distribution of components, large thickness changes, defects such as oxidation inclusions and cracks, and is easy to pollute the environment. Summary of the invention

[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0007] One of the purposes of the present invention is to provide a LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent, which can make metal parts more resistant to oxidation and corrosion at high temperatures after aluminizing.

[0008] To solve the above technical problems, the present invention provides the following technical solutions: a LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent, which comprises, by mass fraction, 50-71% Al2O3, 17-22% Al, 1.1-4.5% Cr, 8-16% Si, 2-6% LaB6 and 1.2-1.5% NH4Cl.

[0009] As a preferred embodiment of the LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent of the present invention, wherein: the LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent is composed of component A and component B, and the component A is composed of Al2O3, Al, LaB6 and 0.8-1.2% NH4Cl;

[0010] The component B consists of Cr, Si and 0.3-0.4% NH4Cl.

[0011] As a preferred scheme of the LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent of the present invention, wherein: in terms of mass fraction, the component A consists of 62.5% Al2O3, 18% Al, 4% LaB6 and 1.3% NH4Cl; the component B consists of 1.5% Cr, 12.4% Si and 0.3% NH4Cl.

[0012] As a preferred embodiment of the LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent of the present invention, the LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent has a particle size of 2 to 10 μm.

[0013] Another object of the present invention is to provide an aluminizing method, comprising heat treating a metal part and the LaB6 reinforced aluminum-chromium-silicon solid powder aluminizing agent described in any one of the above items in an aluminizing furnace, and cooling after completion.

[0014] As a preferred embodiment of the aluminizing method of the present invention, the heat treatment is carried out in an aluminizing furnace, the heat treatment temperature is 750-800° C., and the heat treatment time is 0.5-1.5 h.

[0015] As a preferred embodiment of the aluminizing method of the present invention, the heat treatment is carried out in an aluminizing furnace under an inert gas atmosphere, and the inert gas is selected from argon, helium or neon.

[0016] As a preferred embodiment of the aluminizing method of the present invention, the flow rate of the inert gas is 1.0 to 2.0 m 3 / h.

[0017] As a preferred embodiment of the aluminizing method of the present invention, the method further comprises pre-treating the metal parts, wherein the pre-treating comprises:

[0018] Use paint to protect non-permeable surfaces;

[0019] The aluminized surface of metal parts is ground and polished until it has a metallic luster, then ultrasonically cleaned and dried.

[0020] As a preferred solution of the aluminizing method of the present invention, the aluminizing layer obtained by the aluminizing method has a multi-layer structure and has no obvious defects, and has a thickness of 30 to 70 μm.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention uses LaB6 as a reinforcing agent to refine the grains of the diffusion layer and evenly distribute the components; at the same time, it optimizes the aluminum diffusion method, improves the problems of large variations in coating composition and thickness, oxide inclusions, etc. prepared by traditional diffusing agents, thereby reducing the probability of pitting and stress corrosion, preventing the uniform passivation film on the surface from being destroyed at high temperatures, inhibiting the occurrence of local corrosion to a certain extent, enhancing the high-temperature oxidation resistance, corrosion resistance and resistance to foreign invasion of the aluminum-chromium-silicon coating, and improving the coating efficiency and life. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0024] Figure 1 This is a scanning electron microscope image of the aluminizing agent of Example 2 of the present invention.

[0025] Figure 2 The electrochemical test results of Examples 1 to 4 of the present invention are shown in FIG.

[0026] Figure 3 The figures are scanning electron microscope images of the aluminized layer of the nickel-based high-temperature alloy of the present invention; wherein (a) is comparative example 1; (b) is comparative example 2; (c) is embodiment 3; and (d) is embodiment 4.

[0027] Figure 4 The optical microscope images of the aluminum diffusion layer after oxidation of the present invention; wherein, (a) is comparative example 1; (b) is comparative example 2; (c) is embodiment 3; and (d) is embodiment 4. DETAILED DESCRIPTION

[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0029] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0030] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0031] Example 1

[0032] (1) Weigh component A and component B respectively. By mass fraction, component A is Al2O3: 54%, Al: 20%, LaB6: 6% and NH4Cl: 0.9%; component B is Cr: 3.7%, Si: 15% and NH4Cl: 0.4%. Among them, Al2O3, Al, LaB6, NH4Cl, Cr and Si are all powders with a particle size of 2 to 10 μm. Mix components A and B respectively and let them stand, then mix the two in a ball mill for 8 hours.

[0033] (2) Before aluminizing, the non-aluminized surface of the nickel-based high-temperature alloy is treated with a coating for protection, and then the aluminized surface of the nickel-based high-temperature alloy is ground and polished with 360 mesh, 600 mesh, and 1500 mesh sandpaper until it has a metallic luster, then ultrasonically cleaned and allowed to dry naturally.

[0034] (3) At flow rate 1.5m 3 / h argon atmosphere, preheat the aluminizing furnace at 750℃ for 1h.

[0035] (4) Place the above metals and samples in a crucible in an aluminizing furnace and set the crucible under positive pressure and flow rate of 0.6 m / s. 3 / h argon atmosphere, keep warm at 760℃ for 1h, and adjust the argon flow rate to 1.4m 3 / h, cool down to 80℃ with the furnace and then take out of the furnace for air cooling.

[0036] After testing, the aluminized layer has a continuous and uniform structure, a thickness of about 51μm, a hardness of 336HV, which is 39% higher than the substrate hardness of 241HV, and a corrosion potential of -1.55V. After high-temperature oxidation treatment, the coating morphology has no obvious change.

[0037] Example 2

[0038] (1) Weigh component A and component B respectively. By mass fraction, component A is Al2O3: 57%, Al: 20%, LaB6: 5% and NH4Cl: 0.9%; component B is Cr: 2.8%, Si: 14% and NH4Cl: 0.3%; wherein Al2O3, Al, LaB6, NH4Cl, Cr and Si are all powders with a particle size of 2 to 10 μm; mix components A and B respectively and let them stand, then mix the two in a ball mill for 8 h.

[0039] (2) Before aluminizing, the non-aluminized surface of the nickel-based high-temperature alloy is treated with a coating for protection, and then the aluminized surface of the nickel-based high-temperature alloy is ground and polished with 360 mesh, 600 mesh, and 1500 mesh sandpaper until it has a metallic luster, then ultrasonically cleaned and allowed to dry naturally.

[0040] (3) At flow rate 1.5m 3 / h argon atmosphere, preheat the aluminizing furnace at 760℃ for 1h.

[0041] (4) Place the above metals and samples in a crucible in an aluminizing furnace and set the crucible under positive pressure and flow rate of 0.6 m / s. 3 / h argon atmosphere, keep warm at 780℃ for 0.5h, and adjust the argon flow rate to 1.3m 3 / h, cool down to 80℃ with the furnace and then take out of the furnace for air cooling.

[0042] Figure 1 This is a scanning electron microscope image of the aluminizing agent of Example 2 of the present invention. Figure 1 It can be seen that the particle size of the aluminizing agent is between 2 and 10 microns, with irregular shapes and certain agglomeration.

[0043] After testing, the aluminized layer has a continuous and uniform structure, a thickness of about 49μm, a hardness of 339HV, which is 41% higher than the substrate hardness of 241HV, and a corrosion potential of -1.52V. After high-temperature oxidation treatment, the coating morphology has no obvious change.

[0044] Example 3

[0045] (1) Weigh component A and component B respectively. By mass fraction, component A is Al2O3: 62.5%, Al: 18%, LaB6 powder: 4% and NH4Cl: 1.2%; component B is Cr: 1.5%, Si: 12.4% and NH4Cl: 0.3%. Among them, Al2O3, Al, LaB6, NH4Cl, Cr and Si are all powders with a particle size of 2 to 10 μm. Mix components A and B respectively and let them stand, then mix the two in a ball mill for 8 hours.

[0046] (2) Before aluminizing, the non-aluminized surface of the nickel-based high-temperature alloy is treated with a coating for protection, and then the aluminized surface of the nickel-based high-temperature alloy is ground and polished with 360 mesh, 600 mesh, and 1500 mesh sandpaper until it has a metallic luster, then ultrasonically cleaned and allowed to dry naturally.

[0047] (3) At flow rate 1.5m 3 / h argon atmosphere, preheat the aluminizing furnace at 750℃ for 1h.

[0048] (4) Place the above metals and samples in a crucible in an aluminizing furnace and set the crucible under positive pressure and flow rate of 0.6 m / s. 3 / h argon atmosphere, keep warm at 790℃ for 1.2h, and adjust the argon flow rate to 1.4m 3 / h, cool down to 80℃ with the furnace and then take out of the furnace for air cooling.

[0049] After testing, the aluminized layer was found to be continuous and uniform in structure, with a thickness of about 52μm and a hardness of 357HV, which was 48% higher than the substrate hardness of 241HV. The corrosion potential was -1.44V, and there was no significant change in the coating morphology after high-temperature oxidation treatment.

[0050] Example 4

[0051] (1) Weigh component A and component B respectively. By mass fraction, component A is Al2O3: 62%, Al: 22%, LaB6: 3% and NH4Cl: 1.0%; component B is Cr: 1.6%, Si: 10.2% and NH4Cl: 0.3%; wherein Al2O3, Al, LaB6, NH4Cl, Cr and Si are all powders with a particle size of 2 to 10 μm; mix components A and B respectively and let them stand, then mix the two components in a ball mill for 8 h.

[0052] (2) Before aluminizing, the non-aluminized surface of the nickel-based high-temperature alloy is treated with a coating for protection, and then the aluminized surface of the nickel-based high-temperature alloy is ground and polished with 360 mesh, 600 mesh, and 1500 mesh sandpaper until it has a metallic luster, then ultrasonically cleaned and allowed to dry naturally.

[0053] (3) At flow rate 1.5m 3 / h argon atmosphere, preheat the aluminizing furnace at 760℃ for 1.5h.

[0054] (4) Place the above metals and samples in a crucible in an aluminizing furnace and set the crucible under positive pressure and flow rate of 0.7 m / s. 3 / h argon atmosphere, keep warm at 800℃ for 1h, and adjust the argon flow rate to 1.3m 3 / h, cool down to 80℃ with the furnace and then take out of the furnace for air cooling.

[0055] After testing, the aluminized layer was found to be continuous and uniform in structure, with a thickness of about 54 μm and a hardness of 354 HV, which was 47% higher than the substrate hardness of 241 HV. The corrosion potential was -1.49 V, and there was no significant change in the coating morphology after high-temperature oxidation treatment.

[0056] Figure 2 Figures 1#, 2#, 3#, and 4# are the electrochemical test results of Examples 1 to 4 of the present invention. Figure 2 It can be seen that the corrosion potentials of the four embodiments are -1.55, -1.52, -1.44, and -1.49 V, respectively, and the sample in Embodiment 1 has the best corrosion performance.

[0057] Comparative Example 1

[0058] (1) Weigh component A and component B respectively. By mass fraction, component A is Al2O3: 65% and Al: 22%; component B is Cr: 2% and Si: 11%; wherein Al2O3, Al, Cr, and Si are all powders with a particle size of 2 to 10 μm; mix components A and B respectively and let them stand, then mix the two components in a ball mill for 8 h.

[0059] (2) Before aluminizing, the non-aluminized surface of the nickel-based high-temperature alloy is treated with a coating for protection, and then the aluminized surface of the nickel-based high-temperature alloy is ground and polished with 360 mesh, 600 mesh, and 1500 mesh sandpaper until it has a metallic luster, then ultrasonically cleaned and allowed to dry naturally.

[0060] (3) At flow rate 1.5m 3 / h argon atmosphere, preheat the aluminizing furnace at 750℃ for 1.5h.

[0061] (4) The above metals and samples are placed in a crucible in an aluminizing furnace. The instrument is operated at a positive pressure and a flow rate of 0.7 m / s. 3 / h argon atmosphere, keep warm at 750℃ for 1h, and adjust the argon flow rate to 1.3m 3 / h, cool down to 80℃ with the furnace and then take out of the furnace for air cooling.

[0062] After testing, the coating thickness was about 28μm, the hardness was 302HV, there were cracks inside, and without the active agent NH4Cl and the reinforcing agent LaB6, the density of the coating and the degree of coverage of the substrate were not ideal. After a period of high-temperature oxidation treatment, the outer curve of the coating showed obvious fluctuations, and the temperature change and oxygen erosion caused the coating to peel off.

[0063] Comparative Example 2

[0064] (1) Weigh component A and component B respectively. By mass fraction, component A is Al2O3: 64%, Al: 21.8% and NH4Cl: 0.8%; component B is Cr: 2%, Si: 11% and NH4Cl: 0.4%; wherein Al2O3, Al, NH4Cl, Cr and Si are all powders with a particle size of 2 to 10 μm; mix components A and B respectively and let them stand, then mix the two components in a ball mill for 8 h.

[0065] (2) Before aluminizing, the non-aluminized surface of the nickel-based high-temperature alloy is treated with a coating for protection, and then the aluminized surface of the nickel-based high-temperature alloy is ground and polished with 360 mesh, 600 mesh, and 1500 mesh sandpaper until it has a metallic luster, then ultrasonically cleaned and allowed to dry naturally.

[0066] (3) At flow rate 1.5m 3 / h argon atmosphere, preheat the aluminizing furnace at 760℃ for 1.5h.

[0067] (4) The above metals and samples are placed in a crucible in an aluminizing furnace. The instrument is operated at a positive pressure and a flow rate of 0.7 m / s. 3 / h argon atmosphere, keep warm at 800℃ for 1h, and adjust the argon flow rate to 1.3m 3 / h, cool down to 80℃ with the furnace and then take out of the furnace for air cooling.

[0068] After testing, the coating thickness is in the range of 20 to 33 μm, the hardness is 294 HV, and the coating becomes denser after adding the activator NH4Cl, but the thickness distribution is not uniform. After a period of high-temperature oxidation treatment, similar to Example 1, the coating undergoes obvious changes and peeling.

[0069] Figure 3 a, b, c, d are scanning electron microscope images of the aluminized layer of the nickel-based high-temperature alloy of the present invention, respectively. Figure 3 It can be seen that the coating area, diffusion area, and matrix area have obviously different morphologies. The diffusion area is flat and has a large number of white spots evenly distributed. The coating density of Comparative Example 1 in Figure a is poor and there are a large number of cracks. The coating thickness distribution of Comparative Example 2 in Figure b is uneven. From Figures c and d, it can be seen that the coating morphology of Examples 3 and 4 prepared by the formula and process of this patent has changed, the organization is uniform and dense, and the coating thickness and diffusion layer thickness are increased compared with Comparative Examples 1 and 2.

[0070] Figure 4 a, b, c, d are optical micrographs of the aluminized layer after high temperature oxidation treatment in Comparative Example 1, Comparative Example 2, Example 3, and Example 4 of the present invention. Figure 4It can be seen that the coatings of Comparative Examples 1 and 2 changed significantly, the outermost curves fluctuated, and peeling occurred, while the coatings of Examples 3 and 4 were relatively stable, no local corrosion occurred, and had better thermal shock resistance and oxidation resistance.

[0071] The aluminum-chromium-silicon solid powder aluminizing agent prepared by the present invention uses LaB6 as a reinforcing agent, which can refine the grains of the infiltration layer and evenly distribute the components, not only improving the mechanical properties of the coating; it also improves the problems of large changes in the composition and thickness of the coating prepared by the traditional infiltration agent in the past, oxide inclusions, and reduces the defects of the coating, thereby reducing the formation probability of pitting and stress corrosion, preventing the uniform passivation film on the surface from being destroyed at high temperature, and inhibiting the occurrence of local corrosion to a certain extent. Moreover, LaB6 can absorb oxygen and be converted into La2O3 in a high-temperature oxygen atmosphere. Most of the La in the infiltration layer exists at the Al2O3 grain boundary. The change in the growth mechanism of the oxide film can reduce the diffusion rate of Al ions, thereby enhancing the high-temperature stability and sulfur and oxygen corrosion resistance of the aluminum-chromium-silicon coating. NH4Cl is used as an activator, which will be thermally decomposed during the aluminizing process and converted into a small amount of gas to escape, and will not introduce impurities into the system.

[0072] In summary, it can not only be applied to aircraft engine turbine blades, but can also be extended to various turbine components such as main shafts, impellers, and guide wheels.

[0073] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A LaB 6 Reinforced aluminum-chromium-silicon solid powder aluminizing agent, Features: The LaB 6 The reinforced aluminum-chromium-silicon solid powder aluminizing agent is composed of component A and component B; In terms of mass fraction, the component A is composed of 50-71% Al 2 O 3 , 17~22% Al, 2~6% LaB 6 and 0.8~1.2% NH 4 Cl composition; The component B is composed of 1.1-4.5% Cr, 8-16% Si and 0.3-0.4% NH 4 Cl composition.

2. LaB according to claim 1 6 Reinforced aluminum-chromium-silicon solid powder aluminizing agent, Features: In terms of mass fraction, the component A is composed of 62.5% Al 2 O 3 , 18% Al, 4% LaB 6 and 1.3% NH 4 Cl; the component B consists of 1.5% Cr, 12.4% Si and 0.3% NH 4 Cl composition.

3. LaB according to any one of claims 1 to 2 6 Reinforced aluminum-chromium-silicon solid powder aluminizing agent, Features: The LaB 6 The reinforced aluminum-chromium-silicon solid powder aluminizing agent has a particle size of 2 to 10 μm.

4. A method for aluminizing, Features: include, A metal component and the LaB according to any one of claims 1 to 3 6 The reinforced aluminum-chromium-silicon solid powder aluminizing agent is heat treated in an aluminizing furnace and then cooled.

5. Aluminizing method according to claim 4, Features: The heat treatment is carried out in an aluminizing furnace, the heat treatment temperature is 750-800° C., and the heat treatment time is 0.5-1.5 h.

6. Aluminizing method according to claim 4 or 5, Features: The heat treatment is carried out in an aluminizing furnace under an inert gas atmosphere, and the inert gas is selected from argon, helium or neon.

7. Aluminizing method according to claim 6, Features: The flow rate of the inert gas is 1.0~2.0m 3 / h.

8. The aluminizing method according to any one of claims 4, 5 and 7, Features: The metal parts are pre-processed, and the pre-processing includes: Use paint to protect non-permeable surfaces; The aluminized surface of metal parts is ground and polished until it has a metallic luster, then ultrasonically cleaned and dried.

9. Aluminizing method according to claim 8, Features: The aluminized layer obtained by the aluminizing method has a multi-layer structure and has no obvious defects, and has a thickness of 30-70 μm.