A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn2O4

Through the leaching precipitation method, Mn and Li are recovered from waste lithium-ion batteries, and spinel LiMn2O4 positive electrode material is synthesized, which solves the problems of low lithium recycling efficiency and great environmental impact in the existing lithium-ion battery recycling technology, and achieves high efficiency and low cost Lithium-ion battery resource recycling and new energy vehicle battery materials are provided.

CN115637328BActive Publication Date: 2024-11-05ANHUI GREATPOWER LITHIUM BATTERY CYCLE TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202211365941.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-02
Publication Date
2024-11-05
Estimated Expiration
2042-11-02

Smart Images

  • Figure CN115637328B_ABST
    Figure CN115637328B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing LiMn2O4 by recycling waste zinc-carbon and lithium-ion batteries, comprising the following steps: recycling different waste batteries by leaching precipitation method to obtain Mn2O3 and Li2CO3, mixing the two in a certain proportion by solid-state synthesis method under certain temperature and conditions, and then reacting to generate LiMn2O4 positive electrode material. The present invention provides a method for preparing LiMn2O4 by recycling waste zinc-carbon and lithium-ion batteries, the synthesized product has good electrochemical properties and complete crystal faces, and the method has simple process and short flow, and provides a new route and method for recycling raw materials in waste batteries to prepare positive electrode LiMn2O4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of waste battery recycling, and in particular to a method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn 2 O 4 method. Background Art

[0002] Based on the urgent need for sustainable development and safety of energy, and to reduce dependence on traditional energy and pollutant emissions, new energy vehicles have become a strategic emerging industry. As the country increases its support for the new energy vehicle industry, global sales of new energy vehicles continue to rise. Lithium-ion batteries are one of the core components of new energy vehicles. They have the characteristics of large capacity and high energy density, and are the focus of affecting the performance and cost of new energy vehicles. However, the cycle life of lithium-ion batteries is limited. It is estimated that the amount of lithium-ion batteries scrapped in my country will reach 350,000 tons in 2025, and a new peak of lithium-ion battery scrapping will be ushered in in the future. Lithium-ion batteries contain a large amount of precious metals and are a valuable mineral resource. Recycling them is of great significance and value to environmental protection and solving resource scarcity.

[0003] Common lithium ion recovery technologies include pyrometallurgy, hydrometallurgy, biometallurgy and other technologies. The advantages of the pyrometallurgical recovery process are that the path is short and easy to expand, and it can be applied to the recycling of waste lithium-ion batteries mixed with various materials. However, the main disadvantage of the pyrometallurgical recovery process is that it cannot effectively recover lithium, and lithium usually exists in the form of slag in combination with other metals; the biological recovery of metals from waste lithium-ion batteries is still in its infancy, and low selectivity and low efficiency are the biggest problems currently; the hydrometallurgical process is currently the most widely used technology in the metallurgical industry due to its advantages of high metal leaching rate and high purity. The process has low cost, low energy consumption, and good results.

[0004] At present, there have been many reports on the recycling of waste batteries or the further preparation of positive electrode materials. For example, the invention patent with Chinese patent publication number CN112174214A discloses a lithium battery LiMn 2 O 4 The invention discloses a method for preparing positive electrode materials, which uses a sol-gel method to prepare positive electrode materials with high crystallinity and complete structure by step-by-step heating. Compared with this method, the Mn and Li raw materials of the invention are all derived from the recycling of waste batteries, which is environmentally friendly and conducive to solving the problem of resource scarcity. 2 MnO was obtained by crushing the waste batteries, leaching with acid, adding excess ammonium sulfate, adjusting the pH, and centrifuging. 2The ammonium sulfate used in the precipitation process is harmful to the human body to a certain extent, and the pH needs to be controlled during the process. Compared with this method, the sulfuric acid concentration involved in the process of the present invention is low, the amount used is small, there is no danger, and the process operation is simple. The invention patent with Chinese patent publication number CN106784793A discloses a method for preparing a ternary material positive electrode material. The concentration of each metal ion is adjusted by acid leaching and impurity removal of waste batteries, and a complexing agent is added to generate a ternary positive electrode material precursor with different metal ratios. Compared with this method, this method only precipitates Mn and Li, does not involve impurity removal, and can be directly used as a precursor of the positive electrode material. Fewer reagents are used, which is more conducive to cost control and environmental protection. Summary of the invention

[0005] In view of the prior art, the present invention provides a method for recovering Mn and Li from waste batteries by leaching and precipitation method, and the recovery process forms a metal compound form, which can be directly reacted and regenerated to prepare the next generation of spinel LiMn 2 O 4 The process is simple to operate, has a short process route, and the recovered metal substances can be directly used as LiMn without pretreatment. 2 O 4 Preparation of raw materials.

[0006] A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn 2 O 4 The method comprises the following steps:

[0007] 1). First, the battery slurry recovered from the waste batteries is separated and then the batteries are cut and disassembled;

[0008] 2). Leach the battery slurry with a mixture solution of 2 mol sulfuric acid and glucose;

[0009] 3). Then potassium permanganate is added to the solution as an oxidant to selectively oxidize and precipitate Mn 2+ Get MnO 2 precipitation;

[0010] 4). After the reaction is complete, filter and the residue is MnO 2 ;

[0011] 5). The obtained MnO 2 Heating makes MnO 2 Converted to Mn 2 O 3 , to obtain a manganese source which is further used in solid-state synthesis;

[0012] 6). The selective recovery step of Li is to first soak the waste battery fragments in a 2.5 mol / L NaOH solution at room temperature for 2 hours to dissolve them;

[0013] 7). Then add 1 mol / L oxalic acid solution at 70°C for leaching reaction for 2 hours to form lithium oxalate, and then heat the solution to evaporate and crystallize to precipitate oxalate from the solution;

[0014] 8). The obtained precipitate is collected by filtration and dried, and the lithium oxalate salt is further decomposed at a certain temperature to obtain lithium carbonate;

[0015] 9). MnO 2 or Mn 2 O 3 and C from spent lithium-ion batteries 2 H 2 O 4 ·H 2 O or Li 2 CO 3 Synthetic spinel LiMn 2 O 4 Positive electrode material: the raw materials were fully mixed and ball-milled in a ball mill at a speed of 200 rpm for 10 minutes, then placed in a crucible and heated in a muffle furnace to obtain LiMn 2 O 4 Positive electrode material.

[0016] The concentration of glucose used in step 2) is 2 g / L. The slurry density is ≤2%.

[0017] Potassium permanganate and Mn in step 3) 2+ The dosage ratio is 1:1-3.

[0018] The heating temperature and heating time in step 5) are 600°C for 5 hours.

[0019] The concentration of the NaOH solution used in step 6) is 2.5 mol / L.

[0020] The concentration of the oxalic acid solution in step 7) is 1 mol / L.

[0021] In step 8), the lithium oxalate salt is further decomposed at a temperature of 600° C. for 5 hours.

[0022] Step 9) LiMn 2 O 4 The synthesis reaction temperature is 850°C.

[0023] Step 9) LiMn 2 O 4 The synthesis reaction temperature is 850°C and the time is 10 hours.

[0024] In step 9), the molar ratio of the lithium source to the manganese source is 1.1:2.

[0025] MnO 2 and C 2 H 2 O 4 ·H 2 O Synthetic spinel LiMn 2 O 4 The equation for the positive electrode material is:

[0026] 4MnO 2 + C 2 H 2 O 4 ·H 2 O + 1 / 4O 2 = 2LiMn 2 O 4 + 2CO 2 +3 / 2H 2 O

[0027] Mn 2 O 3 and C 2 H 2 O 4 ·H 2 O Synthetic spinel LiMn 2 O 4 The equation for the positive electrode material is:

[0028] 4Mn 2 O 3 + 2C 2 H 2 O 4 ·H 2 O + 5 / 2O 2 = 4LiMn 2 O 4 + 4CO 2 + 3H 2 O

[0029] MnO 2 and Li 2 CO 3 Synthetic spinel LiMn 2 O 4 The equation for the positive electrode material is:

[0030] 4MnO 2 + Li 2 CO 3 = 2LiMn 2 O 4 + 1CO 2 +1 / 2O 2

[0031] Mn 2 O 3 and Li 2 CO 3 Synthetic spinel LiMn 2 O 4 The equation for the positive electrode material is:

[0032] 2Mn 2 O 3 + Li 2 CO 3 +1 / 2O 2 = 2LiMn 2 O 4 + CO 2

[0033] The present invention recovers Mn and Li from waste batteries by leaching and precipitation method, and further reacts the LiMn obtained under the reaction conditions of 850°C and 10h. 2 O 4 The positive electrode material exhibits good electrochemical properties, the discharge capacity under the synthesis conditions is the best, and it has high charge and discharge capabilities and service life, providing a promising prospect for the valuable materials recovered from various scrapped batteries for the production of high-demand lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Prepare a flow chart for the recycling of waste zinc-carbon and lithium batteries;

[0035] Figure 2 Mn 2 O 3 and Li 2 CO 3 Synthesized LiMn at different calcination times 2 O 4 XRD pattern of

[0036] Figure 3 LiMn synthesized for 10 hours 2 O 4 Cycling performance of cathode materials;

[0037] Figure 4 LiMn 2 O 4 Discharge curves of cathode materials at different rates;

[0038] Figure 5 LiMn synthesized under different manganese sources 2 O 4 Cathode material;

[0039] Figure 6 To synthesize Mn at different temperatures2 O 3 XRD pattern of

[0040] Figure 7 :(a) Mn synthesized at 700℃ 2 O 3 (b) Mn synthesized at 800℃ 2 O 3 Preparation of LiMn 2 O 4 XRD pattern of the positive electrode material. DETAILED DESCRIPTION

[0041] The content of the present invention is further described below in conjunction with the drawings and embodiments, but is not intended to limit the present invention. Example

[0042] A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn 2 O 4 The method comprises the following steps:

[0043] 1). First, the battery slurry recovered from the waste batteries is separated and then the batteries are cut and disassembled;

[0044] 2). Leach the battery slurry with a mixture of 2 mol sulfuric acid and glucose, the concentration of glucose used in step 2) is 2 g / L. The slurry density is ≤2%;

[0045] 3). Then potassium permanganate is added to the solution as an oxidant to selectively oxidize and precipitate Mn 2+ Get MnO 2 Precipitation (potassium permanganate and Mn 2+ The molar ratio of the substances is 1:2);

[0046] 4). After the reaction is complete, filter and the residue is MnO 2 ;

[0047] 5). The MnO obtained above 2 Heating at 600℃ for 5 hours makes MnO 2 Converted to Mn 2 O 3 , obtaining a manganese source that is further used in solid-state synthesis.

[0048] 6). The selective recovery step of Li is to first soak the waste battery fragments in a 2.5 mol / L NaOH solution at room temperature for 2 hours to dissolve them. The concentration of the NaOH solution used in step 6) is 2.5 mol / L.

[0049] 7). Then, 1 mol / L oxalic acid solution is added at 70°C for leaching reaction for 2 hours to form lithium oxalate, and then the solution is heated for evaporation and crystallization to precipitate oxalate from the solution. The concentration of the oxalic acid solution in step 7) is 1 mol / L.

[0050] 8) The resulting precipitate was collected by filtration and dried, and lithium hydrogen oxalate was further decomposed at 600°C for 5 hours to obtain Li 2 CO 3 .

[0051] 9). Raw material Mn 2 O 3 and Li 2 CO 3 The raw materials were fully mixed and ball-milled in a ball mill at 200 rpm for 10 minutes, then placed in a crucible and heated at 850°C in a muffle furnace for 10 hours to obtain LiMn 2 O 4 Positive electrode material. Example

[0052] A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn 2 O 4 The method comprises the following steps:

[0053] Steps 1) to 7) are the same as those in Example 1, except that in step 8) lithium hydrogen oxalate is directly used as the catalyst for reacting with Mn 2 O 3 The raw materials of the reaction are not further dried to generate Li 2 CO 3 ,

[0054] 9). The reaction results show that lithium hydrogen oxalate and Mn 2 O 3 There is a part of MnO in the synthetic product of the reaction 2 and Mn 2 O 3 , indicating that lithium hydrogen oxalate as a lithium source does not react completely during the synthesis process, indicating that Li 2 CO 3 Reacts as a lithium source.

[0055] Comparative Example 1

[0056] A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn 2 O 4 The method is different in that LiMn is synthesized 2 O 4 Use of MnO 2 Rather than Mn 2 O3 ,

[0057] The LiMn prepared in this comparative example 2 O 4 The XRD patterns of the positive electrode materials and the examples are shown in Table 1. Figure 5 As shown, it shows that Mn 2 O 3 As one of the reactants, the product shows a slightly sharp peak, which enhances the crystallinity, indicating that Mn 2 O 3 is a more favorable reactant.

[0058] Comparative Example 2

[0059] A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn 2 O 4 The method is different in that LiMn is synthesized 2 O 4 The heating reaction time of the muffle furnace is 8h.

[0060] The LiMn prepared in this comparative example 2 O 4 The XRD patterns of the positive electrode materials and the examples are shown in Table 1. Figure 2 As shown, compared with the characteristic peaks of the product synthesized under the conditions of 10 hours in Example 1, the diffraction peaks of the product synthesized after 10 hours of reaction are higher, indicating that the crystallinity is stronger, the crystal surface growth will be more complete, and it is easier to achieve ideal electrochemical behavior.

[0061] Comparative Example 3

[0062] A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn 2 O 4 The difference is that the reactant Mn 2 O 3 The synthesis temperature is different, and the synthesis temperature is 700℃.

[0063] Figure 6-Figure 7 It shows that Mn synthesized at 700℃ 2 O 3 and Li 2 CO 3 , only LiMn exists in the product XRD pattern 2 O 4 The characteristic peaks of 2 O 4 The product has complete crystal form and no other side reaction products.

[0064] Comparative Example 4

[0065] A method for recycling waste zinc-carbon and lithium-ion batteries to prepare LiMn2 O 4 The difference is that the reactant Mn 2 O 3 The synthesis temperature is different, and the synthesis temperature is 800℃.

[0066] Figure 6-Figure 7 It shows that Mn will be produced at a synthesis temperature of 800℃ 3 O 4 , which is not conducive to further reaction. The presence of some manganese compounds in the product indicates that the reaction is incomplete at 800℃. Therefore, the Mn synthesized at 700℃ 2 O 3 It is more suitable as raw material for synthetic positive electrode materials.

[0067] The above embodiments are only used to explain the inventive concept of the present invention, rather than to limit the protection of the rights of the present invention. Any non-substantial changes to the present invention using this concept shall fall within the protection scope of the present invention.

Claims

1. A method for preparing LiMn2O4 by recycling waste zinc-carbon and lithium-ion batteries, characterized in that: The following steps are involved: 1). First, the battery slurry recovered from the waste batteries is separated and then the batteries are cut and disassembled; 2). Leach the battery slurry with a mixture of 2 mol sulfuric acid and glucose, with a glucose concentration of 2 g / L; 3). Then potassium permanganate is added to the solution as an oxidant to selectively oxidize and precipitate Mn 2+ MnO2 precipitation is obtained; potassium permanganate and Mn 2+ The ratio of the amount of substance is 1:1-3; 4). After the reaction is complete, filter and the filter residue is MnO2; 5). The obtained MnO2 was heated at 600°C for 5 hours to convert MnO2 into Mn2O3, thereby obtaining a manganese source which was further used in solid-state synthesis; 6) The selective recovery step of Li is to first soak the waste battery fragments in a 2.5 mol / L NaOH solution at room temperature for 2 hours to dissolve them; 7). Then add 1 mol / L oxalic acid solution at 70°C for leaching reaction for 2 hours to form lithium oxalate, then heat the solution and evaporate and crystallize to precipitate oxalate from the solution; 8). The resulting precipitate was collected by filtration and dried, and the oxalate was further decomposed at 600°C for 5 hours to obtain Li2CO3; 9). Mn2O3 and Li2CO3 were mixed in a molar ratio of 2:1.1 to synthesize spinel LiMn2O4 positive electrode material: the raw materials were fully mixed and ball-milled in a ball mill at 200 rpm for 10 minutes, then put into a crucible and heated at 850°C in a muffle furnace for 10 hours to obtain LiMn2O4 positive electrode material.

Citation Information

Patent Citations

  • Method for preparing sigma and gamma-MnO2 from lithium ion battery anode wastes

    CN106517343A

  • Preparation method of lithium ion battery ternary cathode material

    CN106784793A

  • Preparation method of lithium battery LiMn2O4 positive electrode material

    CN112174214A

  • Leaching method for anode and cathode mixed materials of waste LiCoxNiyMnzO2 battery

    CN101586192A

  • Method for preparing ternary material precursor and recovering lithium by using spent lithium-ion battery ternary cathode materials