Aluminum sacrificial anode alloy and preparation method thereof

By adding specific proportions of Zn, Si, Sn and In elements to the aluminum alloy and performing a long-term annealing treatment to form the Al9Fe2Si phase, the problem of the existing aluminum alloy anode generating a passivation film in a Cl- environment is solved and the efficiency is improved. current efficiency and performance, extending service life.

CN115637434BActive Publication Date: 2024-10-01CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211285092.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-20
Publication Date
2024-10-01
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing aluminum alloy sacrificial anode alloys are prone to generate passivation films in Cl- environments, reducing performance, and corrosion products are difficult to fall off, resulting in low current efficiency and poor performance.

Method used

By adding alloy elements such as Zn, Si, Sn and In to aluminum, the composition is Zn: 0.5-5%, Si: 2-10%, Sn: 0.1-3%, In: 0.01-0.2%, Fe element The aluminum alloy reaches the saturated state and is annealed for a long time to form the Al9Fe2Si phase to improve current efficiency and performance.

Benefits of technology

Through component optimization and annealing treatment, the aluminum alloy electrode potential is reduced, the current efficiency and sacrificial anode performance are improved, the formation of passivation film and the adhesion of corrosion products are significantly reduced, and the service life of the alloy is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003899461240000011
    Figure HDA0003899461240000011
  • Figure HDA0003899461240000012
    Figure HDA0003899461240000012
  • Figure HDA0003899461240000013
    Figure HDA0003899461240000013
Patent Text Reader

Abstract

The present invention relates to the field of aluminum anode sacrificial alloys, and specifically discloses an aluminum sacrificial anode alloy and a preparation method thereof. The aluminum sacrificial anode alloy comprises, by mass percentage, alloy elements of Zn: 0.5-5%, Si: 2-10%, Sn: 0.1-3%, In: 0.01-0.2%, and the rest are Al and inevitable impurities (Fe element reaches saturation state). The preparation method thereof is: firstly melting an aluminum ingot, then adding Al-Zn master alloy, Al-Si master alloy, Al-Sn master alloy, Al-In master alloy, casting to form a casting billet after refining and degassing and deslagging, and then annealing the anode alloy for a long time to obtain an Al9Fe2Si phase, the appearance of which can reduce the electrode potential of the aluminum sacrificial anode alloy, while improving the current efficiency of the aluminum alloy and the sacrificial anode performance, and the corrosion product is easier to fall off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum anode sacrificial alloys, and specifically discloses an aluminum sacrificial anode alloy and a preparation method thereof. Background Art

[0002] Zinc-based alloys have good sacrificial properties and are the best choice for sacrificial anode alloys. However, the average content of zinc in the earth's crust is only 0.004%, and its reserves are only enough for 22 years. Therefore, it is crucial to develop an alloy with high current efficiency and good sacrificial properties, and the most promising sacrificial material to replace zinc is aluminum. Compared with magnesium-based and zinc-based alloys, aluminum alloys have low density, high current efficiency, medium driving potential, and large actual capacitance. They are the most suitable anode materials in the periodic table. However, pure aluminum will form hydrous oxides on its surface in aqueous solution, causing aluminum passivation, so pure aluminum cannot be used as a sacrificial anode material. In order to eliminate the passivation film on the aluminum surface, alloying is usually performed, that is, adding alloying elements such as zinc and indium to aluminum. The basic idea of ​​developing aluminum alloy sacrificial anodes is to change the surface state of aluminum through alloying, limit or prevent the formation of a continuous and dense oxide layer on the surface, and promote surface activation, so that the alloy has a more negative electrode potential and a higher current efficiency to meet its basic requirements as a sacrificial anode.

[0003] In order to improve the performance of aluminum alloy anodes, researchers at home and abroad have developed aluminum alloy anode materials with various component systems. Domestic researchers have also developed ternary, quaternary and more aluminum alloy anode materials. However, the current efficiency of existing ternary and quaternary sacrificial anode alloys is low; pentyl and even multi-component sacrificial anode alloys have low current efficiency in the presence of Cl. - A passive film is quickly generated in the environment. The appearance of the passive film reduces the performance of the sacrificial anode alloy, and the corrosion products of the multi-component sacrificial anode alloy are easily attached to the surface of the alloy and are difficult to fall off. Summary of the invention

[0004] The object of the present invention is to provide a sacrificial anode alloy, which comprises aluminum and alloy elements added to the aluminum. The anode alloy comprises, by mass percentage, Zn: 0.5-5%, Si: 2-10%, Sn: 0.1-3%, In: 0.01-0.2%, and the rest is Al and unavoidable impurities, and the Fe element reaches a saturated state.

[0005] The composition of the anode alloy is preferably as follows according to the mass percentage of the elements: Zn: 0.5-5%, Si: 2-10%, Sn: 1.5-3%, In: 0.05-0.2%, the rest being Al and inevitable impurities, and the Fe element reaches a saturated state.

[0006] The present invention also aims to provide a method for preparing an anode alloy after long-term annealing, the preparation method is simple, and the obtained aluminum sacrificial anode alloy has a high anode utilization rate. The Al9Fe2Si phase can be obtained by long-term annealing. Compared with α-Al, the Al9Fe2Si phase is a cathode phase, and the phase can form more tiny galvanic cells with α-Al. The presence of the galvanic cell can reduce the aluminum alloy electrode potential, while improving the aluminum alloy current efficiency and sacrificial anode performance.

[0007] The steps of preparing the aluminum sacrificial anode alloy are as follows:

[0008] (1) First, the aluminum ingot is melted, and then Al-Zn master alloy, Al-Si master alloy, Al-Sn master alloy, and Al-In master alloy are added. After refining, degassing and deslagging, the ingot is cast to form a casting.

[0009] In an optional implementation manner, after the aluminum ingot is melted, the temperature is raised to 680-800° C., kept warm for 1 hour, and then Al-Zn master alloy, Al-Si master alloy, Al-Sn master alloy and Al-In master alloy are added in sequence.

[0010] After adding the intermediate alloy, continue to heat up to 710-750℃ and keep it for 1-2 hours, and then pour at 710℃.

[0011] (2) The ingot is subjected to a long-term annealing treatment.

[0012] The annealing treatment includes: first homogenization annealing, then long-term product annealing;

[0013] Preferably, the homogenization annealing comprises placing the ingot into a furnace at room temperature, annealing at a heating rate of 18-20°C / min to 400-550°C for 1-10h; after annealing, air cooling to room temperature;

[0014] Preferably, the long-term annealing of the finished product comprises placing the ingot into a furnace at room temperature, heating the ingot to 400-550° C. at a heating rate of 18-20° C. / min, annealing for 50-200 hours, and after annealing, air cooling to room temperature.

[0015] In an optional embodiment, after the homogenization annealing and before the finished product long-term annealing, the slab surface oxide layer is removed. After annealing, the slab is air-cooled to room temperature and then cut into alloy blocks of 10×10×10 mm at room temperature.

[0016] The present invention has the following beneficial effects: in the present invention, the composition of the anode alloy is limited and the annealing treatment is performed for a long time, so as to promote the appearance of the Al9Fe2Si phase. The alloy phase and α-Al form a large number of tiny galvanic cells, and the appearance of the galvanic cells can reduce the electrode potential of the aluminum alloy, improve the current efficiency and the performance of the sacrificial anode.

[0017] In the present invention, Si can improve the fluidity of alloy liquid, reduce the content of oxide impurities in the alloy liquid, and significantly reduce the casting defects of the alloy when used in the sacrificial anode aluminum process; Sn can reduce the resistance of the passivation film on the surface of the aluminum anode, so that pores are generated in the passivation film on the surface of the anode, which is conducive to the shedding of the passivation film; Sn also has a higher hydrogen evolution overpotential and can effectively inhibit the hydrogen evolution reaction; Zn is the most basic activation element in the aluminum alloy anode, and the addition of zinc can make the aluminum anode easy to alloy and the potential negatively shift by 0.1 to 0.3V; a trace amount of In element is also an important activation element of the aluminum-based anode, and exists in the aluminum plating layer in the form of an In-rich segregation phase, which reduces the negative charge, improves the current efficiency of the aluminum-based anode, and effectively improves the anode sacrificial protection ability of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The overall morphology of the Al-1Zn-7Si-3Sn-0.20In alloy in Example 1;

[0019] Figure 2 The overall morphology of the Al-1Zn-7Si-3Sn-0.10In alloy in Example 2;

[0020] Figure 3 The overall morphology of the Al-1Zn-7Si-3Sn-0.05In alloy in Example 3;

[0021] Figure 4 The overall morphology of the Al-1Zn-7Si-3Sn-0.05In alloy in Example 4;

[0022] Figure 5 The overall morphology of the Al-4Zn-7Si-1Sn-0.15In alloy in Example 5;

[0023] Figure 6 The overall morphology of the Al-1Zn-7Si-0.5Sn-0.20In alloy in Example 6;

[0024] Figure 7 The overall morphology of the Al-1Zn-7Si-3Sn-0.20In alloy in Comparative Example 1;

[0025] Figure 8 The overall morphology of the Al-1Zn-7Si-3Sn-0.05In alloy in Comparative Example 2;

[0026] Fig. 9 The overall morphology of the Al-4Zn-3Sn-0.20In alloy in Comparative Example 3;

[0027] Fig.10 XRD pattern of alloy of Example 4;

[0028] Fig.11 Polarization curves of Comparative Examples 1-2 and Example 4;

[0029] Fig.12 Corrosion weight loss results of Comparative Examples 1-2 and Example 4. DETAILED DESCRIPTION

[0030] In order to make the purpose, advantages and technical solutions of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described in full and clearly below. The mass percentage of pure aluminum in the embodiments is greater than 99.99%; the mass percentage of Zn in the Al-Zn master alloy is 10%; the mass percentage of Si in the Al-Si master alloy is 20%; the mass percentage of Sn in the Al-Sn master alloy is 10%; the mass percentage of In in the Al-In master alloy is 1%. The Al-10% Zn master alloy is a commercially available Al10Zn master alloy; the Al-20% Si master alloy is a commercially available Al20Si master alloy; the Al-10% Sn master alloy is a commercially available Al10Sn master alloy; the Al-1% In master alloy uses pure Al and pure In with a mass percentage greater than 99.99, and is configured according to the mass percentage and then melted in a vacuum arc furnace.

[0031] The features and properties of the present invention are further described in detail below in conjunction with the embodiments.

[0032] Example 1

[0033] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 1% Zn, 7% Si, 3% Sn, 0.20% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0034] (2) First, pure Al250g was melted and heated to 680℃, kept warm for 60min, 500g Al-10%Zn master alloy, 1750g Al-20%Si master alloy, 1500g Al-10%Sn master alloy, 1000g Al-1%In master alloy were added, and a piece of 40×40×3mm Q235 steel sheet was added. The temperature was continued to be raised to 710℃ and kept warm for 1 hour to make the Fe element reach saturation state. After refining, degassing and deslagging, the ingot was cast and the casting temperature was 710℃.

[0035] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to a uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product was subjected to long-term annealing, and the temperature was raised to an annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 50 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0036] Example 2

[0037] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 1% Zn, 7% Si, 3% Sn, 0.10% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0038] (2) First, 750 g of pure Al was melted and heated to 680°C, kept warm for 60 min, 500 g of Al-10% Zn master alloy, 1750 g of Al-20% Si master alloy, 1500 g of Al-10% Sn master alloy, and 500 g of Al-1% In master alloy were added, and a 40×40×3 mm Q235 steel sheet was added. The temperature was continued to be raised to 710°C and kept warm for 1 hour to make the Fe element reach saturation state. After refining, degassing and deslagging, the ingot was cast and the casting temperature was 710°C.

[0039] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to a uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product was subjected to long-term annealing, and the temperature was raised to an annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 100 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0040] Example 3

[0041] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 1% Zn, 7% Si, 3% Sn, 0.05% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0042] (2) First, 1000g of pure Al was melted and heated to 680°C, kept warm for 60 minutes, 500g of Al-10% Zn master alloy, 1750g of Al-20% Si master alloy, 1500g of Al-10% Sn master alloy, and 250g of Al-1% In master alloy were added, and a 40×40×3mm Q235 steel sheet was added. The temperature was continued to be raised to 710°C and kept warm for 1 hour to make the Fe element reach saturation state. After refining, degassing and deslagging, the billet was cast and the casting temperature was 710°C.

[0043] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to a uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product was subjected to long-term annealing, and the temperature was raised to an annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 150 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0044] Example 4

[0045] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 1% Zn, 7% Si, 3% Sn, 0.05% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0046] (2) First, 1000g of pure Al was melted and heated to 680°C, kept warm for 60 minutes, 500g of Al-10% Zn master alloy, 1750g of Al-20% Si master alloy, 1500g of Al-10% Sn master alloy, and 250g of Al-1% In master alloy were added, and a 40×40×3mm Q235 steel sheet was added. The temperature was continued to be raised to 710°C and kept warm for 1 hour to make the Fe element reach saturation state. After refining, degassing and deslagging, the billet was cast and the casting temperature was 710°C.

[0047] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to a uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product was subjected to long-term annealing, and the temperature was raised to an annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 200 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0048] Example 5

[0049] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 4% Zn, 7% Si, 1% Sn, 0.15% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0050] (2) First, melt 2000g of Al-10% Zn and heat it to 680℃, keep it warm for 60min, add 1750g of Al-20% Si master alloy, 500g of Al-10% Sn master alloy, 750g of Al-1% In master alloy, put in a 40×40×3mm Q235 steel sheet, continue to heat it to 710℃ and keep it warm for 1 hour to make the Fe element reach saturation state, and then cast it into a casting after refining, degassing and deslagging, and the casting temperature is 710℃.

[0051] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to a uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product was subjected to long-term annealing, and the temperature was raised to an annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 200 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0052] Example 6

[0053] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 1% Zn, 7% Si, 0.5% Sn, 0.20% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0054] (2) First, 1500g of pure Al was melted and heated to 680°C, kept warm for 60 minutes, 500g of Al-10% Zn master alloy, 1750g of Al-20% Si master alloy, 250g of Al-10% Sn master alloy, and 1000g of Al-1% In master alloy were added, and a 40×40×3mm Q235 steel sheet was added. The temperature was continued to be raised to 710°C and kept warm for 1 hour to make the Fe element reach saturation state. After refining, degassing and deslagging, the ingot was cast and the casting temperature was 710°C.

[0055] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to a uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product was subjected to long-term annealing, and the temperature was raised to an annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 200 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0056] Comparative Example 1

[0057] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 1% Zn, 7% Si, 3% Sn, 0.20% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0058] (2) First, pure Al250g was melted and heated to 680℃, kept warm for 60min, 500g Al-10%Zn master alloy, 1750g Al-20%Si master alloy, 1500g Al-10%Sn master alloy, 1000g Al-1%In master alloy were added, and a piece of 40×40×3mm Q235 steel sheet was added. The temperature was continued to be raised to 710℃ and kept warm for 1 hour to make the Fe element reach saturation state. After refining, degassing and deslagging, the ingot was cast and the casting temperature was 710℃.

[0059] (3) The ingot was subjected to homogenization annealing by heating the temperature to a uniform annealing temperature of 400°C at a heating rate of 20°C / min and then kept at that temperature for 5 h. After removing the oxide layer on the surface of the ingot, the ingot was cut into alloy blocks of 10×10×10 mm.

[0060] Comparative Example 2

[0061] (1) The present invention provides an anode alloy, the components of which, by mass percentage, include: 1% Zn, 7% Si, 3% Sn, 0.05% In, and the remainder is Al and unavoidable impurities (Fe element saturation).

[0062] (2) First, 1000g of pure Al was melted and heated to 680°C, kept warm for 60 minutes, 500g of Al-10% Zn master alloy, 1750g of Al-20% Si master alloy, 1500g of Al-10% Sn master alloy, and 250g of Al-1% In master alloy were added, and a 40×40×3mm Q235 steel sheet was added. The temperature was continued to be raised to 710°C and kept warm for 1 hour to make the Fe element reach saturation state. After refining, degassing and deslagging, the billet was cast and the casting temperature was 710°C.

[0063] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to the uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product annealing was carried out, and the temperature was raised to the annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 10 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0064] Comparative Example 3

[0065] (1) The present invention provides an anode alloy, the composition of which, by mass percentage, includes: 4% Zn, 3% Sn, 0.05% In, and the rest is Al and unavoidable impurities (Fe element saturation).

[0066] (2) First, 500 g of pure Al was melted and heated to 680°C, kept warm for 60 min, and 2000 g of Al-10% Zn master alloy, 1500 g of Al-10% Sn master alloy, and 1000 g of Al-1% In master alloy were added. A 40×40×3 mm Q235 steel sheet was added, and the temperature was continued to be raised to 710°C and kept warm for 1 hour to allow the Fe element to reach a saturated state. After refining, degassing and deslagging, the ingot was cast and the casting temperature was 710°C.

[0067] (3) The ingot was subjected to homogenization annealing, and the temperature was raised to the uniform annealing temperature of 400°C at a heating rate of 20°C / min and kept at this temperature for 5 hours; after removing the oxide layer on the surface of the ingot, the ingot was cut into 10×10×20 mm alloy blocks, and then the finished product annealing was carried out, and the temperature was raised to the annealing temperature of 550°C at a heating rate of 20°C / min and annealed for 10 hours. The ingot was then cut into 10×10×10 mm alloy blocks.

[0068] Fig.11 2 are polarization curves of the sacrificial anode alloys of Example 4 and Comparative Examples 1-2. It can be seen from the figure that the self-corrosion potential of the sacrificial anode alloys treated by long-term annealing is reduced, the corrosion current density is reduced, and the sacrificial anode performance is improved.

[0069] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with other methods. Any modification, equivalent replacement, or modification made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an aluminum sacrificial anode alloy, characterized in that: The preparation method steps are as follows: (1) Melting the aluminum ingot, then sequentially adding Al-Zn master alloy, Al-Si master alloy, Al-Sn master alloy, and Al-In master alloy, and casting to form a casting billet after refining and standing; (2) annealing the ingot cast in step (1); Annealing the ingot includes: firstly uniform annealing and then finished product annealing; The homogenization annealing is as follows: placing the ingot into a furnace at room temperature, heating the ingot to 400-550°C at a heating rate of 18-20°C / min, and annealing for 1-10 hours; after annealing, air cooling to room temperature; The finished product annealing is as follows: placing the ingot into a furnace at room temperature, heating the ingot to 400-550°C at a heating rate of 18-20°C / min, annealing for 50-200h, and after annealing, air cooling to room temperature; The anode alloy has the following composition by mass percentage: Zn: 0.5-5%, Si: 2-10%, Sn: 0.1-3%, In: 0.01-0.2%, the rest being Al and inevitable impurities, and the Fe element reaches a saturated state.

2. The method for preparing the aluminum sacrificial anode alloy according to claim 1, characterized in that: In step (1), the aluminum ingot is melted and heated to 680-800° C., kept at this temperature for 1 hour, and then Al-Zn master alloy, Al-Si master alloy, Al-Sn master alloy and Al-In master alloy are added in sequence.

3. The method for preparing the aluminum sacrificial anode alloy according to claim 1, characterized in that: After adding the intermediate alloy in step (1), the temperature is continued to be raised to 710-750°C and kept at this temperature for 1-2 hours, and then pouring is performed at 710°C.

4. The method for preparing the aluminum sacrificial anode alloy according to claim 1, characterized in that: Before the finished product is subjected to long-term annealing, the oxide layer on the surface of the slab is removed. After annealing, the slab is air-cooled to room temperature and cut into alloy blocks of 10×10×10mm.

5. The method for preparing an aluminum sacrificial anode alloy according to claim 1, wherein the anode alloy has the following composition by mass percentage: Zn: 0.5-5%, Si: 2-10%, Sn: 1.5-3%, In: 0.05-0.2%, and the rest is Al and unavoidable impurities, and the Fe element reaches a saturated state.