Preparation method and application of polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer

By using polycarboxyl-Fe(III) core complex in the inorganic envelope process of titanium dioxide, the problem of adjusting the b value of titanium dioxide is solved, the b value is improved and the color is improved, and the 'cyan cool' senses are eliminated. It is also suitable for a variety of production processes, meeting the flexibility and performance requirements of market demand.

CN115651100BActive Publication Date: 2024-11-08JINAN YUXING CHEM
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211323317.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-11-08
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

The existing titanium dioxide production process is difficult to flexibly adjust the b value of titanium dioxide and cannot meet changes in market demand, resulting in the discomfort of the product in some application scenarios.

Method used

Using polycarboxyl-Fe(III) core complex as b-value enhancer, the complex is chimerized in the inorganic envelope process of titanium dioxide, and its uniform adsorption and hydrolysis reaction within the temperature and pH range are formed. The polyFe nuclear hydroxyl structure is uniformly adsorbed on the surface of TiO2 particles, increasing the b value and improving the chromaticity.

Benefits of technology

It effectively increases the b-value of titanium dioxide, eliminates the "cyan-cold" sensory senses, and the process can be used in sulfuric acid and chlorination methods, and has almost no impact on the performance of other pigments, providing flexible customized solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115651100B_ABST
    Figure CN115651100B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer, comprising the following steps: (1) a polyacrylic acid dispersant solution is used as a base liquid, a ferrous sulfate solution and a hydrogen peroxide solution are slowly and dripped into the base liquid, stirred and reacted, and the temperature is 25°C to 30°C; (2) after the ferrous sulfate solution and the hydrogen peroxide solution are dripped at the same time, stirring and aging are continued for 2.5 hours; (3) a trace defoamer is added to the base liquid, a sodium bicarbonate solution is slowly added to the base liquid, carbon dioxide is released, and the solution is neutralized to a pH value of 4.5 to 5.0, and finally a wine-red polycarboxyl-Fe (III) core complex solution is obtained. At the same time, the application thereof is disclosed, which can be embedded in the titanium dioxide inorganic coating section, the process flow is simple and flexible, and the titanium dioxide b value enhancer can be added in an appropriate amount according to the incoming material indicators of each titanium dioxide production enterprise and the customized needs of the customer to control the b value of the titanium dioxide product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer, belonging to the field of titanium dioxide. Background Art

[0002] Titanium dioxide is an inorganic white pigment with excellent performance. Its main component is titanium dioxide (TiO2). According to the different crystal forms, it can be divided into rutile titanium dioxide and anatase titanium dioxide. It has good chemical stability, strong hiding power, excellent weather resistance and high pigment performance. There is currently no alternative product in high-performance inorganic white pigments. It is widely used in many important industries related to national production, such as coatings, inks, rubber and resins, papermaking, food and pharmaceuticals, printing, construction, and automobile industries.

[0003] The main performance indicators of titanium dioxide include whiteness, tinting power, oil absorption, pH value, fineness, resistivity, rutile conversion rate, etc. Among them, whiteness is mainly characterized by Lab value, which is based on the color system established by the International Commission on Illumination (CIE). L value represents lightness, corresponding to the visual signal of white-black, a value and b value represent chromaticity, among which a value corresponds to the visual signal of red-green, and b value corresponds to the visual signal of yellow-blue. CIE summarized the results of experimental measurements by many scientists and found that the human eye is most sensitive to visible light with a wavelength of 555nm, and b value corresponds to the visual signal of yellow-blue. Therefore, b value can best represent the human eye's perception of chromaticity. The change of b value of titanium dioxide has the greatest impact on the visual perception of the naked eye. Therefore, titanium dioxide users have different requirements for the b value of titanium dioxide according to different application scenarios. Nowadays, the competition in the titanium dioxide market is becoming increasingly fierce, and it is gradually developing towards professional and customized high-value-added products. Titanium dioxide manufacturers need a method to flexibly adjust the b value of titanium dioxide to meet the challenges of changing market demand.

[0004] At present, the main titanium dioxide production processes in the world are sulfuric acid method and chlorination method. The main raw material of the sulfuric acid method is ilmenite. After the raw ore is crushed to a certain fineness, it reacts with concentrated sulfuric acid in an acid hydrolysis reactor. After leaching, filtering, concentration and crystallization, black titanium liquid with a certain iron-titanium ratio is made. The black titanium liquid is hydrolyzed to obtain metatitanic acid slurry. The slurry is washed, and after adding salt solution and other auxiliary materials to control the conversion of crystal seeds, it is put into a rotary kiln for calcination to obtain rutile or anatase titanium dioxide. The chloride method titanium dioxide production process obtains pure rutile titanium dioxide after batching, chlorination, TiCl4 refining, TiCl4 oxidation and other stages. Regardless of the sulfuric acid method or the chlorination method, after obtaining titanium dioxide solid particles, inorganic coating treatment is generally required. By coating the surface of titanium dioxide particles with a coating layer of aluminum oxide, silicon oxide, zirconium oxide, and phosphorus aluminum, the active sites are blocked to reduce the photocatalytic activity, and the weather resistance, dispersibility, whiteness, and decolorization of titanium dioxide are improved. The final performance and application scenarios of titanium dioxide are affected by the coating process. The coated titanium dioxide slurry is then washed, flashed, finely crushed, and other processes to obtain commercial titanium dioxide. Summary of the invention

[0005] The present invention provides a preparation method and application of a polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer, wherein the enhancer is applied to the titanium dioxide coating process to controllably enhance the b value of the titanium dioxide product. The b value enhancer and the corresponding b value enhancement process can be universally used and embedded in the sulfuric acid method and chloride method titanium dioxide production processes, thereby eliminating the "cold blue" color of the titanium dioxide product that causes discomfort to the human eye. The chemical structure of the polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer is shown as follows:

[0006]

[0007] A method for preparing a polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer comprises the following steps:

[0008] (1) The polyacrylic acid dispersant solution is used as the base liquid. The ferrous sulfate solution and the hydrogen peroxide solution are slowly and dropwise added to the base liquid, and the reaction is stirred at a temperature of 25°C to 30°C.

[0009] (2) After the ferrous sulfate solution and hydrogen peroxide solution are added simultaneously, continue stirring and aging for 2.5 h;

[0010] (3) Slowly add sodium bicarbonate solution to the base liquid to release carbon dioxide gas and neutralize to a pH of 4.5-5.0, ultimately obtaining a wine-red polycarboxyl-Fe(III) core complex solution. A trace amount of defoamer can be added to the base liquid to prevent bubbles and foam from overflowing the reactor.

[0011] Preferably, the weight average molecular weight of the polyacrylic acid is 10,000, and the monomer content in the solution is 20%; the mass fraction of the ferrous sulfate solution is 20%, and the mass ratio of the polyacrylic acid monomer to the ferrous sulfate is 3-6:1.

[0012] Preferably, the mass fraction of the hydrogen peroxide is 3%, and the mass ratio of ferrous sulfate to hydrogen peroxide is 8-10:1.

[0013] The polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer prepared by the above preparation method and its application in titanium dioxide inorganic coating process.

[0014] Application of polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer in titanium dioxide coating, the coating method is:

[0015] (1) Place the TiO2 slurry with adjusted density in a reactor, start stirring and preheat to 85°C, first dropwise add the aqueous solution of polyacrylic acid-Fe (III) core complex, stir and age for 30 minutes after the dropwise addition is completed;

[0016] (2) Rapidly add the sodium silicate solution, keep the temperature at 85°C after the addition is complete, stir and mature for 60 minutes, and control the pH value to 10.5;

[0017] (3) Add dilute sulfuric acid to pH 6.0 for the first time, and control the addition time to 60 minutes;

[0018] (4) First, add sodium aluminate solution to adjust the pH value to 10.0, and then add dilute sulfuric acid in parallel. After the addition is completed, ripen for 60 minutes and control the pH value at 9.5-10.0;

[0019] (5) Add dilute sulfuric acid for the second time, stir for 60 minutes after the addition is completed, control the pH value to 5.7, filter the slurry, wash, dry and crush the filter cake to obtain the silicon-aluminum coated titanium dioxide product.

[0020] The possible mechanism of action of the b-value enhancer is as follows: during the process of inorganic coating of titanium dioxide, the aqueous solution of the polyacrylic acid-Fe (III) core complex is gradually added to the TiO2 slurry. The carboxyl groups in the complex that are not bound to the Fe (III) core can "bite" on the surface of TiO2 particles (particle size d50≈350 nm) due to van der Waals forces and hydrogen bonds. It has partial dispersant effects that can reduce the agglomeration of TiO2 particles and promote the release of trapped water in the gaps of particle agglomerations. The complex can be more evenly adsorbed on the surface of TiO2 particles. Since the temperature of the TiO2 slurry medium is about 70~85℃ and the pH value is about 8.5~9.5, the Fe core in the complex will combine with the hydroxyl group to separate from the main chain of the polymer, undergo a hydrolysis reaction to form an inorganic colloid with a multi-Fe core hydroxyl structure that is adsorbed on the surface of the TiO2 particles. In this process, the carboxyl ligand of the polyacrylic acid plays a role in delaying the Fe3+ The effect of ion hydrolysis is different from that of simple Fe 3+ When the salt solution is dripped into the hot TiO2 slurry, it will immediately hydrolyze to form colloids, causing the surface of the TiO2 particles to be unevenly coated. The complex has outstanding advantages in terms of coating uniformity. With the subsequent process of coating the surface of the TiO2 particles with silicon, aluminum or zirconium, the "silicon layer", "aluminum layer" or "zirconium layer" will coat the "iron layer" inside. Finally, after the high-temperature process of washing, flash evaporation and steam-powder technology, the colloids with multi-Fe core hydroxyl structures are dehydrated to form a structure similar to iron yellow pigments, which is yellow in color. This increases the b value of titanium dioxide products and eliminates the discomfort of the "cold blue" color of titanium dioxide products to the naked eye.

[0021] Beneficial effects:

[0022] 1. The b-value enhancer and the corresponding process of the present invention can be generally used in the sulfuric acid process and the chloride process titanium dioxide production process, and can effectively enhance the b-value of titanium dioxide products without affecting the performance of other pigments, thereby eliminating the discomforting sense of the naked eye caused by the "cold green color" of titanium dioxide products.

[0023] 2. It can be embedded in the inorganic coating section of titanium dioxide. The process flow is simple and flexible. According to the incoming material indicators of each titanium dioxide production enterprise and the customized needs of customers, the titanium dioxide b value enhancer can be added in an appropriate amount to accurately control the b value of the titanium dioxide product.

[0024] 3. The polyacrylic acid ligand in the polycarboxyl-Fe (III) core complex itself has excellent TiO2 particle dispersion performance and delays Fe 3+ The dual effects of ion hydrolysis ensure the uniform growth and coating of the iron coating on the surface of TiO2 particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is the molecular weight distribution of polyacrylic acid dispersant (GPC gel chromatography). DETAILED DESCRIPTION

[0026] The present invention is further illustrated by the following examples of some representative compounds, but these illustrations are not intended to limit the present invention.

[0027] Example 1

[0028] Preparation method of polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer

[0029] (1) Using a polyacrylic acid dispersant solution (monomer mass fraction of about 20%) as the base liquid under stirring conditions, ferrous sulfate solution (calculated as FeSO4, mass fraction of about 20%) and hydrogen peroxide solution (calculated as H2O2, mass fraction of about 3%) are slowly and dropwise added to the base liquid, maintaining the reaction temperature at 25℃~30℃.

[0030] (2) After the ferrous sulfate solution and hydrogen peroxide solution are added simultaneously, stirring and aging are continued for 2.5 h. During the co-flow process, the red color of the solution gradually deepens.

[0031] (3) Slowly add sodium bicarbonate solution into the base liquid to release carbon dioxide gas and neutralize it to a pH of about 4.5-5.0. A small amount of commercially available defoamer can be added to the base liquid to prevent the generated foam from overflowing the reactor. Finally, a wine-red polycarboxyl-Fe(III) core complex solution with an Fe content of about 0.5-2.5% is obtained.

[0032] Among them, ferrous sulfate is a byproduct of the production of titanium dioxide by the sulfuric acid process. As an iron source of the b-value enhancer, it can reduce the production cost of the b-value enhancer. The mass ratio of the dispersant monomer to ferrous sulfate is 3-6:1, and the mass ratio of ferrous sulfate to hydrogen peroxide is 8-10:1. The molecular weight distribution (GPC gel chromatography) test results of the polyacrylic acid dispersant show that the weight average molecular weight is about Mw≈10000.

[0033] Table 1 GPC test results of polyacrylic acid dispersant

[0034]

[0035] Example 2

[0036] The b-value enhancer of the present invention is applied to the inorganic coating section of titanium dioxide production. The starting material of the coating section is a TiO2 slurry with a temperature of about 70-85°C and a pH value of about 8.5-9.5. Since the amount of the b-value enhancer used is relatively small, the pH value of the overall system hardly decreases after the b-value enhancer is gradually added to the material medium. Under the process conditions, the Fe (III) nucleus in the b-value enhancer is gradually hydrolyzed and uniformly coated on the surface of the TiO2 particles under the dispersion of the polycarboxylic acid ligand to form an "iron layer", and then the classic traditional titanium dioxide inorganic coating processes such as aluminum coating, silicon coating, and zirconium coating are carried out. The b-value enhancement process related to the b-value enhancer of the present invention can be perfectly integrated into the current titanium dioxide inorganic coating process, which is simple and convenient, taking the classic silicon-aluminum coated titanium dioxide product as an example.

[0037] (1) Place the TiO2 slurry with adjusted density in a reactor, start stirring and preheat to 85°C, first drop different amounts of polyacrylic acid-Fe (III) core complex aqueous solution, stir and age for about 30 minutes after the addition is complete.

[0038] (2) Rapidly add the sodium silicate solution. After the addition is complete, stir and mature at a constant temperature for 60 minutes, and control the pH value to around 10.5.

[0039] (3) The first addition of dilute sulfuric acid was controlled within 60 minutes, and the final pH value was around 6.0.

[0040] (4) First, add sodium aluminate solution to adjust the pH value to 10.0, and then add dilute sulfuric acid in parallel. After the addition is completed, mature for 60 minutes and control the pH value to 9.5-10.0.

[0041] (5) Add dilute sulfuric acid for the second time, stir for 60 minutes after the addition is completed, control the pH value to about 5.7, filter the slurry, wash, dry and crush the filter cake to obtain the silicon-aluminum coated titanium dioxide product.

[0042] Results Characterization

[0043] The pigment performance indexes, particle size, whiteness, water phase dispersibility and decolorizing power of silicon-aluminum coated titanium dioxide with different amounts of b-value enhancers were tested. Each index was tested according to the titanium dioxide industry practice: the amount of b-value enhancer added was measured by Fe2O3 and X-ray fluorescence spectrometer; the particle size of titanium dioxide product was measured by Malvern laser particle size analyzer; the whiteness of dry powder was measured by whiteness meter; the water phase dispersibility was measured by scraper fineness meter; the decolorizing power test refers to the blue paste decolorization visual method. The results are shown in Table 2.

[0044] Table 2 Effect of the b-value enhancer of the present invention on the product index of silicon-aluminum coated titanium dioxide

[0045]

[0046] Compared with the silicon-aluminum coated product without the addition of the b-value enhancer, the b-value enhancer and the corresponding addition process of the present invention can increase the b-value of the titanium dioxide product, and the "green and cold" visual sense of the sample is significantly improved. Except for a slight decrease in the L value, the addition of a trace amount of the b-value enhancer has no significant effect on other pigment indicators of the product.

[0047] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer, characterized in that: The following steps are involved: (1) The polyacrylic acid dispersant solution is used as the base liquid. The ferrous sulfate solution and the hydrogen peroxide solution are slowly and dropwise added to the base liquid, and the reaction is stirred at a temperature of 25°C to 30°C. (2) After the ferrous sulfate solution and hydrogen peroxide solution are added simultaneously, continue stirring and aging for 2.5 h; (3) Add a defoamer to the base liquid, slowly add a sodium bicarbonate solution to the base liquid, release carbon dioxide, and neutralize to a pH value of 4.5-5.0, and finally obtain a wine-red polycarboxyl-Fe(III) core complex solution; The weight average molecular weight of the polyacrylic acid is 10000, and the monomer content in the solution is 20%; the mass fraction of the ferrous sulfate solution is 20%, and the mass ratio of the polyacrylic acid monomer to the ferrous sulfate is 3-6:

1.

2. The method for preparing a polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer according to claim 1, characterized in that: The mass fraction of the hydrogen peroxide solution is 3%, and the mass ratio of ferrous sulfate to hydrogen peroxide is 8-10:

1.

3. A polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer prepared by the preparation method according to claim 1 or 2.

4. Use of the polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer according to claim 3 in a titanium dioxide inorganic coating process.

5. Use of the polycarboxyl-Fe (III) core complex titanium dioxide b value enhancer according to claim 4 in the titanium dioxide inorganic coating process, characterized in that: The coating method is: (1) Place the TiO2 slurry with adjusted density in a reactor, start stirring and preheat to 85°C, first dropwise add the aqueous solution of polyacrylic acid-Fe (III) core complex, stir and age for 30 minutes after the dropwise addition is completed; (2) Rapidly add the sodium silicate solution, keep the temperature at 85°C after the addition is complete, stir and mature for 60 minutes, and control the pH value to 10.5; (3) Add dilute sulfuric acid to pH 6.0 for the first time, and control the addition time to 60 minutes; (4) First, add sodium aluminate solution to adjust the pH value to 10.0, and then add dilute sulfuric acid in parallel. After the addition is completed, ripen for 60 minutes and control the pH value at 9.5-10.0; (5) Add dilute sulfuric acid for the second time, stir for 60 minutes after the addition is completed, control the pH value to 5.7, filter the slurry, wash, dry and crush the filter cake to obtain the silicon-aluminum coated titanium dioxide product.

Citation Information

Patent Citations

  • Aqueous poly(meth)acrylic acid (salt) solution and process for preparing same

    CN103249748A

  • Method of polymerization of acrylate on surface of titanium dioxide

    CN106749859A

  • Preparation method of anatase titanium dioxide with high weather resistance

    CN112143261A

  • Aqueous solution of poly(METH)acrylic acid polymer and method for producing same

    WO2011126059A1