Method for preparing nano silicon powder from monocrystalline silicon diamond wire cutting waste
By performing multi-stage cyclic sand milling and spray drying of single crystal silicon diamond wire cutting waste in anhydrous ethanol suspension, combined with magnetic separation, nano-silicon powder is prepared, which solves the high cost of nano-silicon powder in the prior art and The problem of uneven particle size distribution has achieved efficient and low-cost nano-silicon powder preparation, meeting the needs of lithium-ion battery negative electrode materials.
Patent Information
- Application Number
- CN202411527087.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is expensive when preparing nano silicon powder, has a large energy consumption, and has uneven particle size distribution, which affects the stability and cycle life of silicon negative electrode materials, making it difficult to meet the demand for lithium-ion battery negative electrode materials.
采用单晶硅金刚线切割废料通过无水乙醇悬浮液进行多级循环砂磨处理,加入分散剂后进行喷雾干燥和粉碎解聚,结合磁选分离,制备出粒径均匀、颗粒分散性好的纳米硅粉。
It reduces the production cost of nano-silicon, improves the preparation efficiency, meets the needs of large-scale industrial production, realizes the high purity and uniform particle size distribution of nano-silicon powder, and improves the stability and cycle life of the negative electrode material of lithium-ion battery.
Smart Images

Figure CN119038559A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano silicon powder preparation, and in particular to a method for preparing nano silicon powder from waste materials cut by diamond wire of single crystal silicon. Background Art
[0002] The traditional negative electrode material of lithium battery, graphite, has been unable to meet the requirements of lithium battery development due to its theoretical specific capacity of only 372 mAh / g. In contrast, silicon negative electrode material, with its theoretical specific capacity of up to 4200 mAh / g, is regarded as one of the key negative electrode materials to solve the bottleneck of long-range electric vehicles.
[0003] However, during the insertion and extraction process of lithium ions, the silicon negative electrode will undergo significant volume changes (the expansion rate can be as high as 300%, which is more than 10 times the expansion of the graphite negative electrode), resulting in a short cycle life of the silicon negative electrode and unstable performance, which seriously affects the practical application of the silicon negative electrode in lithium-ion batteries.
[0004] Research has found that nano-sizing is a potential direction to solve the expansion of silicon negative electrodes, aiming to alleviate the stress caused by volume changes by reducing the size of silicon particles, thereby improving the stability and cycle life of silicon negative electrodes. Current nano-sizing methods include vapor deposition, molten salt electrolysis, spatial confinement, plasma, and thermochemical methods. Although these methods have achieved the preparation of nano-silicon to a certain extent, the high cost and energy consumption limit its large-scale industrial application. For example, the price of nano-silicon prepared by vapor deposition is as high as 5 million yuan / ton (particle size range is 1~10 nm); while the price of nano-silicon prepared by other methods is also between 700,000 and 1 million yuan / ton (particle size range is 10~100 nm). The high cost of nano-silicon is mainly due to the high cost of raw materials, complex process and high energy consumption in the preparation process. Among them, ball milling, as a low-cost method for preparing nanomaterials, has reduced the preparation cost to a certain extent, but as the particle size is refined to below 100nm, the agglomeration of silicon particles is intensified, affecting the dispersibility and performance of nano-silicon.
[0005] On the other hand, the waste of single crystal silicon diamond wire cutting is waste silicon generated in the process of silicon wafer production, with a purity of up to 99.85% and a huge annual output. However, most of these wastes are sold at low prices or piled up, and have not been used at a high value. Waste silicon materials are mainly composed of two-dimensional micron sheets with a thickness of about 4~5 nm and a particle size D50 of about 1 μm. In addition to the main element Si, the specific composition also contains metal impurities such as Al, Ca, Ni, Fe, Zn, and non-metallic impurities such as Cl, S, and P. These impurities mainly come from auxiliary materials in the cutting process such as nickel-plated diamond wire, organic additives, and aluminum pads.
[0006] Although there have been studies attempting to use waste silicon materials for the preparation of nano silicon-based materials, the prior art still has many problems, such as uneven particle size distribution, difficulty in ensuring silicon purity, etc. The preparation method disclosed in CN 112645333B uses wet ball milling technology, but the two heat treatment processes not only consume a lot of energy, but also the ball milling medium uses a mixture of multiple solvents, which increases the preparation cost; and the method for preparing nano silicon powder by thermal plasma method disclosed in CN 110817882A can obtain nano silicon powder with low oxygen content and uniform distribution, but this method requires specific equipment support, strict operating conditions, and high cost, and is also not suitable for large-scale industrial production.
[0007] Therefore, there is an urgent need to provide a method for preparing nano-silicon powder from single crystal silicon diamond wire cutting waste to solve the above problems. Summary of the invention
[0008] The purpose of the present invention is to overcome the shortcomings and defects of the prior art and provide a method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste, so as to realize secondary resource recycling of single crystal silicon diamond wire cutting waste, reduce the production cost of nano silicon, improve the preparation efficiency, meet the needs of large-scale industrial production, and at the same time, the nano silicon powder prepared by this method has uniform particle size distribution, good particle dispersion, and high product purity, which meets the use requirements of lithium ion battery negative electrode materials.
[0009] The objective of the present invention is achieved through the following technical solutions: A method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste comprises the following steps: S1: dissolving the single crystal silicon diamond wire cutting waste in anhydrous ethanol to prepare a suspension, and subjecting the suspension to multi-stage circulation sand milling treatment by a dual-power horizontal sand milling system to obtain a slurry, wherein a dispersant is added before and during the sand milling process; S2: adding a dispersant to the slurry obtained by sand grinding in S1, and spray drying the slurry to obtain dry silicon powder; S3: The silicon powder is crushed and deagglomerated, and then magnetically separated to remove the metal on the silicon surface to obtain nano silicon powder.
[0010] As a preferred technical solution of the present invention, the mass ratio of the single crystal silicon diamond wire cutting waste to anhydrous ethanol in S1 is 1:1 to 1:10.
[0011] As a preferred technical solution of the present invention, the dual-power horizontal sand mill system in S1 is an integrated single-tank sand mill system composed of a grinding material power system and a separation material power system. Specifically, the single crystal silicon diamond wire cutting waste is first ground in the grinding tank, and then the waste and the grinding medium are centrifugally separated in the grinding tank, wherein the multi-stage circulating sand milling is performed in the same tank.
[0012] As a preferred technical solution of the present invention, the multi-stage circulating sand mill in S1 is a three-stage circulating sand mill, the grinding medium of each stage of circulating sand mill is 0.1-1 mm zirconia beads, the sand milling speed is 1000-1350 rpm, the first-stage sand milling time is 3-7.5 h, the second-stage sand milling time is 7-15 h, and the third-stage sand milling time is 10-15 h.
[0013] As a preferred technical solution of the present invention, the spray drying inlet temperature in S2 is 180-220°C, and the outlet temperature is 80-100°C.
[0014] As a preferred technical solution of the present invention, the silicon powder is crushed and deagglomerated in S3, specifically, the agglomerated silicon powder is broken up and reduced to nano-particle size, and the deagglomeration equipment is a gas flow mill; the metal on the surface of the silicon includes Fe, Ni, Ca, Al, and Zn, and the magnetic separation equipment is a dry magnetic separator.
[0015] As a preferred technical solution of the present invention, the dispersant in S1 and S2 is a mixture of one or more of cetyltrimethylammonium bromide, sodium hexametaphosphate, polyvinylpyrrolidone, triethanolamine, polyethylene glycol 2000, sodium carboxymethyl cellulose, sodium pyrophosphate, sodium citrate, sodium dodecylbenzene sulfonate, and polyether polyols.
[0016] As a preferred technical solution of the present invention, the amount of dispersant added in S1 and S2 is 0.1-2.5% of the mass of the powder.
[0017] Compared with the prior art, the present invention has the following beneficial effects: The present invention prepares nano silicon powder by mixing waste silicon material from cutting of single crystal silicon, anhydrous ethanol and a dispersant, performing a multi-stage cyclic sand milling treatment step, spray drying the sand milled mixture, and performing crushing, depolymerization and magnetic separation steps on the dried silicon powder. The prepared nano silicon powder has uniform particle size distribution, good particle dispersibility and high product purity, meeting the use requirements of negative electrode materials for lithium ion batteries. The present invention has a simple process flow, realizes secondary resource recycling of waste material from cutting of single crystal silicon diamond wire, reduces the production cost of nano silicon, improves preparation efficiency and meets the needs of large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a process flow chart of the present invention.
[0019] Figure 2 This is a scanning electron microscope image of single crystal silicon diamond wire cutting waste according to an embodiment of the present invention.
[0020] Figure 3 This is a particle size distribution diagram of single crystal silicon diamond wire cutting waste according to an embodiment of the present invention. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0022] The technical solution of the present invention provides a method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste.
[0023] Reference Figures 1 to 3 , Figure 1 It is a process flow chart of the present invention. Figure 2 This is a scanning electron microscope image of the waste material of single crystal silicon diamond wire cutting in this embodiment. Figure 2 (a) is an electron microscope image of silicon waste before grinding; Figure 2 (b) is an electron microscope image of silicon waste after primary grinding; Figure 2 (c) is an electron microscope image of silicon waste after secondary grinding; Figure 2 (d) is an electron microscope image of silicon waste after three-stage grinding. Figure 3 This is the particle size distribution diagram of the single crystal silicon diamond wire cutting waste in this embodiment. Figure 3 (a) is the particle size of silicon waste before grinding; Figure 3 (b) is the particle size of silicon waste after primary grinding; Figure 3 (c) in the figure is the particle size of silicon waste after secondary grinding; Figure 3 (d) is the particle size of silicon waste after three-stage grinding. In this embodiment, the following steps are specifically included: S1: Dissolve the single crystal silicon diamond wire cutting waste in anhydrous ethanol to prepare a suspension, and subject the suspension to multi-stage circulation sand grinding treatment by a dual-power horizontal sand grinding system, and add a dispersant before and during the sand grinding process; S2: adding a dispersant to the slurry obtained by sand grinding in S1, and spray drying the slurry to obtain dry silicon powder; S3: The silicon powder is crushed and deagglomerated, and then magnetically separated to remove the metal on the silicon surface to obtain nano silicon powder.
[0024] Optionally, in this embodiment, firstly, the single crystal silicon diamond wire cutting waste is weighed and dissolved in anhydrous ethanol to prepare a suspension; then, the suspension is placed in a dual-power horizontal sand mill system for multi-stage circulation sand milling treatment. In order to meet the requirement that the silicon powder particle size is less than 100nm, the circulation sand milling level is preferably three; the dual-power horizontal sand mill system is an integrated single-tank sand mill system composed of a grinding material power system and a separation material power system. The specific operation is to pump the dispersed suspension into the grinding tank through a diaphragm pump for high-speed grinding. While grinding, the ground suspension will be centrifuged in the grinding tank to separate the waste and the grinding medium. The separated suspension will be discharged into the suspension container, and then enter the grinding chamber through the diaphragm pump for grinding again, and the circulation sand milling is completed until the three-stage sand milling is completed. In addition, dispersants are added before and during sand milling; finally, dispersants are added to the slurry after the third stage of sand milling, and then spray drying is performed to obtain dry silicon powder, and then the dried silicon powder is placed in a gas flow mill to break up the agglomerated silicon powder and reduce it to nanometer particle size, and the silicon powder is placed in a dry magnetic separator for magnetic separation to remove metals such as Fe, Ni, Ca, Al, and Zn on the silicon surface, and finally nano silicon powder is obtained. By reducing the volume of the silicon negative electrode, the problem of short cycle life and unstable performance caused by the expansion of the silicon negative electrode is solved. The dual-power horizontal sand mill system used in the present invention separates the dynamic separator from the original grinding rotor structure, and realizes independent operation of material grinding and separation through independent driving, so as to achieve bead material without mesh centrifugal separation and efficient ultrafine grinding. The role of adding dispersants is to prevent the agglomeration of silicon particles during sand milling and spray drying. Through the above steps, the use of single crystal silicon diamond wire cutting waste for secondary resource recycling is realized, the production cost of nano silicon is reduced, the preparation efficiency is improved, and the needs of large-scale industrial production are met. At the same time, the prepared nano silicon powder has uniform particle size distribution, good particle dispersion and high product purity, which meets the use requirements of lithium-ion battery negative electrode materials and effectively improves the stability and cycle life of silicon negative electrodes.
[0025] The present invention will be further described below in conjunction with specific embodiments.
[0026] Example 1
[0027] In the 60L grinding chamber of the dual-power horizontal sand mill, 120kg of zirconia beads with a particle size of 1mm were added. Then, 99% anhydrous ethanol was added to the stirring barrel of the dual-power horizontal sand mill, and single crystal silicon diamond wire cutting waste with a silicon content of 99.99% and a particle size D50 of 330μm was added thereto. The two were mixed to form a suspension with a liquid-to-solid ratio of 10:1, and then 0.5% sodium dodecylbenzene sulfonate was added and dispersed evenly to obtain a slurry.
[0028] Next, the grinding speed of the sand mill was set to 1000 rpm, the separation speed was set to 1500 rpm, the cavity temperature was controlled at 49.5±0.5°C, and after starting the machine for sand milling for 2 hours, 0.5% sodium dodecylbenzene sulfonate was added to the mixing barrel, and the sand milling was continued for 3 hours. Samples were taken for testing, and the average particle size of the silicon particles in the slurry reached 580 nm.
[0029] Afterwards, the grinding medium was replaced with 120 kg of zirconia beads with a particle size of 0.3-0.4 mm, the slurry was moved back into the slurry barrel, the grinding speed was adjusted to 1200 rpm, the separation speed was adjusted to 1500 rpm, the chamber temperature was controlled at 59.5±0.5℃, and after starting the machine for sand grinding for 2 hours, 0.3% of sodium dodecylbenzene sulfonate was added to the mixing barrel, and sand grinding was continued for 5 hours. Samples were taken for testing, and the average particle size of the silicon particles in the slurry was reduced to 110 nm.
[0030] The grinding medium was replaced again with 120 kg of zirconia beads with a particle size of 0.1 mm. The slurry was moved back into the slurry barrel, the grinding speed was adjusted to 1300 rpm, the separation speed was set to 1500 rpm, the chamber temperature was controlled at 49±0.5℃, and after sand grinding for 10 hours, samples were taken for testing. The average particle size of the silicon particles in the slurry reached 90 nm.
[0031] Finally, 0.1% sodium dodecylbenzene sulfonate was added to the sand-milled silicon slurry and spray-dried, where the spray drying inlet temperature was 200°C, the outlet temperature was 100°C, and the atomizer frequency was 250HZ. The spray-dried silicon powder was then crushed and depolymerized by an air flow mill with an air flow rate of 40m³ / min, and magnetically separated in a dry magnetic separator to finally obtain nano silicon powder.
[0032] Example 2
[0033] In the 60L grinding chamber of the dual-power horizontal sand mill, 120kg of zirconia beads with a particle size of 1mm were added. Then, 99% anhydrous ethanol was added to the stirring barrel of the dual-power horizontal sand mill, and single-crystal silicon diamond wire cutting waste with a silicon content of 99.99% and a particle size D50 of 330μm was added thereto. The two were mixed to form a suspension with a liquid-solid ratio of 3:1, and then 0.2% polyvinyl pyrrolidone with a molecular weight of 58000 was added and evenly dispersed to obtain a slurry.
[0034] Next, the grinding speed of the sand mill was set to 1000 rpm, the separation speed was set to 1500 rpm, the cavity temperature was controlled at 49±0.5°C, and after starting the machine for sand milling for 2 hours, 0.5% polyvinyl pyrrolidone with a molecular weight of 58,000 was added to the mixing barrel. The sand milling was continued for 3 hours, and samples were taken for testing. At this time, the average particle size of the silicon particles in the slurry reached 620 nm.
[0035] Afterwards, the grinding medium was replaced with 120kg of zirconia beads with a particle size of 0.3-0.4mm, the slurry was moved back into the slurry barrel, the grinding speed was adjusted to 1200rpm, the separation speed was 1500rpm, the chamber temperature was controlled at 60.5±0.5℃, and after starting the machine for sand grinding for 2 hours, 0.2% triethanolamine was added to the mixing barrel, and sand grinding was continued for 6 hours. Samples were taken for testing, and the average particle size of the silicon particles in the slurry was reduced to 122nm.
[0036] The grinding medium was replaced again with 120 kg of zirconia beads with a particle size of 0.1 mm. The slurry was moved back into the slurry barrel, the grinding speed was adjusted to 1300 rpm, the separation speed was set to 1500 rpm, the chamber temperature was controlled at 50±0.5℃, and after sand grinding for 10 hours, samples were taken for testing. The average particle size of the silicon particles in the slurry reached 95 nm.
[0037] Finally, 0.1% triethanolamine was added to the sand-milled silicon slurry for spray drying, where the spray drying inlet temperature was 200°C, the outlet temperature was 100°C, and the atomizer frequency was 250HZ. The spray-dried silicon powder was then crushed and depolymerized by an air flow mill with an air flow rate of 40m³ / min, and magnetically separated in a dry magnetic separator to finally obtain nano silicon powder.
[0038] Example 3
[0039] In the 60L grinding chamber of the dual-power horizontal sand mill, 120kg of zirconia beads with a particle size of 1mm were added. Then, 99% anhydrous ethanol was added to the stirring barrel of the dual-power horizontal sand mill, and single-crystal silicon diamond wire cutting waste with a silicon content of 99.99% and a particle size D50 of 330μm was added thereto. The two were mixed to form a suspension with a liquid-to-solid ratio of 5.5:1, and then 0.3% sodium hexametaphosphate was added and dispersed evenly to obtain a slurry.
[0040] Next, the grinding speed of the sand mill was set to 1000 rpm, the separation speed was set to 1500 rpm, the cavity temperature was controlled at 51.5±0.5°C, and after starting the machine for sand milling for 2 hours, 0.5% hexadecyltrimethylammonium bromide was added to the mixing barrel, and the sand milling was continued for 4 hours. Samples were taken for testing, and the average particle size of the silicon particles in the slurry reached 550 nm.
[0041] Afterwards, the grinding medium was replaced with 120kg of zirconium oxide beads with a particle size between 0.3-0.4mm, the slurry was moved back into the slurry barrel, the grinding speed was adjusted to 1250rpm, the separation speed was 1500rpm, the chamber temperature was controlled at 62±0.5℃, and after starting the machine for sand grinding for 2 hours, 0.3% of hexadecyltrimethylammonium bromide was added to the stirring barrel, and sand grinding was continued for 10 hours. Samples were taken for testing, and the average particle size of the silicon particles in the slurry was reduced to 100nm.
[0042] Finally, 0.1% hexadecyl trimethyl ammonium bromide was added to the sand-milled silicon slurry for spray drying, where the spray drying inlet temperature was 200°C, the outlet temperature was 100°C, and the atomizer frequency was 250HZ. The spray-dried silicon powder was then crushed and depolymerized by an air flow mill with an air flow rate of 40m³ / min, and magnetically separated in a dry magnetic separator to finally obtain nano silicon powder.
[0043] Example 4
[0044] In the 60L grinding chamber of the dual-power horizontal sand mill, 120kg of zirconia beads with a particle size of 1mm were added. Then, 99% anhydrous ethanol was added to the stirring barrel of the dual-power horizontal sand mill, and single-crystal silicon diamond wire cutting waste with a silicon content of 99.99% and a particle size D50 of 330μm was added thereto. The two were mixed to form a suspension with a liquid-to-solid ratio of 6.5:1, and then 0.3% sodium hexametaphosphate was added and dispersed evenly to obtain a slurry.
[0045] Next, the grinding speed of the sand mill was set to 1000 rpm, the separation speed was set to 1500 rpm, the cavity temperature was controlled at 45±0.5°C, and after starting the machine for sand milling for 2 hours, 0.5% sodium hexametaphosphate was added to the mixing barrel, and the sand milling was continued for 4 hours. Samples were taken for testing, and the average particle size of the silicon particles in the slurry reached 650 nm.
[0046] Afterwards, the grinding medium was replaced with 120kg of zirconia beads with a particle size of 0.3-0.4mm, and the slurry was moved back into the slurry barrel. The grinding speed was adjusted to 1200rpm, the separation speed was 1500rpm, and the chamber temperature was controlled at 55±1℃. After starting the machine for sand grinding for 2 hours, 0.2% of sodium hexametaphosphate was added to the mixing barrel, and sand grinding was continued for 7 hours. Samples were taken for testing. At this time, the average particle size of the silicon particles in the slurry was reduced to 120nm.
[0047] The grinding medium was replaced again with 120 kg of zirconia beads with a particle size of 0.1 mm. The slurry was moved back into the slurry barrel, the grinding speed was adjusted to 1350 rpm, the separation speed was set to 1500 rpm, the chamber temperature was controlled at 48±1°C, and after sand grinding for 10 hours, samples were taken for testing. The average particle size of the silicon particles in the slurry reached 90 nm.
[0048] Finally, 0.1% sodium hexametaphosphate was added to the sand-milled silicon slurry and spray-dried, where the spray drying inlet temperature was 200°C, the outlet temperature was 100°C, and the atomizer frequency was 250HZ. The spray-dried silicon powder was then crushed and depolymerized by an air flow mill with an air flow rate of 40m³ / min, and magnetically separated in a dry magnetic separator to finally obtain nano silicon powder.
[0049] The above-mentioned embodiments only express the implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste, characterized in that: The following steps are involved: S1: dissolving the single crystal silicon diamond wire cutting waste in anhydrous ethanol to prepare a suspension, and subjecting the suspension to multi-stage circulation sand milling treatment by a dual-power horizontal sand milling system to obtain a slurry, wherein a dispersant is added before and during the sand milling process; S2: adding a dispersant to the slurry obtained by sand grinding in S1, and spray drying the slurry to obtain dry silicon powder; S3: The silicon powder is crushed and deagglomerated, and then magnetically separated to remove the metal on the silicon surface to obtain nano silicon powder.
2. The method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste according to claim 1, characterized in that: The mass ratio of the single crystal silicon diamond wire cutting waste to anhydrous ethanol in S1 is 1:1 to 1:
10.
3. The method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste according to claim 1, characterized in that: The dual-power horizontal sand mill system in S1 is an integrated single-tank sand mill system consisting of a grinding material power system and a separation material power system. Specifically, the single crystal silicon diamond wire cutting waste is first ground in the grinding tank, and then the waste and the grinding medium are centrifugally separated in the grinding tank, wherein the multi-stage circulation sand milling is performed in the same tank.
4. The method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste according to claim 1, characterized in that: The multi-stage circulating sand mill in S1 is a three-stage circulating sand mill, the grinding medium of each stage of circulating sand mill is 0.1-1 mm zirconium oxide beads, the sand milling speed is 1000-1350 rpm, the first-stage sand milling time is 3-7.5 h, the second-stage sand milling time is 7-15 h, and the third-stage sand milling time is 10-15 h.
5. The method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste according to claim 1, characterized in that: The spray drying inlet temperature in S2 is 180-220°C, and the outlet temperature is 80-100°C.
6. The method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste according to claim 1, characterized in that: In S3, the silicon powder is crushed and deagglomerated, specifically, the agglomerated silicon powder is broken up and reduced to nano-particle size, and the deagglomeration equipment is a jet mill; the metals on the surface of the silicon include Fe, Ni, Ca, Al, and Zn, and the magnetic separation equipment is a dry magnetic separator.
7. The method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste according to claim 1, characterized in that: The dispersant in S1 and S2 is a mixture of one or more of cetyltrimethylammonium bromide, sodium hexametaphosphate, polyvinyl pyrrolidone, triethanolamine, polyethylene glycol 2000, sodium carboxymethyl cellulose, sodium pyrophosphate, sodium citrate, sodium dodecylbenzene sulfonate, and polyether polyol.
8. The method for preparing nano silicon powder from single crystal silicon diamond wire cutting waste according to claim 1, characterized in that: The amount of dispersant added in S1 and S2 is 0.1-2.5% of the powder mass.
Citation Information
Patent Citations
Method for recovering silicon powder from cut mortar waste
CN104176737A
Preparation method of nanometer silicon powder
CN111266162A
Method for preparing nano silicon powder by cutting waste silicon material