A production process of environmentally friendly silicone leather
Through the tri-coating method of liquid silicone rubber and the pressing treatment technology of rubber roller machine, the wear resistance and environmental protection of silicone leather are improved, and the problems of short service life and environmental pollution in the existing technology are solved, thus achieving efficient Environmentally friendly silicone leather production.
Patent Information
- Application Number
- CN202210964990.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-24
AI Technical Summary
The existing silicone leather has shortcomings in its wear resistance and environmental protection, has a short service life, and is prone to volatile and harmful gases during the production process, polluting the environment.
Liquid silicone rubber is used as raw material, and the three-way coating method is implemented through a release paper coating machine, including primary surface coating, secondary intermediate layer and three-way primer. The multi-layer structure of silicone is used to improve wear resistance and bonding fastness. It also uses a rubber roller machine to press and combines the infinite speed regulation technology of the drive speed change end to avoid the generation of volatile gases.
It significantly improves the wear resistance and service life of silicone leather, making its feel close to the genuine leather, and achieves wear resistance of more than 1,500 times under the ASTM D3884-09 standard, reducing environmental pollution.
Smart Images

Figure CN115652651B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of leather, and more particularly to a manufacturing process of environmentally friendly organic silicon leather. Background Art
[0002] Silicone leather is a new type of environmentally friendly leather, made from silicone. This new material is combined with microfibers, non-woven fabrics, knitted fabrics and other substrates, and is processed and prepared for a variety of industry applications. Silicone leather uses solvent-free technology to coat and bond silicone on various substrates to make leather.
[0003] Silicone leather has the properties of weather resistance, flame retardancy, high wear resistance, antifouling and easy care, waterproof, skin-friendly and non-irritating, mildew-proof and antibacterial, safe and environmentally friendly, low odor and VOC-free. It can be used for wall interiors, car seats, car steering wheels and car interiors, child safety seats, shoes, bags and fashion accessories, medical, sanitary, ships and yachts and other public transportation places, outdoor equipment, etc. It belongs to the new material industry developed in the 21st century and has broad development and application prospects. Therefore, the development and design of a silicone leather with environmental protection and overall performance improvement to extend the service life has good application prospects. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a process for producing environmentally friendly silicone leather, which has the effect of significantly improving the environmental friendliness and wear resistance of the silicone leather and extending its service life.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A process for producing environmentally friendly silicone leather comprises adopting liquid silicone rubber as a raw material and implementing a three-layer coating method with a release paper coater; the three-layer coating method comprises a first surface coating, a second intermediate layer and a third primer coating; wherein the first surface coating comprises coating a layer of silicone in the gaps on the release paper, and then drying the layer of silicone in the gaps on the release paper through a heated thermal oil oven; the second intermediate layer comprises coating two layers of silicone on the release paper treated with the first surface coating, and then drying the two layers of silicone on the release paper through a heated thermal oil oven; the third primer coating comprises coating three layers of silicone on the release paper treated with the second intermediate layer, and then drying the third silicone on the release paper to a semi-dry state through a heated thermal oil oven, making the microfiber base fabric and the semi-dry third silicone adhere and subjected to a pressure treatment by a rubber roller machine, and finally placed in a aging room to be fully cured.
[0007] By adopting the above technical scheme, a layer of silicone formed by intermittent coating realizes the effect of surface texture, and the second layer of silicone increases the thickness of the environmentally friendly silicone leather, so that the second layer of silicone plays a role of supporting the first layer of silicone, thereby improving the overall wear resistance; the three layers of silicone are used to ensure the bonding strength between the silicone resin and the microfiber base cloth, so that the production process of the environmentally friendly silicone leather has the effect of significantly improving the environmental protection and wear resistance of the silicone leather and extending the service life.
[0008] The present invention is further configured as follows: in the one-time surface coating, the thickness of a layer of silicone is 0.01-0.02 mm, the coating speed is 6 m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140-160° C., and the drying time is 1.5 min.
[0009] The present invention is further configured as follows: in the secondary intermediate layer, the thickness of the two layers of silicone is 0.2-0.25 mm, the coating speed is 6 m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140-160° C., and the drying time is 1.5 min.
[0010] The present invention is further configured as follows: in the three primer coatings, the thickness of the three layers of silicone is 0.3-0.35 mm, the coating speed is 6 m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 80°C for the first stage, 100°C for the second stage, 120°C for the third stage, 140°C for the fourth stage and 160°C for the fifth stage, and the drying time is 3 minutes.
[0011] The present invention is further configured as follows: the liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1; the component A includes hydroxyl-terminated polydimethylsiloxane and silicon dioxide in a mass ratio of 3:2; the component B includes silicone oil, color powder and dispersant in a mass ratio of 60-70:30-40:2-5.
[0012] By adopting the above technical scheme, the generation of volatile harmful gases and pollution and damage to the environment can be avoided during the production process of the coating; and the overall wear resistance and service life of the environmentally friendly silicone leather obtained through the production process of the environmentally friendly silicone leather can be significantly improved, so that the feel of the environmentally friendly silicone leather is similar to that of genuine leather, thereby improving the feel, and after testing, the leather wear resistance reaches more than 1500 times under the ASTM D3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard.
[0013] The present invention is further configured as follows: the second layer of silica gel also includes expanded microspheres with a mass fraction of 0.5-2%, and the particle size of the expanded microspheres is 80-120 μm; and the second layer of silica gel includes a pretreatment process, and the pretreatment process is pre-baking at 100-120° C. for 60-90 seconds.
[0014] By adopting the above technical scheme, the expanded microspheres are effectively dispersed in the high-viscosity second layer of silicone and maintain a stable structure while being subjected to strong stirring at a high shear rate. The pretreatment process also prevents the expanded microspheres from expanding during the drying process in the heated thermal oil oven and affecting the stability of the environmentally friendly silicone leather obtained by the production process of the environmentally friendly silicone leather.
[0015] The present invention is further configured as follows: the rubber roller machine includes a roller machine end for performing a pressure treatment on the laminated microfiber base fabric and the semi-dry three-times silicone and a drive speed-changing end for adjusting the running speed of the roller machine end; the roller machine end includes two rubber rollers and two roller machine frames respectively located at the two ends of the rubber rollers and rotatably connected; the same end of the two rubber rollers is provided with mutually meshing connecting gears, and one of the rubber rollers is connected to the drive speed-changing end.
[0016] By adopting the above technical scheme, the driving speed-changing end is used to adjust the running speed of the roller machine end, so that when the laminated microfiber base cloth and the semi-dry tertiary silicone rubber are subjected to a pressure treatment, the pressure treatment speed is adjusted in order, and the rotation speed of the rubber roller is adjusted in real time in combination with the dry state of the tertiary silicone rubber, so as to significantly improve the bonding firmness of the environmentally friendly silicone leather obtained by the pressure treatment of the rubber roller machine, thereby significantly extending the service life of the environmentally friendly silicone leather.
[0017] The present invention is further configured as follows: the driving speed-changing end comprises a driving shaft coaxially connected to the corresponding rubber roller, two speed-changing frames respectively connected to the two ends of the driving shaft for rotation, and a horizontal linear moving unit; the outer peripheral side wall of the driving shaft is axially provided with a limiting ridge, and is sleeved with a friction wheel matching the limiting ridge; the horizontal linear moving unit is used to drive the friction wheel to move axially along the driving shaft; the outer peripheral side wall of the friction wheel is abutted with a rotating cone, the upper side of the rotating cone is horizontal, and its two ends are respectively connected to the corresponding speed-changing frames for rotation, and the speed-changing frame is provided with a uniform-speed motor for driving the rotating cone to make a uniform circumferential rotation motion with its axis as the axis.
[0018] By adopting the above technical scheme, when the horizontal linear moving unit drives the friction wheel to move axially along the active rotating shaft, the friction wheel will contact the outer peripheral side wall of the rotating cone which is driven by a uniform speed motor to make a uniform circumferential rotational motion along its axial direction at different linear speeds, thereby achieving the purpose of steplessly and orderly adjusting the circumferential rotation speed of the friction wheel, and significantly improving the bonding strength of the environmentally friendly silicone leather obtained by the pressure treatment of the rubber roller machine, thereby effectively extending the service life of the environmentally friendly silicone leather.
[0019] The present invention is further configured as follows: the horizontal linear moving unit includes a speed regulating frame connected and fixed to the corresponding speed regulating frame, a double-headed screw inserted into the speed regulating frame in the vertical direction, and a stepping motor used to drive the double-headed screw to rotate and fixed to the speed regulating frame; the upper and lower ends of the double-headed screw are threadedly connected with lifting thread blocks that are symmetrically distributed up and down, the lifting thread blocks are connected with adapter swing arms for vertical rotation, and the ends of the two adapter swing arms away from the corresponding lifting thread blocks are simultaneously connected with the same lateral push part for vertical rotation, and the lateral push part is provided with two push plates that respectively contact the side surfaces of the friction wheel on both sides.
[0020] By adopting the above technical solution, the stepper motor drives the double-headed screw to make a circumferential rotational motion about its axis during operation, thereby driving the two lifting thread blocks to move closer to or away from each other, and when the two lifting thread blocks move closer to each other, the lateral push part gradually moves away from the double-headed screw in the horizontal direction, thereby pushing the friction wheel to move away from the double-headed screw; and when the two lifting thread blocks move away from each other, the lateral push part gradually moves closer to the double-headed screw in the horizontal direction, thereby pushing the friction wheel to move closer to the double-headed screw, thereby achieving the purpose of stepless speed regulation.
[0021] The present invention is further configured as follows: a limiting column is arranged between the two speed change frames and penetrates the lateral push portion along the axial direction of the active rotating shaft, and a positioning intermediate body is arranged in the middle part of the double-headed screw; a cone top fitting body and a cone bottom fitting body matching with the corresponding end of the rotating cone are respectively arranged on opposite sides of the two speed change frames.
[0022] By adopting the above technical scheme, the cone top fitting body and the cone bottom fitting body can significantly improve the rotational stability of the rotating cone, so as to significantly improve the rotational stability of the friction wheel in contact with the surface of the rotating cone; and the limiting column will improve the horizontal displacement stability of the lateral push part, and the positioning intermediate body will improve the movement stability of the lifting thread block, so that the rubber roller machine has the effect of stable operation and improving the structural stability and bonding firmness of the obtained environmentally friendly silicone leather.
[0023] In summary, the present invention has the following beneficial effects: by adopting liquid silicone rubber composed of component A and component B in a mass ratio of 1:1; and component A includes hydroxyl-terminated polydimethylsiloxane and silica in a mass ratio of 3:2; component B includes silicone oil, color powder and dispersant in a mass ratio of 60-70:30-40:2-5, and then combining with a release paper coating machine to implement a three-time coating method, after the three-time coating method is completed, it is processed by a rubber roller machine including a roller machine end for pressing the laminated microfiber base cloth with the semi-dry three-time silica gel and a driving speed-changing end for adjusting the running speed of the roller machine end, thereby achieving stepless speed regulation, avoiding the generation of volatile harmful gases and pollution and damage to the environment, and significantly improving the overall wear resistance and service life of the environmentally friendly silicone leather obtained by the production process of the environmentally friendly silicone leather. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a structural schematic diagram of this embodiment;
[0025] Figure 2 It is a schematic diagram of the local structure of this embodiment.
[0026] Explanation of the reference numerals: 1. roller machine end; 11. roller frame; 12. rubber roller; 13. connecting gear; 2. driving speed change end; 21. speed change frame; 211. speed regulating stand; 212. cone top fitting body; 213. cone bottom fitting body; 214. limiting column; 22. rotating cone; 23. uniform speed motor; 24. driving shaft; 241. limiting ridge; 242. friction wheel; 25. double-headed screw; 251. positioning intermediate body; 26. stepping motor; 27. lateral push part; 271. push plate; 28. lifting thread block; 29. transfer swing arm. DETAILED DESCRIPTION
[0027] In order to make the technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0028] The following is a specific description of the manufacturing process of the environmentally friendly silicone leather according to the embodiment of the present invention:
[0029] A process for producing environmentally friendly silicone leather, including using liquid silicone rubber as a raw material and a release paper coater to implement a three-coating method. Specifically, the raw material liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes hydroxyl-terminated polydimethylsiloxane and silicon dioxide in a mass ratio of 3:2, and component B includes silicone oil, color powder and dispersant in a mass ratio of 60-70:30-40:2-5. Conventional products can be used for color powder and dispersant, which will not be described here. At the same time, the three-coating method includes a top coating, a second intermediate layer and three primer coatings. Among them, the first surface coating includes coating a layer of silicone in the gaps on the release paper, and then drying the layer of silicone coated on the gaps on the release paper through a heated thermal oil oven; the second intermediate layer includes coating two layers of silicone on the release paper treated with the first surface coating, and then drying the two layers of silicone coated on the release paper through a heated thermal oil oven; the third primer coating includes coating three layers of silicone on the release paper treated with the second intermediate layer, and then drying the third silicone on the release paper to a semi-dry state through a heated thermal oil oven, making the microfiber base cloth and the semi-dry third silicone bonded and pressed by a rubber roller machine, and finally placed in a aging room until fully cured.
[0030] Therefore, a layer of silicone formed by gap coating achieves the effect of surface texture, and the second layer of silicone increases the thickness of the environmentally friendly silicone leather, so that the second layer of silicone plays the role of supporting the first layer of silicone, thereby improving the overall wear resistance; the third layer of silicone is used to ensure the bonding strength between the silicone resin and the microfiber base cloth, so that the production process of the environmentally friendly silicone leather has the effect of significantly improving the environmental protection, wear resistance and service life of the silicone leather. In the process of coating production, the generation of volatile harmful gases and pollution and damage to the environment are avoided; and the overall wear resistance and service life of the environmentally friendly silicone leather obtained through the production process of the environmentally friendly silicone leather are significantly improved, so that the feel of the environmentally friendly silicone leather is similar to that of genuine leather, thereby improving the feel.
[0031] It should be mentioned that in the first top coating, the thickness of the first layer of silicone is 0.01-0.02mm, the coating speed is 6m / min, the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140-160℃, and the drying time is 1.5min. In the secondary intermediate layer, the thickness of the second layer of silicone is 0.2-0.25mm, the coating speed is 6m / min, the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140-160℃, and the drying time is 1.5min. In the third primer coating, the thickness of the three layers of silicone is 0.3-0.35mm, the coating speed is 6m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 80℃ for the first stage, 100℃ for the second stage, 120℃ for the third stage, 140℃ for the fourth stage, and 160℃ for the fifth stage, and the drying time is 3min.
[0032] like Figure 1 As shown, the rubber roller machine includes a roller machine end 1 for pressing the laminated microfiber base fabric with the semi-dry three-times silicone and a drive speed change end 2 for adjusting the running speed of the roller machine end 1. The roller machine end 1 includes two rubber rollers 12 and two roller machine frames 11 respectively located at both ends of the rubber rollers 12 and rotatably connected. A connecting gear 13 meshing with each other is provided at the same end of the two rubber rollers 12, and one of the rubber rollers 12 is connected to the drive speed change end 2, so that when the drive speed change end 2 drives the corresponding rubber roller 12 to rotate, the connecting gear 13 drives the other rubber roller 12 to rotate at the same angular velocity. Therefore, by driving the speed-changing end 2 to adjust the running speed of the roller machine end 1, the pressing treatment speed is adjusted in order when the laminated microfiber base cloth and the semi-dry tertiary silicone rubber are subjected to a pressing treatment, so as to adjust the rotation speed of the rubber roller 12 in real time in combination with the dry state of the tertiary silicone rubber, so as to significantly improve the bonding firmness of the environmentally friendly silicone leather obtained by the pressing treatment of the rubber roller machine, thereby significantly extending the service life of the environmentally friendly silicone leather.
[0033] It should be noted that the drive speed change end 2 includes a driving shaft 24 coaxially connected to the corresponding rubber roller 12, two speed change frames 21 respectively connected to the two ends of the driving shaft 24, and a horizontal linear moving unit. Among them, a limit rib 241 is axially arranged on the outer peripheral side wall of the driving shaft 24, and a friction wheel 242 matching the limit rib 241 is sleeved. The horizontal linear moving unit is used to drive the friction wheel 242 to move axially along the driving shaft 24.
[0034] At the same time, in order to realize the driving friction wheel 242 to make circumferential rotational motion and drive the rubber roller 12 to rotate, a rotating cone 22 is abutted against the outer peripheral side wall of the friction wheel 242. The upper side of the rotating cone 22 is in a horizontal state, so as to maintain a stable abutting contact state with the friction wheel 242, and the two ends of the rotating cone 22 are respectively connected to the corresponding speed change frame 21 for rotation, and a uniform speed motor 23 is provided on the speed change frame 21 for driving the rotating cone 22 to make a uniform circumferential rotational motion with its axis as the axis. Therefore, when the horizontal linear moving unit drives the friction wheel 242 to move axially along the active rotating shaft 24, the friction wheel 242 will be in contact with the outer peripheral side wall of the rotating cone 22 that is driven by the uniform speed motor 23 to make a uniform circumferential rotational motion along its axial direction at different linear speeds, thereby achieving the purpose of infinitely and orderly adjusting the circumferential rotation speed of the friction wheel 242, so that the bonding firmness of the environmentally friendly silicone leather obtained by the rubber roller machine pressing treatment is significantly improved, thereby effectively extending the service life of the environmentally friendly silicone leather.
[0035] like Figure 1 , Figure 2As shown, the horizontal linear moving unit includes a speed regulating frame 211 connected and fixed to the corresponding speed-changing frame 21, a double-headed screw 25 inserted in the vertical direction on the speed regulating frame 211, and a stepping motor 26 for driving the double-headed screw 25 to rotate and fixed on the speed regulating frame 211. Among them, the upper and lower ends of the double-headed screw 25 are both threadedly connected with lifting thread blocks 28 symmetrically distributed up and down, and the two lifting thread blocks 28 are both rotatably connected with the transfer swing arm 29 up and down. The ends of the two transfer swing arms 29 that are away from the corresponding lifting thread blocks 28 are simultaneously rotated up and down and connected to the same lateral push portion 27, and two push plates 271 are provided on the lateral push portion 27, which are respectively in contact with the side surfaces of the friction wheel 242. Then, when the stepper motor 26 is running, the stepper motor 26 drives the double-headed screw 25 to make a circumferential rotational movement with its axis as the axis, and then the two lifting thread blocks 28 are driven to move closer to or away from each other. When the two lifting thread blocks 28 move closer to each other, the lateral push portion 27 gradually moves away from the double-headed screw 25 in the horizontal direction, thereby pushing the friction wheel 242 to move away from the double-headed screw 25; and when the two lifting thread blocks 28 move away from each other, the lateral push portion 27 gradually moves closer to the double-headed screw 25 in the horizontal direction, thereby pushing the friction wheel 242 to move closer to the double-headed screw 25, so as to achieve the purpose of stepless speed regulation.
[0036] It should be noted that a limiting column 214 is provided between the two speed change frames 21, which penetrates the lateral push portion 27 along the axial direction of the driving shaft 24, and a positioning intermediate body 251 is provided in the middle of the double-headed screw 25. A cone top matching body 212 and a cone bottom matching body 213 matching with the corresponding end of the rotating cone 22 are provided on the opposite sides of the two speed change frames 21. Therefore, the cone top matching body 212 and the cone bottom matching body 213 play a role in significantly improving the rotation stability of the rotating cone 22, so as to significantly improve the rotation stability of the friction wheel 242 in contact with the surface of the rotating cone 22; and the limiting column 214 will improve the horizontal displacement stability of the lateral push portion 27, and the positioning intermediate body 251 plays a role in improving the movement stability of the lifting screw block 28, so that the rubber roller machine has the effect of stable operation and improving the structural stability and bonding firmness of the obtained environmentally friendly silicone leather.
[0037] Embodiment 1
[0038] A process for producing environmentally friendly silicone leather, including using liquid silicone rubber as a raw material and a release paper coater to implement a three-coating method. Specifically, the raw material liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes hydroxyl-terminated polydimethylsiloxane and silicon dioxide in a mass ratio of 3:2, and component B includes silicone oil, color powder and dispersant in a mass ratio of 63:34:3. Among them, the color powder and dispersant can be conventional products, which will not be described here. At the same time, the three-coating method includes one top coating, two intermediate layers and three primer coatings. Among them, the first surface coating includes coating a layer of silicone in the gaps on the release paper, and then drying the layer of silicone coated on the gaps on the release paper through a heated thermal oil oven; the second intermediate layer includes coating two layers of silicone on the release paper treated with the first surface coating, and then drying the two layers of silicone coated on the release paper through a heated thermal oil oven; the third primer coating includes coating three layers of silicone on the release paper treated with the second intermediate layer, and then drying the third silicone on the release paper to a semi-dry state through a heated thermal oil oven, making the microfiber base cloth and the semi-dry third silicone bonded and pressed by a rubber roller machine, and finally placed in a aging room until fully cured.
[0039] Therefore, a layer of silicone formed by gap coating achieves the effect of surface texture, and the second layer of silicone increases the thickness of the environmentally friendly silicone leather, so that the second layer of silicone plays the role of supporting the first layer of silicone, thereby improving the overall wear resistance; the third layer of silicone is used to ensure the bonding strength between the silicone resin and the microfiber base cloth, so that the production process of the environmentally friendly silicone leather has the effect of significantly improving the environmental protection, wear resistance and service life of the silicone leather. In the process of coating production, the generation of volatile harmful gases and pollution and damage to the environment are avoided; and the overall wear resistance and service life of the environmentally friendly silicone leather obtained through the production process of the environmentally friendly silicone leather are significantly improved, so that the feel of the environmentally friendly silicone leather is similar to that of genuine leather, thereby improving the feel.
[0040] It should be mentioned that in the first top coating, the thickness of the silicone layer is 0.01mm, the coating speed is 6m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140℃, and the drying time is 1.5min. In the secondary intermediate layer, the thickness of the second layer of silicone is 0.2mm, the coating speed is 6m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140℃, and the drying time is 1.5min. In the third primer coating, the thickness of the three layers of silicone is 0.3mm, the coating speed is 6m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 80℃ for the first stage, 100℃ for the second stage, 120℃ for the third stage, 140℃ for the fourth stage, and 160℃ for the fifth stage, and the drying time is 3min.
[0041] like Figure 1As shown, the rubber roller machine includes a roller machine end 1 for pressing the laminated microfiber base fabric with the semi-dry three-times silicone and a drive speed change end 2 for adjusting the running speed of the roller machine end 1. The roller machine end 1 includes two rubber rollers 12 and two roller machine frames 11 respectively located at both ends of the rubber rollers 12 and rotatably connected. A connecting gear 13 meshing with each other is provided at the same end of the two rubber rollers 12, and one of the rubber rollers 12 is connected to the drive speed change end 2, so that when the drive speed change end 2 drives the corresponding rubber roller 12 to rotate, the connecting gear 13 drives the other rubber roller 12 to rotate at the same angular velocity. Therefore, by driving the speed-changing end 2 to adjust the running speed of the roller machine end 1, the pressing treatment speed is adjusted in order when the laminated microfiber base cloth and the semi-dry tertiary silicone rubber are subjected to a pressing treatment, so as to adjust the rotation speed of the rubber roller 12 in real time in combination with the dry state of the tertiary silicone rubber, so as to significantly improve the bonding firmness of the environmentally friendly silicone leather obtained by the pressing treatment of the rubber roller machine, thereby significantly extending the service life of the environmentally friendly silicone leather.
[0042] It should be noted that the drive speed change end 2 includes a driving shaft 24 coaxially connected to the corresponding rubber roller 12, two speed change frames 21 respectively connected to the two ends of the driving shaft 24, and a horizontal linear moving unit. Among them, a limit rib 241 is axially arranged on the outer peripheral side wall of the driving shaft 24, and a friction wheel 242 matching the limit rib 241 is sleeved. The horizontal linear moving unit is used to drive the friction wheel 242 to move axially along the driving shaft 24.
[0043] At the same time, in order to realize the driving friction wheel 242 to make circumferential rotational motion and drive the rubber roller 12 to rotate, a rotating cone 22 is abutted against the outer peripheral side wall of the friction wheel 242. The upper side of the rotating cone 22 is in a horizontal state, so as to maintain a stable abutting contact state with the friction wheel 242, and the two ends of the rotating cone 22 are respectively connected to the corresponding speed change frame 21 for rotation, and a uniform speed motor 23 is provided on the speed change frame 21 for driving the rotating cone 22 to make a uniform circumferential rotational motion with its axis as the axis. Therefore, when the horizontal linear moving unit drives the friction wheel 242 to move axially along the active rotating shaft 24, the friction wheel 242 will be in contact with the outer peripheral side wall of the rotating cone 22 that is driven by the uniform speed motor 23 to make a uniform circumferential rotational motion along its axial direction at different linear speeds, thereby achieving the purpose of infinitely and orderly adjusting the circumferential rotation speed of the friction wheel 242, so that the bonding firmness of the environmentally friendly silicone leather obtained by the rubber roller machine pressing treatment is significantly improved, thereby effectively extending the service life of the environmentally friendly silicone leather.
[0044] like Figure 1 , Figure 2As shown, the horizontal linear moving unit includes a speed regulating frame 211 connected and fixed to the corresponding speed-changing frame 21, a double-headed screw 25 inserted in the vertical direction on the speed regulating frame 211, and a stepping motor 26 for driving the double-headed screw 25 to rotate and fixed on the speed regulating frame 211. Among them, the upper and lower ends of the double-headed screw 25 are both threadedly connected with lifting thread blocks 28 symmetrically distributed up and down, and the two lifting thread blocks 28 are both rotatably connected with the transfer swing arm 29 up and down. The ends of the two transfer swing arms 29 that are away from the corresponding lifting thread blocks 28 are simultaneously rotated up and down and connected to the same lateral push portion 27, and two push plates 271 are provided on the lateral push portion 27, which are respectively in contact with the side surfaces of the friction wheel 242. Then, when the stepper motor 26 is running, the stepper motor 26 drives the double-headed screw 25 to make a circumferential rotational movement with its axis as the axis, and then the two lifting thread blocks 28 are driven to move closer to or away from each other. When the two lifting thread blocks 28 move closer to each other, the lateral push portion 27 gradually moves away from the double-headed screw 25 in the horizontal direction, thereby pushing the friction wheel 242 to move away from the double-headed screw 25; and when the two lifting thread blocks 28 move away from each other, the lateral push portion 27 gradually moves closer to the double-headed screw 25 in the horizontal direction, thereby pushing the friction wheel 242 to move closer to the double-headed screw 25, so as to achieve the purpose of stepless speed regulation.
[0045] It should be noted that a limiting column 214 is provided between the two speed change frames 21, which penetrates the lateral push portion 27 along the axial direction of the driving shaft 24, and a positioning intermediate body 251 is provided in the middle of the double-headed screw 25. A cone top matching body 212 and a cone bottom matching body 213 matching with the corresponding end of the rotating cone 22 are provided on the opposite sides of the two speed change frames 21. Therefore, the cone top matching body 212 and the cone bottom matching body 213 play a role in significantly improving the rotation stability of the rotating cone 22, so as to significantly improve the rotation stability of the friction wheel 242 in contact with the surface of the rotating cone 22; and the limiting column 214 will improve the horizontal displacement stability of the lateral push portion 27, and the positioning intermediate body 251 plays a role in improving the movement stability of the lifting screw block 28, so that the rubber roller machine has the effect of stable operation and improving the structural stability and bonding firmness of the obtained environmentally friendly silicone leather.
[0046] After testing, the environmentally friendly silicone leather of the first embodiment reached more than 1500 times under the ASTM D3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance.
[0047] Embodiment 2
[0048] The difference between Example 2 and Example 1 is that the component B in Example 2 includes silicone oil, color powder and dispersant in a mass ratio of 60:38:2.
[0049] In the first top coating, the thickness of the first layer of silicone is 0.02mm, the coating speed is 6m / min, and the coating temperature is room temperature; the drying temperature of the thermal oil oven is 160℃, and the drying time is 1.5min. In the second intermediate layer, the thickness of the second layer of silicone is 0.25mm, the coating speed is 6m / min, and the coating temperature is room temperature; the drying temperature of the thermal oil oven is 160℃, and the drying time is 1.5min. In the third primer coating, the thickness of the third layer of silicone is 0.35mm, the coating speed is 6m / min, and the coating temperature is room temperature; the drying temperature of the thermal oil oven is 80℃ for the first stage, 100℃ for the second stage, 120℃ for the third stage, 140℃ for the fourth stage, and 160℃ for the fifth stage, and the drying time is 3min.
[0050] After testing, the environmentally friendly silicone leather of the second embodiment reached more than 1500 times under the ASTM D3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance.
[0051] Embodiment 3
[0052] The difference between Example 3 and Example 1 is that the component B in Example 3 includes silicone oil, color powder and dispersant in a mass ratio of 65:30:5.
[0053] In the first top coating, the thickness of the first layer of silicone is 0.015mm, the coating speed is 6m / min, and the coating temperature is room temperature; the drying temperature of the thermal oil oven is 150℃, and the drying time is 1.5min. In the second intermediate layer, the thickness of the second layer of silicone is 0.23mm, the coating speed is 6m / min, and the coating temperature is room temperature; the drying temperature of the thermal oil oven is 150℃, and the drying time is 1.5min. In the third primer coating, the thickness of the third layer of silicone is 0.33mm, the coating speed is 6m / min, and the coating temperature is room temperature; the drying temperature of the thermal oil oven is 80℃ for the first stage, 100℃ for the second stage, 120℃ for the third stage, 140℃ for the fourth stage, and 160℃ for the fifth stage, and the drying time is 3min.
[0054] After testing, the environmentally friendly silicone leather of the third embodiment reached more than 1500 times under the ASTM D3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance.
[0055] Embodiment 4
[0056] The difference between Example 4 and Example 1 is that the second layer of silica gel in Example 4 also includes expanded microspheres with a mass fraction of 0.5%, and the particle size of the expanded microspheres is 80 μm. At the same time, the second layer of silica gel includes a pretreatment process, and the pretreatment process is pre-baking at 100°C for 60 seconds, and then the coating operation is carried out by a release paper coater. Therefore, this embodiment will effectively disperse the expanded microspheres in the high-viscosity second layer of silica gel, and maintain structural stability while withstanding strong stirring at high shear rates, and the pretreatment process prevents the expanded microspheres from expanding during the drying process in the heated thermal oil oven, thereby affecting the stability of the environmentally friendly silicone leather obtained by the production process of the environmentally friendly silicone leather.
[0057] After testing, the environmentally friendly silicone leather of the fourth embodiment reached more than 1500 times under the ASTM D3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance.
[0058] Embodiment 5
[0059] The difference between Example 5 and Example 4 is that the second layer of silica gel in Example 5 further includes expanded microspheres with a mass fraction of 1%, and the particle size of the expanded microspheres is 100 μm. At the same time, the second layer of silica gel includes a pretreatment process, and the pretreatment process is pre-baking at 110° C. for 75 seconds, and then coating by a release paper coating machine.
[0060] After testing, the environmentally friendly silicone leather of the fifth embodiment reached more than 1500 times under the ASTM D3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance.
[0061] Embodiment 6
[0062] The difference between Example 6 and Example 4 is that the second layer of silica gel in Example 6 further includes expanded microspheres with a mass fraction of 2%, and the particle size of the expanded microspheres is 120 μm. At the same time, the second layer of silica gel includes a pretreatment process, and the pretreatment process is pre-baking at 120° C. for 90 seconds, and then coating by a release paper coating machine.
[0063] After testing, the environmentally friendly silicone leather of Example 6 reached more than 1500 times under the ASTM D3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance.
[0064] In summary, the present application adopts liquid silicone rubber composed of component A and component B in a mass ratio of 1:1; and component A includes hydroxyl-terminated polydimethylsiloxane and silica in a mass ratio of 3:2; component B includes silicone oil, color powder and dispersant in a mass ratio of 60-70:30-40:2-5, and then combines with a release paper coating machine to implement a three-coating method. After the three-coating method is completed, it is processed by a rubber roller machine including a roller machine end for pressing the laminated microfiber base cloth with the semi-dry silicone three-times and a driving speed-changing end for adjusting the running speed of the roller machine end, thereby achieving stepless speed regulation, avoiding the generation of volatile harmful gases and pollution and damage to the environment, and significantly improving the overall wear resistance and service life of the environmentally friendly silicone leather obtained by the production process of the environmentally friendly silicone leather.
[0065] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods or devices.
[0066] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0067] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A process for producing environmentally friendly silicone leather, characterized in that: The invention comprises adopting liquid silicone rubber as raw material and a release paper coating machine to implement a three-layer coating method; the three-layer coating method comprises a first surface coating, a second intermediate layer and three primer coatings; wherein the first surface coating comprises coating a layer of silicone on the release paper in a gap, and then drying the layer of silicone coated on the release paper in a heated thermal oil oven; the second intermediate layer comprises coating two layers of silicone on the release paper treated with the first surface coating, and then drying the two layers of silicone coated on the release paper in a heated thermal oil oven; the three primer coatings comprises coating three layers of silicone on the release paper treated with the second intermediate layer, and then drying the three layers of silicone on the release paper to a semi-dry state in a heated thermal oil oven, so that the microfiber primer coating is The cloth is laminated with three layers of semi-dry silicone rubber and subjected to a pressure treatment by a rubber roller machine, and finally placed in a curing room until fully cured; the liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1; the component A includes hydroxyl-terminated polydimethylsiloxane and silicon dioxide in a mass ratio of 3:2; the component B includes silicone oil, color powder and dispersant in a mass ratio of 60-70:30-40:2-5; the two layers of silicone rubber also include expanded microspheres with a mass fraction of 0.5-2%, and the particle size of the expanded microspheres is 80-120μm; and the two layers of silicone rubber include a pretreatment process, and the pretreatment process is pre-baking at 100-120℃ for 60-90s; wherein: The rubber roller machine comprises a roller machine end (1) for pressing the laminated microfiber base fabric with three-times semi-dry silicone and a drive speed-changing end (2) for adjusting the running speed of the roller machine end (1); the roller machine end (1) comprises two rubber rollers (12) and two roller machine frames (11) respectively located at the two ends of the rubber rollers (12) and rotatably connected; the same end of the two rubber rollers (12) is provided with a mutually meshing connecting gear (13), and one of the rubber rollers (12) is connected to the drive speed-changing end (2); The driving speed-changing end (2) comprises a driving shaft (24) coaxially connected to the corresponding rubber roller (12), two speed-changing frames (21) respectively connected to the two ends of the driving shaft (24) for rotation, and a horizontal linear moving unit; the outer peripheral side wall of the driving shaft (24) is provided with a limiting ridge (241) along the axial direction, and is sleeved with a friction wheel (242) matching the limiting ridge (241); the horizontal linear moving unit is used to drive the friction wheel (242) to move axially along the driving shaft (24); the outer peripheral side wall of the friction wheel (242) is provided with a limiting ridge (241) along the axial direction, and is sleeved with a friction wheel (242) matching the limiting ridge (241); the horizontal linear moving unit is used to drive the friction wheel (242) to move axially along the driving shaft (24); The side wall is abutted against a rotating cone (22), the upper side of the rotating cone (22) is horizontal, and the two ends thereof are respectively rotatably connected to the corresponding speed change frame (21), and the speed change frame (21) is provided with a uniform speed motor (23) for driving the rotating cone (22) to perform uniform circumferential rotational motion with its axis as the axis; the horizontal linear moving unit comprises a speed regulating frame (211) connected and fixed to the corresponding speed change frame (21), a double-headed screw (25) plugged into the speed regulating frame (211) in a vertical direction, and a double-headed screw (25) for driving the double-headed screw (25) a stepper motor (26) that is rotated and fixed on the speed regulating stand (211); the upper and lower ends of the double-headed screw rod (25) are threadedly connected with lifting thread blocks (28) that are symmetrically distributed up and down, and the lifting thread blocks (28) are connected to the transfer swing arms (29) for rotation up and down, and the ends of the two transfer swing arms (29) away from the corresponding lifting thread blocks (28) are simultaneously connected to the same lateral push part (27) for rotation up and down, and the lateral push part (27) is provided with two push plates (271) that are respectively in contact with the side surfaces of the friction wheel (242).
2. The process for producing environmentally friendly silicone leather according to claim 1, characterized in that: In the one-time surface coating, the thickness of a layer of silica gel is 0.01-0.02 mm, the coating speed is 6 m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140-160° C., and the drying time is 1.5 min.
3. The process for producing environmentally friendly silicone leather according to claim 1, characterized in that: In the secondary intermediate layer, the thickness of the two layers of silica gel is 0.2-0.25 mm, the coating speed is 6 m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 140-160° C., and the drying time is 1.5 min.
4. The process for producing environmentally friendly silicone leather according to claim 1, characterized in that: In the three primer coatings, the thickness of the three layers of silicone is 0.3-0.35 mm, the coating speed is 6 m / min, and the coating temperature is room temperature; and the drying temperature of the thermal oil oven is 80°C for the first stage, 100°C for the second stage, 120°C for the third stage, 140°C for the fourth stage and 160°C for the fifth stage, and the drying time is 3 minutes.
5. The process for producing environmentally friendly silicone leather according to claim 1, characterized in that: A limiting column (214) is arranged between the two speed change frames (21) and penetrates the lateral push portion (27) along the axial direction of the active rotating shaft (24); a positioning intermediate body (251) is arranged in the middle of the double-headed screw (25); and a cone top matching body (212) and a cone bottom matching body (213) matching with a corresponding end of the rotating cone (22) are respectively arranged on opposite sides of the two speed change frames (21).