A method for preparing ultrafine nano silver wires under aqueous solution system conditions

Through the hydrothermal method in the aqueous solution system, the nucleation and growth rate of silver halide were controlled, and ultrafine nano silver wires with a diameter of 25nm to 40nm were prepared, which solved the problems of high costs and environmental pollution in the existing technology, and achieved high levels of Compatibility of conductivity and high light transmittance, suitable for the preparation of flexible optoelectronic devices.

CN115673335BActive Publication Date: 2024-11-01NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211483772.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-11-01
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

The prior art uses polyol method when preparing nano silver wires, resulting in high production costs and environmental pollution, and it is difficult to obtain low-diameter nano silver wires with a diameter of less than 100 nm, which cannot meet the high requirements of flexible optoelectronic devices for conductivity and light transmission. .

Method used

By using the hydrothermal method in the aqueous solution system, the nucleation, growth and reduction rate of silver halide is controlled, and reducing sugars and polyvinylpyrrolidone are used as structural guides to generate ultrafine nano silver with a diameter of 25nm to 40nm and a length of more than 160μm. Line, achieving compatibility with high conductivity and high light transmittance.

Benefits of technology

It realizes low-cost, environmentally friendly ultrafine nano silver wire preparation, has good mechanical flexibility and high light transmittance, and is suitable for the preparation of transparent conductive films and flexible optoelectronic devices, reducing the number of subsequent washings and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115673335B_ABST
    Figure CN115673335B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing ultrafine nano silver wires in an aqueous solution system, comprising the following steps: 1. dissolving reducing sugar and polyvinyl pyrrolidone in deionized water to obtain a mixed solution; 2. adding a halide solution to the mixed solution, and then adding a silver nitrate solution, stirring to obtain a milky suspension solution; 3. pouring the milky suspension solution into a hydrothermal reactor, performing a hydrothermal reaction, and obtaining a product; 4. centrifuging and washing the product to obtain an ultrafine nano silver wire. The invention adopts a hydrothermal method to synthesize ultrafine nano silver wires, and the whole process adopts an aqueous solution system, which only requires a one-pot method, and obtains ultrafine nano silver wires by controlling the nucleation, growth and reduction rates of silver halide. The obtained ultrafine nano silver wires have a small diameter, a high aspect ratio, good mechanical flexibility, and can achieve high conductivity and high transmittance compatibility. They are ideal materials for preparing transparent conductive films and can be widely used in various flexible optoelectronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flexible electronics, and in particular relates to a method for preparing ultrafine nano silver wires under aqueous solution system conditions. Background Art

[0002] Transparent conductive film (TCF) refers to a film with a visible light transmittance greater than 80% and a resistivity less than 10 -3 Ω·m thin film. Because of its high transmittance to visible light and low resistivity, it can be used to prepare a variety of optoelectronic devices, such as solar cells, light-emitting diodes (LEDs), touch screens, supercapacitors, etc. Indium tin oxide (ITO) has high electrical conductivity and optical transparency and is a commonly used traditional conductive film material. However, with the development of optoelectronic devices towards flexibility, low cost and intelligence, the defects of ITO such as high brittleness, high cost and the use of toxic materials have become increasingly prominent, resulting in its inability to meet the current development of transparent conductive film materials and optoelectronic devices. In contrast, nanosilver wires, as one-dimensional nanomaterials with good light transmittance, conductivity and stability, as a transparent conductive film made of conductive materials, have the advantages of low square resistance, good bendability, high light transmittance, simple process and easy access to raw materials, which meet the preparation requirements of flexible and intelligent optoelectronic devices. Therefore, nanosilver wires are a strong alternative to ITO and a key research and development direction in the field of transparent conductive films.

[0003] At present, the commercial preparation of silver nanowires generally uses the polyol method. This method can control the diameter of silver nanowires, but a large amount of polyol organic solvents are used in the preparation process. Toluene, acetone and other organic reagents may also be used in the subsequent separation and purification process, which increases production costs and is harmful to the human body. Therefore, it is necessary to find a technology with lower cost and simpler operation to solve the problems brought about by the above method. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing ultrafine nano silver wires under aqueous solution system conditions in view of the deficiencies of the above-mentioned prior art. The method adopts a hydrothermal method to synthesize ultrafine nano silver wires, and adopts an aqueous solution system to implement the whole process. By controlling the nucleation, growth and reduction rates of silver halide, ultrafine nano silver wires with a diameter of 25nm to 40nm, a length of more than 160μm, and an aspect ratio of more than 4000 are obtained. The ultrafine nano silver wires have a small diameter, a high aspect ratio, good mechanical flexibility, and can achieve high conductivity and high transmittance compatibility. It is an ideal material for preparing transparent conductive films and can be widely used in various flexible optoelectronic devices.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing ultrafine nano silver wires under aqueous solution system conditions, characterized in that the method comprises the following steps:

[0006] Step 1, dissolving reducing sugar and polyvinyl pyrrolidone in deionized water, and then stirring to obtain a mixed solution;

[0007] Step 2: Add the halide solution to the mixed solution obtained in step 1, stir, add the silver nitrate solution, and stir again to obtain a milky white suspension solution;

[0008] Step 3: pour the milky white suspension solution obtained in step 2 into a hydrothermal reaction kettle, perform a hydrothermal reaction in an electric heated blast drying oven, and obtain a product in the hydrothermal reaction kettle;

[0009] Step 4: Centrifuge and wash the product obtained in step 3 to obtain ultrafine nano silver wires; the ultrafine nano silver wires have a diameter of 25nm to 40nm, a length of more than 160μm, and an aspect ratio of more than 4000.

[0010] The present invention proposes to prepare nano silver wires in an aqueous solution system to solve the existing problems, but the collision speed between ions in the aqueous solution is fast, the direction and size of crystal growth are more difficult to control, and it is more difficult to obtain nano silver wires with low diameters. At present, the diameter of nano silver wires prepared in an aqueous solution system is usually above 100nm, but the optical properties of flexible devices determine that nano silver wires with low diameters are more in line with the demand, and there are few reports on the preparation of nano silver wires with low diameters in an aqueous solution system, because the preparation of nano silver wires with low diameters is still difficult;

[0011] In view of the above problems, the present invention proposes a new method for preparing ultrafine nano silver wires in an aqueous solution system, wherein a one-dimensional silver halide nanowire precursor is first generated, and then the ultrafine nano silver wire material is obtained by in-situ reduction. The present invention adopts an aqueous solution system, adopts reducing sugar as a reducing agent, and polyvinyl pyrrolidone as a structural directing agent to control the crystal growth direction, adopts a halide as a precipitating agent to generate silver halide as a precursor of the nano silver wire, and adds a silver nitrate solution to the reaction system to immediately generate a silver halide precipitate. Due to the adsorption of silver ions and polyvinyl pyrrolidone, a silver halide nanowire structure is generated under the structural directing effect of polyvinyl pyrrolidone on the nucleation and growth of silver halide crystals. Accompanied by a hydrothermal reaction, the reducing sugar is continuously hydrolyzed, the reducibility of the system is continuously enhanced, and the silver halide is gradually reduced to a one-dimensional nano silver wire, thereby obtaining an ultrafine nano silver wire of a material for preparing a transparent conductive film.

[0012] The method for preparing ultrafine silver nanowires under the conditions of an aqueous solution system is characterized in that the molar ratio of reducing sugar to polyvinyl pyrrolidone in the mixed solution in step 1 is 1:1.03-216.08. In the present invention, polyvinyl pyrrolidone can adsorb silver ions, effectively control the nucleation and growth rate of silver halide crystals, and play an important structural guiding role in one-dimensional silver halide nanowires. Insufficient or excessive amounts of polyvinyl pyrrolidone cannot obtain a single silver nanowire structure.

[0013] The method for preparing ultrafine nano silver wires under the conditions of an aqueous solution system is characterized in that the mass ratio of reducing sugar to deionized water in the mixed solution in step 1 is 1:50 to 333. The concentration of reducing sugar in the present invention has a direct impact on the reduction rate of silver chloride. If the concentration of reducing sugar is too low, the silver halide cannot be completely reduced within the reaction time. If the concentration is too high, the precursor is reduced before it grows into a nanowire structure, and a low-diameter nanowire structure cannot be obtained.

[0014] The method for preparing ultrafine nano silver wires under the conditions of an aqueous solution system is characterized in that the molar ratio of silver nitrate to halide in the milky white suspension solution in step 2 is 1:0.8-6.3. In the present invention, if there is too little halide, silver ion precipitation is insufficient, part of the silver ions will be directly reduced, and particles will exist in the product; if there is too much halide, the excess halide ions will etch the reduced product, resulting in irregular product morphology.

[0015] The method for preparing ultrafine silver nanowires under the conditions of an aqueous solution system is characterized in that the molar ratio of silver nitrate to reducing sugar in the mixed solution in step 2 is 1:0.49-2.97. In the present invention, the amount of reducing sugar has a direct impact on the reducibility of the reaction system. If the amount of reducing sugar is insufficient, the reducibility in the reaction system is insufficient, part of the silver halide cannot be reduced, and silver halide nanowires exist in the product; if the amount of reducing sugar is too much, the reducibility in the reaction system is too strong, the silver halide has been reduced before it is oriented, and the product has an irregular morphology.

[0016] The above-mentioned method for preparing ultrafine silver nanowires under the conditions of an aqueous solution system is characterized in that the reducing sugar described in step 1 includes glucose, fructose, sucrose, lactose, galactose or maltose. In the present invention, the reducing sugars are all weak reducing agents. In the initial reaction, the temperature is low, no hydrolysis reaction occurs, no reducing property, and does not affect the generation of one-dimensional silver halide nanowires. In the hydrothermal reaction, as the temperature rises, the reducing sugar begins to hydrolyze and then shows a certain reducing property, reducing the one-dimensional silver halide nanowires to nanosilver wires.

[0017] The method for preparing ultrafine silver nanowires under the conditions of an aqueous solution system is characterized in that the halide in step 2 is a metal halide, and the metal halide includes sodium chloride, potassium chloride, sodium bromide or potassium bromide. In the present invention, sodium chloride, potassium chloride, sodium bromide or potassium bromide is used as a precipitant in the system, and the generated halide can produce one-dimensional silver halide nanowires under the action of polyvinyl pyrrolidone, and generate nanosilver wires after reduction; while the precipitation stability produced by other halides is too strong and cannot be reduced by the reducing agent.

[0018] The method for preparing ultrafine nano silver wires under the conditions of an aqueous solution system is characterized in that the stirring time in step 2 is greater than 1 hour. The present invention controls the stirring time of adding silver nitrate solution to be greater than 1 hour after stirring, and controls the stirring time of the milky white suspension solution obtained after stirring again to be greater than 1 hour, thereby ensuring sufficient reaction.

[0019] The method for preparing ultrafine silver nanowires under the conditions of an aqueous solution system is characterized in that the temperature of the hydrothermal reaction in step 2 is 120°C to 170°C and the time is 8h to 20h. In the present invention, the temperature of the hydrothermal reaction is controlled to avoid insufficient reduction due to too low temperature, and the presence of a large number of intermediate products in the product. When the temperature is too high, the reducing sugar is carbonized and some carbon particles are present in the product. The reaction is fully ensured by controlling the time of the hydrothermal reaction.

[0020] The method for preparing ultrafine silver nanowires under the conditions of an aqueous solution system is characterized in that the centrifugal cleaning process in step 3 is: first centrifugation, and then cleaning with deionized water and anhydrous ethanol in sequence. The present invention removes impurities on the surface of the ultrafine silver nanowires by centrifugal cleaning.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] 1. The present invention adopts a hydrothermal method to synthesize ultrafine nano silver wires. An aqueous solution system is used in the whole process. By controlling the nucleation, growth and reduction rates of silver chloride, ultrafine nano silver wires with a diameter of 25nm to 40nm, a length of more than 160μm, and an aspect ratio of more than 4000 are obtained. The ultrafine nano silver wires have a small diameter, a high aspect ratio, good mechanical flexibility, and can achieve compatibility between high conductivity and high transmittance. They are an ideal material for preparing transparent conductive films and can be widely used in various flexible optoelectronic devices.

[0023] 2. The present invention uses water as a solvent to participate in the reaction, which can effectively avoid the pollution of the environment caused by organic solvents. At the same time, the product obtained from the aqueous solution system is easy to wash, which can effectively reduce the number of subsequent washing times compared with the polyol preparation technology.

[0024] 3. The present invention can prepare ultrafine nano silver wires in a one-pot process, the method is simple to operate, the process parameters are controllable, the repeatability is high, the preparation process cost is low, and it is suitable for large-scale production.

[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a high-magnification SEM image of the ultrafine nanosilver wire prepared in Example 1 of the present invention.

[0027] Figure 2 This is a low-magnification SEM image of the ultrafine nanosilver wire prepared in Example 1 of the present invention.

[0028] Figure 3 This is a high-magnification SEM image of the ultrafine nanosilver wire prepared in Example 2 of the present invention.

[0029] Figure 4 This is a medium magnification SEM image of the ultrafine nanosilver wire prepared in Example 2 of the present invention.

[0030] Figure 5 This is a low-magnification SEM image of the ultrafine nanosilver wire prepared in Example 2 of the present invention.

[0031] Figure 6 3 is the XRD diagram of the ultrafine nano silver wire prepared in Example 2 of the present invention.

[0032] Figure 7 This is a high-magnification SEM image of the ultrafine nanosilver wire prepared in Example 3 of the present invention.

[0033] Figure 8 This is a low-magnification SEM image of the ultrafine nanosilver wire prepared in Example 3 of the present invention.

[0034] Fig. 9 This is a high-magnification SEM image of the ultrafine nanosilver wire prepared in Example 4 of the present invention.

[0035] Fig.10 This is a low-magnification SEM image of the ultrafine nanosilver wire prepared in Example 4 of the present invention.

[0036] Fig.11 This is a high-magnification SEM image of the ultrafine nanosilver wire prepared in Example 5 of the present invention.

[0037] Fig.12 This is a low-magnification SEM image of the ultrafine nanosilver wire prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0038] Example 1

[0039] This embodiment includes the following steps:

[0040] Step 1, dissolving 0.6 g lactose and 12.5 g polyvinyl pyrrolidone in 60 ml deionized water, and then stirring to obtain a mixed solution;

[0041] Step 2: Add 3.6 mmol of sodium chloride solution to the mixed solution obtained in step 1, stir for 1 hour, add 0.6 mmol of silver nitrate solution, and stir again for 1 hour to obtain a milky white suspension solution;

[0042] Step 3: Pour the milky white suspension solution obtained in step 2 into a hydrothermal reaction kettle, and heat it in an electric blast drying oven at 170° C. for 8 h to perform a hydrothermal reaction to obtain a product in the hydrothermal reaction kettle;

[0043] Step 4: Centrifuge the product obtained in step 3, and then wash it with deionized water and anhydrous ethanol in turn to obtain ultrafine nano silver wires.

[0044] Figure 1 is a high-magnification SEM image of the ultrafine silver nanowire prepared in this embodiment. Figure 2 is a low-magnification SEM image of the ultrafine silver nanowires prepared in this embodiment. Figure 1 and Figure 2 It can be seen that the diameter of the ultrafine nanosilver wire is about 50nm, the length is more than 160μm, the aspect ratio is more than 1000, and the wire diameter is relatively uniform.

[0045] Example 2

[0046] This embodiment includes the following steps:

[0047] Step 1, dissolving 3.5 g maltose and 50 g polyvinyl pyrrolidone in 200 ml deionized water, and then stirring to obtain a mixed solution;

[0048] Step 2: Add 21 mmol of sodium chloride solution to the mixed solution obtained in step 1, stir for 1 hour, add 5.8 mmol of silver nitrate solution, and stir again for 1 hour to obtain a milky white suspension solution;

[0049] Step 3: Pour the milky white suspension solution obtained in step 2 into a hydrothermal reaction kettle, and heat it in an electric blast drying oven at 140° C. for 18 hours to perform a hydrothermal reaction to obtain a product in the hydrothermal reaction kettle;

[0050] Step 4: Centrifuge the product obtained in step 3, and then wash it with deionized water and anhydrous ethanol in turn to obtain ultrafine nano silver wires.

[0051] According to the test, the ultrafine silver nanowire prepared in this embodiment has a diameter of 30 nm, a length of more than 160 μm, and an aspect ratio of more than 4000.

[0052] Figure 3 is a high-magnification SEM image of the ultrafine silver nanowire prepared in this embodiment. Figure 4 This is a medium magnification SEM image of the ultrafine silver nanowire prepared in this example. Figure 5 is a low-magnification SEM image of the ultrafine silver nanowires prepared in this embodiment. Figure 3 to Figure 5 It can be seen that the diameter of the ultrafine nanosilver wire is about 30nm, the aspect ratio exceeds 4000, and the wire diameter is relatively uniform.

[0053] Figure 6 is the XRD pattern of the ultrafine silver nanowire prepared in this embodiment. Figure 6 It can be seen that the ultrafine nanosilver wire prepared in this embodiment has good crystallinity, a face-centered cubic structure, and no other impurities.

[0054] Example 3

[0055] This embodiment includes the following steps:

[0056] Step 1, dissolving 3 g of maltose and 6 g of polyvinyl pyrrolidone in 300 ml of deionized water, and then stirring to obtain a mixed solution;

[0057] Step 2: Add 17 mmol potassium bromide solution to the mixed solution obtained in step 1, stir for 1 hour, add 14 mmol silver nitrate solution, and stir again for 1 hour to obtain a milky white suspension solution;

[0058] Step 3: Pour the milky white suspension solution obtained in step 2 into a hydrothermal reaction kettle, and heat it in an electric blast drying oven at 120° C. for 20 h to perform a hydrothermal reaction to obtain a product in the hydrothermal reaction kettle;

[0059] Step 4: Centrifuge the product obtained in step 3, and then wash it with deionized water and anhydrous ethanol in turn to obtain ultrafine nano silver wires.

[0060] According to the test, the ultrafine silver nanowire prepared in this embodiment has a diameter of 25 nm to 40 nm, a length of more than 160 μm, and an aspect ratio of more than 4000.

[0061] Figure 7 is a high-magnification SEM image of the ultrafine silver nanowire prepared in this embodiment. Figure 8 is a low-magnification SEM image of the ultrafine silver nanowires prepared in this embodiment. Figure 7 and Figure 8 It can be seen that the diameter of the ultrafine nano silver wire prepared in this embodiment is about 60 nm, the aspect ratio is more than 1000, and the wire diameter is uniform.

[0062] Example 4

[0063] This embodiment includes the following steps:

[0064] Step 1, dissolving 0.9 g of glucose and 30 g of polyvinyl pyrrolidone in 100 ml of deionized water, and then stirring to obtain a mixed solution;

[0065] Step 2: Add 9 mmol of sodium bromide solution to the mixed solution obtained in step 1, stir for 1 hour, then add 6 mmol of silver nitrate solution, and stir again for 1 hour to obtain a milky white suspension solution;

[0066] Step 3: Pour the milky white suspension solution obtained in step 2 into a hydrothermal reaction kettle, and heat it in an electric blast drying oven at 150° C. for 15 h to perform a hydrothermal reaction to obtain a product in the hydrothermal reaction kettle;

[0067] Step 4: Centrifuge the product obtained in step 3, and then wash it with deionized water and anhydrous ethanol in turn to obtain ultrafine nano silver wires.

[0068] According to the test, the ultrafine silver nanowire prepared in this embodiment has a diameter of 25 nm to 40 nm, a length of more than 160 μm, and an aspect ratio of more than 4000.

[0069] Fig. 9 is a high-magnification SEM image of the ultrafine silver nanowire prepared in this embodiment. Fig.10 is a low-magnification SEM image of the ultrafine silver nanowires prepared in this embodiment. Fig. 9 and Fig.10 It can be seen that the diameter of the ultrafine nano silver wire prepared in this embodiment is about 40 nm, the aspect ratio is more than 2000, and the wire diameter is uniform.

[0070] Example 5

[0071] This embodiment includes the following steps:

[0072] Step 1, dissolving 0.6 g of fructose and 3.6 g of polyvinyl pyrrolidone in 60 ml of deionized water, and then stirring to obtain a mixed solution;

[0073] Step 2: Add 0.76 mmol potassium chloride solution to the mixed solution obtained in step 1, stir for 1 hour, add 0.6 mmol silver nitrate solution, and stir again for 1 hour to obtain a milky white suspension solution;

[0074] Step 3: Pour the milky white suspension solution obtained in step 2 into a hydrothermal reaction kettle, and heat it in an electric blast drying oven at 160° C. for 12 h to perform a hydrothermal reaction to obtain a product in the hydrothermal reaction kettle;

[0075] Step 4: Centrifuge the product obtained in step 3, and then wash it with deionized water and anhydrous ethanol in turn to obtain ultrafine nano silver wires.

[0076] According to the test, the ultrafine silver nanowire prepared in this embodiment has a diameter of 25 nm to 40 nm, a length of more than 160 μm, and an aspect ratio of more than 4000.

[0077] Fig.11 is a high-magnification SEM image of the ultrafine silver nanowire prepared in this embodiment. Fig.12 is a low-magnification SEM image of the ultrafine silver nanowires prepared in this embodiment. Fig.11 and Fig.12 It can be seen that the diameter of the ultrafine nano silver wire prepared in this embodiment is about 40 nm, the aspect ratio is more than 2000, and the wire diameter is uniform.

[0078] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing ultrafine nano silver wires under aqueous solution conditions, characterized in that: The method comprises the following steps: Step 1, dissolving reducing sugar and polyvinyl pyrrolidone in deionized water, and then stirring to obtain a mixed solution; Step 2: Add the halide solution to the mixed solution obtained in step 1, add the silver nitrate solution after stirring, and stir again to obtain a milky white suspension solution; the stirring time is greater than 1 hour; Step 3: pour the milky white suspension solution obtained in step 2 into a hydrothermal reaction kettle, perform a hydrothermal reaction in an electric heated blast drying oven, and obtain a product in the hydrothermal reaction kettle; the temperature of the hydrothermal reaction is 120° C. to 170° C., and the time is 8 h to 20 h; Step 4: Centrifuge and wash the product obtained in step 3 to obtain ultrafine nano silver wires; the ultrafine nano silver wires have a diameter of 25nm to 40nm, a length of more than 160μm, and an aspect ratio of more than 4000.

2. The method for preparing ultrafine nano silver wires under aqueous solution system conditions according to claim 1, characterized in that: The molar ratio of reducing sugar to polyvinyl pyrrolidone in the mixed solution in step 1 is 1:1.03-216.

08.

3. The method for preparing ultrafine nano silver wires under aqueous solution system conditions according to claim 1, characterized in that: The mass ratio of reducing sugar to deionized water in the mixed solution in step 1 is 1:50-333.

4. The method for preparing ultrafine nano silver wires under aqueous solution system conditions according to claim 1, characterized in that: The molar ratio of silver nitrate to halide in the milky white suspension solution in step 2 is 1:0.8-6.

3.

5. The method for preparing ultrafine nano silver wires under aqueous solution system conditions according to claim 1, characterized in that: The molar ratio of silver nitrate to reducing sugar in the mixed solution in step 2 is 1:0.49-2.

97.

6. The method for preparing ultrafine nano silver wires under aqueous solution system conditions according to claim 1, characterized in that: The reducing sugar described in step 1 includes glucose, fructose, sucrose, lactose, galactose or maltose.

7. The method for preparing ultrafine nano silver wires under aqueous solution system conditions according to claim 1, characterized in that: The halide in step 2 is a metal halide, and the metal halide includes sodium chloride, potassium chloride, sodium bromide or potassium bromide.

8. The method for preparing ultrafine nano silver wires under aqueous solution system conditions according to claim 1, characterized in that: The process of centrifugal cleaning in step three is: first centrifugation, and then cleaning with deionized water and anhydrous ethanol in sequence.