A wear-resistant and weather-resistant TPU material for casters and preparation method thereof
By introducing modified potassium hexatitate whiskers into the TPU material, the problem of short service life of TPU casters is solved, significantly improving wear and weather resistance, extending service life, and improving performance in harsh environments.
Patent Information
- Application Number
- CN202211082739.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-06
AI Technical Summary
The existing TPU caster materials have a short service life and are not well-resistant and weather-resistant, so they need to be replaced frequently.
Modified potassium hexattitanate whiskers are used as reinforcement and treated with polyester diol, isocyanate, chain extender, antioxidant, lubricant and catalyst in a twin-screw extruder. Synthesize wear-resistant and weather-resistant TPU materials, and use the high tensile strength and infrared emissivity of modified potassium hexatitate whiskers to improve material performance.
It improves the wear resistance of TPU materials by 22% and weather resistance by 19%, extends the service life of casters, and shows higher mechanical properties and weather resistance in harsh environments.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer material synthesis and preparation, and particularly relates to a wear-resistant and weather-resistant TPU material for casters and a preparation method thereof. Background Art
[0002] Thermoplastic polyurethane elastomer materials have the elongation, resilience and mechanical deformation recovery of ordinary elastomers, as well as high tensile strength and elongation at break. Due to the excellent tensile strength, tear resistance, flexibility and wear resistance of thermoplastic polyurethane elastomers, they are widely used in many fields such as automobiles, shoes, films, mobile phone cases, casters, etc.
[0003] At present, casters are classified according to material properties. Conventional materials include PVC, nylon, PU, TPR, rubber and other materials. However, the most environmentally friendly material is PU, and TPU in PU has good mechanical properties and weather resistance. However, the preparation method of TPU caster material is relatively simple. Although the performance of TPU itself can meet the performance of casters in a short time, its service life is short and needs to be replaced frequently. Summary of the invention
[0004] In view of the shortcomings and limitations of existing caster materials, the purpose of the present invention is to provide a wear-resistant and weather-resistant TPU caster material to enhance the wear resistance, weather resistance and service life of the caster. The wear-resistant and weather-resistant TPU caster material of the present invention comprises the following raw materials in parts by weight: 35-70 parts of polyester diol, 23-45 parts of isocyanate, 5-13 parts of chain extender, 0.1-0.3 parts of antioxidant, 0.1-0.3 parts of lubricant, 6-10 parts of modified potassium hexatitanate whisker, and 0.007-0.02 parts of catalyst;
[0005] The modified potassium hexatitanate whisker is obtained by modifying the potassium hexatitanate whisker with a titanate coupling agent.
[0006] Furthermore, the modified potassium hexatitanate whisker is prepared by the following method:
[0007] (1) preparing a titanate coupling agent and water in a mass ratio of 1:(6-8), adding glacial acetic acid to hydrolyze for 1-2 hours, and setting aside; drying the potassium hexatitanate whisker in an oven at 110-120° C. for 2-3 hours, and setting aside;
[0008] (2) adding the titanate coupling agent solution and potassium hexatitanate whiskers obtained in (1) into distilled water, blending, and heating;
[0009] (3) After stirring for 1-2 hours, filtering, drying, and grinding, the modified potassium hexatitanate whiskers are obtained.
[0010] Furthermore, the polyester diol is one or more of polyethylene adipate diol, polyethylene adipate-1,3-propylene glycol ester diol, polyethylene adipate-1,4-butylene glycol ester diol, and polyethylene adipate-1,4-butylene glycol ester diol.
[0011] Furthermore, the polyester diol is preferably polyethylene adipate diol, and the molecular weight of polyethylene adipate diol is 1000-3000.
[0012] Furthermore, the isocyanate is one or more of 4,4'-diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, toluene isocyanate, and phenylene-1,4-diisocyanate.
[0013] Furthermore, the isocyanate is preferably 4,4'-diphenylmethane diisocyanate.
[0014] Furthermore, the chain extender is one or more of ethylene glycol, 1,3-propylene glycol, and 1,4-butanediol.
[0015] Furthermore, the chain extender is preferably 1,4-butanediol.
[0016] Furthermore, the antioxidant is one or more of hindered phenol antioxidants and phosphite antioxidants.
[0017] Furthermore, the antioxidant is preferably pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.
[0018] Furthermore, the lubricant is one or more of glyceryl monostearate, pentaerythritol stearate, montan wax or OP wax.
[0019] Furthermore, the lubricant is preferably montan wax.
[0020] Furthermore, the catalyst is one or more of organic bismuth, organic tin, and titanate catalysts.
[0021] Furthermore, the catalyst is preferably an organic bismuth catalyst.
[0022] Furthermore, a method for preparing a wear-resistant and weather-resistant TPU material for casters comprises the following steps:
[0023] (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker, and catalyst into reactor A and mixing, placing isocyanate into reactor B, and placing chain extender into reactor C;
[0024] (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer.
[0025] Furthermore, it is characterized in that: the temperature of the reactor A is 90-120°C, the temperature of the reactor B is 70-90°C, and the temperature of the reactor C is 70-90°C; the temperature of the twin-screw extruder is 120-210°C, and the rotation speed is 180-240r / min.
[0026] Potassium hexatitanate whiskers are used as reinforcements for composite materials. They have few internal defects, extremely high tensile strength and elastic modulus, high infrared emissivity, and are wear and corrosion resistant. The whiskers have high strength in all dimensions. They are used as a reinforcement phase in casters to improve their wear and weather resistance and service life.
[0027] Potassium hexatitanate whiskers are potassium hexatitanate whiskers modified by titanate coupling agents. Since potassium hexatitanate whiskers have high surface energy, they are difficult to disperse evenly in organic polymers and are prone to agglomeration, so potassium hexatitanate whiskers must be modified.
[0028] The present invention can bring the following beneficial effects:
[0029] 1. The present invention modifies potassium hexatitanate whiskers so that they can be evenly dispersed in polyester diols to avoid agglomeration, thereby making the performance of the TPU caster material finally prepared stable.
[0030] 2. The present invention introduces potassium hexatitanate whiskers into TPU. Due to the properties of potassium hexatitanate itself, it plays a role of a reinforcing phase in the caster material, and the wear resistance is improved by 22% and the weather resistance is improved by 19%. DETAILED DESCRIPTION
[0031] The present invention will be further described below with reference to specific embodiments.
[0032] Example 1
[0033] The modified potassium hexatitanate whiskers are prepared by the following method:
[0034] (1) titanate coupling agent and water are mixed in a mass ratio of 1:8, and glacial acetic acid is added to hydrolyze for 1 hour, and the mixture is set aside; potassium hexatitanate whiskers are placed in an oven at 110° C. and dried for 2 hours, and the mixture is set aside;
[0035] (2) adding the titanate coupling agent solution and potassium hexatitanate whiskers obtained in (1) into distilled water, blending, and heating;
[0036] (3) After stirring for 1 hour, filtering, drying, and grinding, the modified potassium hexatitanate whiskers are obtained.
[0037] A wear-resistant and weather-resistant TPU material for casters, made from the following raw materials:
[0038]
[0039] The molecular weight of polyethylene adipate diol is 1000.
[0040] The preparation method is as follows: (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker and catalyst into a reaction kettle A and mixing, placing isocyanate into a reaction kettle B, and placing a chain extender into a reaction kettle C;
[0041] (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer; the temperature of reactor A is 100°C, the temperature of reactor B is 90°C, and the temperature of reactor C is 90°C; the temperature of the twin-screw extruder is 190°C, and the speed is 220 r / min.
[0042] Example 2
[0043] The preparation method of the modified potassium hexatitanate whiskers is the same as that in Example 1.
[0044] A wear-resistant and weather-resistant TPU material for casters, made from the following raw materials:
[0045]
[0046] The molecular weight of polyethylene adipate diol is 2,000.
[0047] The preparation method is as follows: (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker and catalyst into a reaction kettle A and mixing, placing isocyanate into a reaction kettle B, and placing a chain extender into a reaction kettle C;
[0048] (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer; the temperature of reactor A is 110°C, the temperature of reactor B is 80°C, and the temperature of reactor C is 90°C; the temperature of the twin-screw extruder is 180°C, and the speed is 210 r / min.
[0049] Example 3
[0050] The preparation method of the modified potassium hexatitanate whiskers is the same as that in Example 1.
[0051] A wear-resistant and weather-resistant TPU material for casters, made from the following raw materials:
[0052]
[0053] The molecular weight of polyethylene adipate diol is 3,000.
[0054] The preparation method is as follows: (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker and catalyst into a reaction kettle A and mixing, placing isocyanate into a reaction kettle B, and placing a chain extender into a reaction kettle C;
[0055] (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer; the temperature of reactor A is 120°C, the temperature of reactor B is 85°C, and the temperature of reactor C is 85°C; the temperature of the twin-screw extruder is 205°C, and the speed is 200 r / min.
[0056] Comparative Example 1
[0057] A wear-resistant and weather-resistant TPU material for casters, made from the following raw materials:
[0058]
[0059] The molecular weight of polyethylene adipate diol is 1000.
[0060] The preparation method is as follows: (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker and catalyst into a reaction kettle A and mixing, placing isocyanate into a reaction kettle B, and placing a chain extender into a reaction kettle C;
[0061] (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer; the temperature of reactor A is 110°C, the temperature of reactor B is 85°C, and the temperature of reactor C is 90°C; the temperature of the twin-screw extruder is 200°C, and the rotation speed is 210 r / min.
[0062] Comparative Example 2
[0063] A wear-resistant and weather-resistant TPU material for casters, made from the following raw materials:
[0064]
[0065] The molecular weight of polyethylene adipate diol is 2,000.
[0066] The preparation method is as follows: (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker and catalyst into a reaction kettle A and mixing, placing isocyanate into a reaction kettle B, and placing a chain extender into a reaction kettle C;
[0067] (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer; the temperature of reactor A is 100°C, the temperature of reactor B is 90°C, and the temperature of reactor C is 90°C; the temperature of the twin-screw extruder is 180°C, and the speed is 200 r / min.
[0068] Comparative Example 3
[0069] A wear-resistant and weather-resistant TPU material for casters, made from the following raw materials:
[0070]
[0071] The molecular weight of polyethylene adipate diol is 3,000.
[0072] The preparation method is as follows: (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker and catalyst into a reaction kettle A and mixing, placing isocyanate into a reaction kettle B, and placing a chain extender into a reaction kettle C;
[0073] (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer; the temperature of reactor A is 100°C, the temperature of reactor B is 80°C, and the temperature of reactor C is 90°C; the temperature of the twin-screw extruder is 190°C, and the speed is 220 r / min.
[0074] Table 1 Surface energy comparison of potassium hexatitanate whiskers before and after modification (23°C)
[0075]
[0076] It can be seen from the table that the surface energy of the modified potassium hexatitanate whiskers changes from 71 to 49, which is significantly reduced. The titanate coupling agent coated on the surface changes its surface properties, and the polarity component also decreases from 50 to 10. After the modified potassium titanate whiskers are added, there is no obvious agglomeration phenomenon in the polyester diol. From the microscopic and macroscopic perspectives, the solubility of the modified potassium hexatitanate whiskers in the organic polymer matrix is greatly improved.
[0077] Table 2 Test results of caster materials prepared in Examples 1-3 and Comparative Examples 1-3
[0078] Test items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Hardness(Shore A) 98 83 95 98 83 95 Tensile strength(MPa) 42.9 39.1 41.3 38.4 36.3 37.2 <![CDATA[DIN wear / mm 3 > 55 58 54 70 71 74 Yellowing resistance level (3 months) 4.5 4.6 4.7 3.8 3.7 3.9
[0079] From the comparative results of the above embodiments, the higher the hardness, the lower the DIN wear; for materials with similar hardness, the materials with modified potassium hexatitanate whiskers have lower DIN wear than those without DIN wear, and the materials with modified potassium hexatitanate whiskers have higher yellowing resistance. For Example 1 and Comparative Example 1, the introduction of modified potassium hexatitanate whiskers improves the tensile strength of the caster material, the wear resistance is improved by 21%, and the weather resistance is improved by 18%, which improves the mechanical properties and weather resistance of the caster material and can extend the service life of the caster material under relatively harsh environmental conditions.
[0080] The above are all preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may also have different changes and modifications. All corresponding modifications made within the principles and spirit of the present invention shall be included in the protection scope of the present invention. The protection scope required by the present invention shall be based on the content of its claims, and the specific implementation methods and other records in the specification may be used to interpret the content of the claims.
Claims
1. A wear-resistant and weather-resistant TPU material for casters, It is characterized in that The method comprises the following raw materials in parts by weight: 35-70 parts of polyester diol, 23-45 parts of isocyanate, 5-13 parts of chain extender, 0.1-0.3 parts of antioxidant, 0.1-0.3 parts of lubricant, 6-10 parts of modified potassium hexatitanate whisker, and 0.007-0.02 parts of catalyst; The modified potassium hexatitanate whisker is obtained by modifying the potassium hexatitanate whisker with a titanate coupling agent; The modified potassium hexatitanate whisker is prepared by the following method: (1) preparing a titanate coupling agent and water in a mass ratio of 1:(6-8), adding glacial acetic acid to hydrolyze for 1-2 hours, and setting aside; drying the potassium hexatitanate whisker in an oven at 110-120° C. for 2-3 hours, and setting aside; (2) adding the titanate coupling agent solution and potassium hexatitanate whiskers obtained in (1) into distilled water, blending, and heating; (3) After stirring for 1-2 hours, filtering, drying, and grinding, the modified potassium hexatitanate whiskers are obtained.
2. The wear-resistant and weather-resistant TPU material for casters according to claim 1, Features: The polyester diol is one or more of polyethylene adipate diol, polyethylene adipate-1,3-propylene glycol ester diol, polyethylene adipate-1,4-butylene glycol ester diol, and polyethylene adipate-1,4-butylene glycol ester diol.
3. The wear-resistant and weather-resistant TPU material for casters according to claim 1, Features: The isocyanate is one or more of 4,4'-diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, toluene isocyanate, and phenylene-1,4-diisocyanate.
4. The wear-resistant and weather-resistant TPU material for casters according to claim 1, Features: The chain extender is one or more of ethylene glycol, 1,3-propylene glycol, and 1,4-butanediol.
5. The wear-resistant and weather-resistant TPU material for casters according to claim 1, Features: The antioxidant is one or more of hindered phenol antioxidants and phosphite antioxidants.
6. The wear-resistant and weather-resistant TPU material for casters according to claim 1, Features: The lubricant is one or more of glyceryl monostearate, pentaerythritol stearate, montan wax or OP wax.
7. The wear-resistant and weather-resistant TPU material for casters according to claim 1, Features: The catalyst is one or more of organic bismuth, organic tin and titanate catalysts.
8. The method for preparing the wear-resistant and weather-resistant TPU material for casters according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) adding polyester diol, lubricant, antioxidant, modified potassium hexatitanate whisker, and catalyst into reactor A and mixing, placing isocyanate into reactor B, and placing chain extender into reactor C; (2) The raw materials in reactors A, B, and C are injected into the feeding port of a twin-screw extruder through a metered pouring system, reacted and plasticized in the twin-screw extruder, and cut into elliptical particles by an underwater pelletizer.
9. The method for preparing the wear-resistant and weather-resistant TPU material for casters according to claim 8, Features: The temperature of the reactor A is 90-120° C., the temperature of the reactor B is 70-90° C., and the temperature of the reactor C is 70-90° C.; the temperature of the twin-screw extruder is 120-210° C., and the rotation speed is 180-240 r / min.
Citation Information
Patent Citations
Crystal whisker reinforced poly(ether-ether-ketone) composite material and preparation method thereof
CN105504763A
Polyetheretherketone cable material and preparation method thereof
CN107674374A
High-weather-resistance ultra-transparent thermoplastic polyurethane elastomer and preparation method thereof
CN111548472A
Thermoplastic polyester elastomer resin composition
JP2007146076A