Addition reaction curing type organopolysiloxane composition, release paper and release film
By adding polyalkenyl and (meth)acrylic acid groups to organopolysiloxane, and using a low amount of platinum catalyst, combined with organohydrogenpolysiloxane, the problems of excessive platinum catalyst amount and insufficient hardening are solved, achieving It achieves low-cost, efficient hardening effects and maintains the integrity of the hardening reaction on catalyst-poisoned substrates.
Patent Information
- Application Number
- CN202180040771.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-03
AI Technical Summary
In the prior art, the amount of platinum catalyst is too much and it is difficult to achieve sufficient hardening at low platinum concentrations, resulting in insufficient hardened film, reduced peeling force, and difficulty in hardening reactions on substrates containing catalyst poison components.
In the addition reaction curable organopolysiloxane composition, an organopolysiloxane containing two or more silicon atoms bonded to an alkenyl group has an average of 0.01 to 2.9 (meth)acrylic acid groups, and is used relative to The total mass of the platinum group metal catalyst is 1 to 100 ppm by mass, and it is combined with the Si-H group of the organohydrogenpolysiloxane to perform addition reaction and hardening.
It achieves full hardening at a low platinum concentration, forms a hardened film with the same peeling force, reduces manufacturing costs, and can fully harden even on substrates containing catalyst poisons.
Smart Images

Figure GDA0003983165900000201 
Figure GDA0003983165900000211
Abstract
Description
Technical Field
[0001] The present invention relates to an addition reaction-curable organopolysiloxane composition that can be cured with a small amount of a platinum catalyst. More specifically, the present invention provides an addition reaction-curable organopolysiloxane composition that provides a cured film for release paper and a release film. Background Art
[0002] Conventionally, in order to prevent adhesion and fixation between sheet substrates such as paper or plastic and adhesive materials, a hardened film of an organopolysiloxane composition is formed on the substrate surface to impart peeling properties. As a method for forming a hardened organopolysiloxane film on a substrate surface, the methods described in the following Patent Documents 1 to 3 are known.
[0003] (1) A method of forming a peelable film by addition-reacting an alkenyl-containing organopolysiloxane with an organohydrogenpolysiloxane using a platinum-based compound as a catalyst (Patent Document 1: Japanese Patent Application Laid-Open No. 47-32072)
[0004] (2) A method of forming a peelable film by condensing an organopolysiloxane having a functional group such as a hydroxyl group or an alkoxy group using an organic metal salt as a catalyst (Patent Document 2: Japanese Patent Publication No. 35-13709)
[0005] (3) A method of forming a peelable film by using ultraviolet rays or electron beams to radically polymerize an acrylic group-containing organopolysiloxane and a photoreaction initiator (Patent Document 3: Japanese Patent Application Laid-Open No. 54-162787)
[0006] Among the above, (1) the platinum catalyst described in Patent Document 1 has excellent hardening properties and can meet various requirements for peeling properties from low-speed peeling to high-speed peeling. Therefore, the platinum catalyst is widely used in the method of forming a peelable film by an addition reaction.
[0007] Previously, the amount of platinum group metal catalyst contained in the organopolysiloxane composition for release paper or release film was mostly 60 mass ppm to 400 mass ppm in terms of platinum group metal concentration. When the platinum concentration is lower than the lower limit, the curing reaction cannot be fully carried out, and the hardened film becomes soft. In addition, the amount of residual Si-H groups increases, and the peeling force increases. In addition, the unreacted raw material organopolysiloxane exists and becomes a transfer component, so the organopolysiloxane may be transferred to the adhesive surface attached to the release paper, thereby causing a decrease in adhesion.
[0008] Furthermore, platinum group metals are rare and precious metals, so they are expensive, and platinum catalysts account for a large proportion of the cost of manufacturing release paper or release film. Therefore, reducing platinum group metal catalysts is related to price reduction. In addition, there are also substrates containing nitrogen compounds, sulfur compounds, phosphorus compounds and other components that become catalyst poisons for platinum group metal catalysts. The catalyst poison components may bond with platinum group metals, making it impossible to harden by addition reaction.
[0009] Therefore, a method for forming a peelable film with a small amount of platinum is required. For example, Patent Documents 4 and 5 describe the following composition.
[0010] (4) A silicone composition comprising a polyorganosiloxane having at least two alkenyl groups bonded to silicon atoms per molecule, a hydrogenated organosiloxane having SiHH groups at the ends and in the side chains, and an MD as an adhesion regulating system. Vi Q resin and hydrosilylation inhibitor (wherein M is R 3 SiO 1 / 2 , D Vi RPSiO 2 / 2 , Q is SiO 4 / 2 , R are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and having no aliphatic unsaturated bonds, and P is -(CH 2 ) n -CH=CH 2 (n is an integer of 0 to 6)) (Patent Document 4: Japanese Patent No. 4221300)
[0011] (5) A release coating composition comprising an alkenyl functionalized polysiloxane, a silicon hydride functionalized polysiloxane, and a platinum group metal, wherein the alkenyl functionalized polysiloxane is prepared using a phosphazene base catalyst. (Patent Document 5: Japanese Patent Publication No. 2009-513740)
[0012] However, the compositions described in Patent Documents 4 and 5 do not sufficiently harden as described below.
[0013] For example, the composition described in Patent Document 4 uses a terminal SiHH group with good reactivity and a film-forming MD Vi In the examples, the Q resin was cured by heating the composition at 150°C for 1.8 seconds at a platinum concentration of 60 ppm, but there is no description of a method for curing with a platinum amount of less than 60 ppm. In addition, the extracted component (amount of unreacted siloxane) in the cured film cured at a platinum concentration of 60 ppm was as high as 5.8% to 6.5%, and a large amount of uncured siloxane existed, resulting in insufficient curing. In addition, Patent Document 4 does not describe the peeling properties.
[0014] In the composition described in Patent Document 5, the alkenyl functionalized polysiloxane is a branched siloxane having an MDQ unit. It is described that the probability of producing a cross-linked film is increased by a branched chain having a terminal vinyl group. In the example described in Patent Document 5, tetrakis-dimethylvinylsiloxysilane is reacted with a phosphazene catalyst to synthesize an alkenyl-containing branched siloxane, and then a silhydride functionalized polysiloxane and a platinum catalyst are prepared at a platinum concentration of 40 ppm, and the composition is cured at 100°C for 15 seconds and 115°C for 20 seconds. In Patent Document 5, the cured state of the composition is evaluated by extracting the cured product with methyl isobutyl ketone. The proportion of unreacted siloxane extracted is 6.4% to 25.2%, which is relatively large, and the curing is insufficient. In addition, other evaluations such as peeling properties were not performed.
[0015] Prior art literature
[0016] Patent Literature
[0017] Patent Document 1: Japanese Patent Publication No. 47-32072
[0018] Patent Document 2: Japanese Patent Publication No. 35-13709
[0019] Patent Document 3: Japanese Patent Publication No. 54-162787
[0020] Patent Document 4: Japanese Patent No. 4221300
[0021] Patent Document 5: Japanese Patent Publication No. 2009-513740 Summary of the invention
[0022] Problems to be solved by the invention
[0023] In a film that has been fully cured, the amount of unreacted siloxane extracted is generally at least 5% or less, preferably 3% or less. As described in Patent Documents 4 and 5, when there is more than 5% unreacted siloxane in the cured film, the siloxane is transferred to the surface of the glue, and the residual adhesion rate is greatly reduced. In addition, since there are many residual SiH groups, the peeling force becomes higher than in the case of full cure. Therefore, an organopolysiloxane composition that can be cured with a small amount of platinum catalyst is needed, but an addition reaction curing type organopolysiloxane composition that can obtain a sufficiently cured film at a platinum concentration of less than 60 mass ppm is not known.
[0024] The present invention is made in view of the above situation, and its purpose is to provide an addition reaction curing type organopolysiloxane composition, which can fully cure even with a small amount of platinum group metal catalyst to exert good adhesion and form a hardened film with the same peeling force as before, and the addition reaction curing also proceeds sufficiently in a substrate containing a catalyst poison component, and is suitable for providing a release film for silicone rubber, release paper or release film.
[0025] Technical means of solving problems
[0026] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by providing an addition reaction-curable organopolysiloxane composition in which the alkenyl-containing organopolysiloxane has two or more silicon-bonded alkenyl groups in one molecule and has an average of 0.01 to 2.9 (meth)acrylic groups, thereby completing the present invention.
[0027] That is, the present invention provides an addition reaction-curable organopolysiloxane composition containing the following components (A) to (C).
[0028] (A) an organopolysiloxane having two or more silicon-bonded alkenyl groups in one molecule and having an average of 0.01 to 2.9 (meth)acrylic groups
[0029] (B) an organohydrogenpolysiloxane having two or more silicon-bonded hydrogen atoms (Si—H groups) in one molecule: an amount in which the ratio of the number of Si—H groups in the component (B) to the number of alkenyl groups in the component (A) is 1 to 5, and
[0030] (C) Platinum group metal catalyst: The content of the platinum group metal is 1 to 100 ppm by mass relative to the total mass of the composition.
[0031] Effects of the Invention
[0032] The organopolysiloxane composition of the present invention can be sufficiently cured to form a cured film having the same peeling force as the conventional addition type composition, although the amount of the platinum group metal catalyst is small. The organopolysiloxane composition of the present invention can be cured even under conditions that were difficult to cure in the past, and the manufacturing cost can be greatly reduced due to the small amount of the platinum group metal catalyst. In addition, even substrates containing catalyst poison can be cured by the addition reaction. DETAILED DESCRIPTION
[0033] Hereinafter, the present invention will be described in detail.
[0034] [(A)Component]
[0035] One molecule of the component (A) has two or more, preferably 2 to 50, silicon-bonded alkenyl groups, and an average of 0.01 to 2.9, preferably 0.03 to 2.7, and more preferably 0.05 to 2.5 (meth)acrylic groups. The organopolysiloxane may be an existing organopolysiloxane, which may be one type alone or two or more types may be appropriately combined. Since the alkenyl-containing organopolysiloxane has a (meth)acrylic group within the above range, it can be cured well even with a small amount of catalyst. The component (A) may be represented by the following average formula (1), for example.
[0036] [Chemistry 1]
[0037] (R 3 SiO 1 / 2 ) a (R 2 PSiO 1 / 2 ) b (R 2 ASiO 1 / 2 ) c (R 2 SiO 2 / 2 ) d (RPSiO 2 / 2 ) e (RASiO 2 / 2 ) f (RSiO 3 / 2 ) g (PSiO 3 / 2 ) h (ASiO 3 / 2 ) i (SiO 4 / 2 ) (1)
[0039] In formula (1), R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and having no aliphatic unsaturated bond, and P is -(CH 2 ) n -CH=CH 2 (n is 0 or a positive number of 0 to 6), wherein A is CH 2 =CR 2 COR 3 - is a (meth)acrylic acid group-containing group, R 2 is a hydrogen atom or a methyl group, R 3 OR 4 or R 4A divalent group, R4 is a divalent organic group having 1 to 20 carbon atoms, which may have a branched or cyclic structure, and may also contain an epoxy group, an ester bond, a urethane bond, an ether bond, an isocyanate bond, or a hydroxyl group. a, b, c, e, h, i, and f are independently 0 or a positive number. b, e, and n are not 0 at the same time, and 2≤b+e+h≤300. d is a positive number of 50 to 4,000, g is 0 or a positive number of 0 to 50, j is 0 or a positive number of 0 to 50, c, f, and i are not 0 at the same time, and 0.01≤c+f+i≤2.9. Preferably, 0.03≤c+f+i≤2.7, and more preferably, 0.05≤c+f+i≤2.5.
[0040] In the formula (1), R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and having no aliphatic unsaturated bond, preferably having 1 to 10 carbon atoms, and more preferably having 1 to 8 carbon atoms. More specifically, alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, naphthyl, and tolyl; aralkyl groups such as benzyl and phenethyl; and groups in which a part of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms, epoxy groups, amino groups, polyether groups, cyano groups, hydroxyl groups, and the like. Among these, it is preferred that 80 mol% or more of the total number of R is methyl group from the viewpoint of curability and reduction of the peeling force of the obtained cured product.
[0041] P is composed of -(CH 2 ) n -CH=CH 2 (n is an integer of 0 to 6). Examples thereof include vinyl, allyl, butenyl, propenyl, 5-hexenyl, octenyl, and decenyl. Among them, vinyl is preferred.
[0042] A is composed of CH 2 =CR 2 COR 3 - is a (meth)acrylic acid group-containing group. 2 is a hydrogen atom or a methyl group, preferably a hydrogen atom. 3 Yes OR 4 or R 4 The divalent group represented by R 4 It is a divalent organic group having 1 to 20 carbon atoms, may have a branched or cyclic structure, and may contain an epoxy group, an ester bond, a urethane bond, an ether bond, an isocyanate bond, and a hydroxyl group. 4, for example, there can be illustrated straight-chain alkylene groups such as methylene, ethylene, propylene, butylene, hexamethylene, octamethylene, and decylene; branched alkylene groups such as methylethylene and methylpropylene; cyclic alkylene groups such as cyclohexylene; alkenylene groups such as propenylene; arylene groups such as phenylene; and aralkylene groups such as methylenephenylene and methylenephenylmethylene. Ester bonds, carbamate bonds, ether bonds, and isocyanate bonds may be inserted into the divalent hydrocarbon groups, and these may also be used in combination. Furthermore, part or all of the hydrogen atoms of these divalent hydrocarbon groups may be substituted with epoxy groups or hydroxyl groups. Among these, R 4 , preferably propylene.
[0043] a, b, c, e, and h in formula (1) are each independently 0 or a positive number. b, e, and h are not simultaneously 0, and 2≤b+e+h≤300, preferably 2≤b+e+h≤10, and further preferably in the range of 2≤b+e+h≤4. a is preferably 0 or a positive number of 1 to 4. In particular, the alkenyl group is preferably bonded to the silicon atom of the M unit or the D unit, b is preferably a positive number of 1 to 6, and a+b is preferably a positive number of 2 to 10. e is preferably 0 or a positive number of 1 to 10, and h is preferably 0 or a positive number of 1 to 5.
[0044] In formula (1), c, f, and i are each independently 0 or a positive number. c, f, and i are not simultaneously 0, and the preferred range is 0.01≤c+f+i≤2.9. Preferably, it is 0.03≤c+f+i≤2.7, and more preferably, it is 0.05≤c+f+i≤2.5. In particular, the (meth)acrylic acid group is preferably bonded to the silicon atom of the D unit, c and i are preferably 0, and f is preferably a positive number of 0.01 to 2.9.
[0045] In formula (1), R 2 SiO 2 / 2 The number of units d is a positive number of 50 to 4,000, preferably a positive number of 60 to 1,000, and more preferably a positive number of 70 to 300. When d is less than the lower limit, if the coating speed is 200 m / min or more, the amount of smoke generated increases, and the coated surface of the organopolysiloxane composition may be rough. On the other hand, when d exceeds the upper limit, the dynamic viscosity of the organopolysiloxane composition becomes too high, the coating property decreases, and the smoothness deteriorates, and the difference in the coating amount may become large depending on the position.
[0046] In formula (1), RSiO 3 / 2 The number of units g is 0 or a positive number of 0 to 50, preferably 0 or a positive number of 0 to 10, and more preferably 0 or a positive number of 0 to 5. 4 / 2 The number of units, j, is 0 or a positive number of 0-50, preferably 0 or a positive number of 0-10, and more preferably 0 or a positive number of 0-5.
[0047] The component (A) preferably has an ethylene value of 0.0001 mol / 100 g to 0.7 mol / 100 g, more preferably 0.005 mol / 100 g to 0.5 mol / 100 g, and even more preferably 0.01 mol / 100 g to 0.3 mol / 100 g. When the ethylene value is below the lower limit, the number of reaction points becomes too small, which may cause poor curing. When the ethylene value exceeds the upper limit, the crosslinking density becomes too high, the low-speed peeling force becomes too high, and it may become difficult to peel.
[0048] The component (A) preferably has a weight average molecular weight of 3,000 to 300,000, preferably 5,000 to 100,000, more preferably 7,000 to 30,000, and particularly preferably 9,000 to 20,000. When the weight average molecular weight of the component (A) is lower than the lower limit, the amount of coating on the substrate may be insufficient. In addition, when the upper limit is exceeded, the workability may be reduced. In the present invention, the weight average molecular weight may be, for example, 29 The molecular weight is measured by Si-nuclear magnetic resonance (NMR) measurement (measurement solvent: deuterated chloroform) or by a weight average molecular weight in terms of polystyrene obtained by gel permeation chromatography (GPC) analysis (solvent: toluene) (the same applies hereinafter).
[0049] The component (A) preferably has a viscosity of 10 mPa·s or more at 25°C measured by a rotational viscometer and a 30% toluene solution viscosity (viscosity of a solution obtained by dissolving 30% by mass of an organopolysiloxane in toluene) of 70,000 mPa·s or less, and more preferably has a 30% toluene solution viscosity of 50 mPa·s or more and a 30% toluene solution viscosity of 60,000 mPa·s or less. When the viscosity is less than 10 mPa·s, the amount of coating may become insufficient. In addition, when the 30% toluene solution viscosity exceeds 70,000 mPa·s, workability may be reduced.
[0050] In the (A) organopolysiloxane of the present invention, the bonding site of the alkenyl group and the (meth)acrylic group may be any one of the molecular chain terminal and the side chain, but the (meth)acrylic group is preferably located in the side chain, and in particular, it is preferably directly or via a hydrocarbon and bonded to the silicon atom of the D unit. It is particularly preferred that the (meth)acrylic group is located only in the side chain. The alkenyl group is preferably bonded to the silicon atom of the M unit or the D unit. As the (A) component, for example, there can be listed: siloxanes containing alkenyl groups at both ends and (meth)acrylic groups in the side chain, siloxanes containing alkenyl groups in the side chain and (meth)acrylic groups in the side chain, siloxanes containing alkenyl groups at one end and in the side chain and (meth)acrylic groups in the side chain, siloxanes containing alkenyl groups at both ends and in the side chain and (meth)acrylic groups in the side chain, and siloxanes containing alkenyl groups at branched ends and (meth)acrylic groups in the side chain.
[0051] More specifically, siloxanes having the following structures can be mentioned.
[0052] M Vi 2 D d D A f ,
[0053] M 2 D d D Vi e D A f ,
[0054] M Vi 3 D d D A f T 1 ,
[0055] M Vi 4 D e D A f T 2 ,
[0056] M Vi 2 D d D Vi e D A f ,
[0057] M Vi 2 D d D Vi e D A f Q 1 ,
[0058] M A 2 D d D Vi e D A f ,and
[0059] M A 2 M 1 D d D Vi e D A f T 1 wait.
[0060] More specifically, siloxanes having the following structures can be mentioned.
[0061] M Vi 2 D 100 D A 0.01 ,
[0062] M Vi 2 D 150 D A 0.05 ,
[0063] M Vi 2 D 200 D A 0.1 ,
[0064] M Vi 2 D 300 D A 2.5 ,
[0065] M Vi 3 D 200 D A 0.1 ,and
[0066] M Vi 2 D 200 D A 0.5 Q 1 wait.
[0067] In the description, M is R 3 SiO 1 / 2 、M Vi For R 2PSiO 1 / 2 、D is R 2 SiO 2 / 2 , D Vi RPSiO 2 / 2 , D A RASiO 2 / 2 、T is RSiO 3 / 2 Q is SiO 4 / 2 . R, A and P are as described above.
[0068] [(B) ingredient]
[0069] The component (B) is an organohydrogenpolysiloxane having two or more silicon-bonded hydrogen atoms (Si-H groups) in one molecule and having no (meth)acrylic group, and one or more of them can be used alone or in combination. The Si-H groups of the organohydrogenpolysiloxane react with the alkenyl groups of the component (A) to form an organopolysiloxane crosslinked product.
[0070] The component (B) preferably has 3 to 100 silicon-bonded hydrogen atoms (Si-H groups) in one molecule, and more preferably has 10 to 100. In addition, the Si-H group content is preferably 0.001 mol / 100g to 3.5 mol / 100g, more preferably 0.01 mol / 100g to 2.5 mol / 100g, and further preferably 0.02 mol / 100g to 2.0 mol / 100g. When the Si-H group content is too low, the curability or adhesion of the composition may deteriorate. When it is too much, the peeling force may sometimes become heavier.
[0071] (B) The organohydrogenpolysiloxane is preferably represented by the following formula (2).
[0072] [Chemistry 2]
[0073] (R′ 3 SiO 1 / 2 ) m (R′ 2 HSiO 1 / 2 ) n (R′ 2 SiO 2 / 2 ) o (R′HSiO 2 / 2 ) p (R′SiO 3 / 2 ) q (HSiO 3 / 2 ) r (SiO 4 / 2 ) s (2)
[0075] In formula (2), R' is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and having no aliphatic unsaturated bond. m, n, o, and q are each independently 0 or a positive number, p is a positive number of 0 to 100, r is a positive number of 0 to 10, s is a positive number of 0 to 10, n, p, and r are not simultaneously 0, and 2≤n+p+r≤100.
[0076] In the formula (2), R' is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and having no aliphatic unsaturated bond, preferably having 1 to 10 carbon atoms, and more preferably having 1 to 8 carbon atoms. Examples thereof include: alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, naphthyl, tolyl; aralkyl groups such as benzyl and phenethyl; and groups in which a part of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms, epoxy groups, amino groups, polyether groups, cyano groups, hydroxyl groups, etc. Among them, from the viewpoint of curability and reducing the peeling force of the obtained cured product, it is preferred that 80 mol% or more of the total number of R' is methyl.
[0077] In formula (2), m, n, o, and q are each independently 0 or a positive number, m is preferably 0 or a positive number of 1 to 10, n is preferably 0 or a positive number of 1 to 10, and m+n is preferably a positive number of 2 to 12. o is preferably a positive number of 0 or 1 to 100, and q is preferably a positive number of 0 or 1 to 10. In addition, p is a positive number of 0 to 100, preferably a positive number of 2 to 100, and more preferably a positive number of 10 to 80. r is a positive number of 0 to 10, preferably a positive number of 0 or 1 to 5, and s is a positive number of 0 to 10, preferably a positive number of 0 or 1 to 5. In addition, n, p, and r are not 0 at the same time, and n+p+r is a positive number of 3 to 100, and preferably a positive number of 10 to 80.
[0078] Examples of the (B) organohydrogenpolysiloxane include siloxanes containing hydrosilyl groups at both ends, siloxanes containing hydrosilyl groups at side chains, siloxanes containing hydrosilyl groups at one end and in side chains, and siloxanes containing hydrosilyl groups at both ends and in side chains.
[0079] More specifically, organohydrogenpolysiloxanes having the following structures are mentioned.
[0080] M H 2 D o 、M 2 D H p ,
[0081] M 2 D o D H p ,
[0082] M H 2 D o D H p ,
[0083] M H 3 D o T 1 ,
[0084] M H 4 D o T 2 ,and
[0085] M m D o D H p T H r wait.
[0086] More specifically, organohydrogenpolysiloxanes having the following structures are mentioned.
[0087] M H 2 D 10 ,
[0088] M H 2 D 100 ,
[0089] M 2 D H 80 ,
[0090] M 2 D 27 D H 3 ,
[0091] M 2 D 97 D H 3 ,
[0092] M 2 D 26 D H 4 ,
[0093] M 2 D 25 D H 5 ,
[0094] M 2 D 24 D H6 ,
[0095] M 2 D 96 D H 4 ,
[0096] M 2 D 95 D H 5 ,
[0097] M H 3 D 100 T 1 ,
[0098] M H 4 D 100 T 2 ,
[0099] M H 2 D 97 D H 1 ,
[0100] M H 2 D 95 D H 3 ,
[0101] M 3 D 93 D H 3 T H 1 ,
[0102] M 2 D H 30 、M 2 D H 60 wait.
[0103] In the above formulas, M is R' 3 SiO 1 / 2 、M H R′ 2 HSiO 1 / 2 , D is R′ 2 SiO 2 / 2 , D H R′HSiO 2 / 2 、T is R′SiO 3 / 2 , T H For HSiO 3 / 2 . R′ is as described above.
[0104] The component (B) preferably has a weight average molecular weight of 194 to 10,000, more preferably 874 to 5,000. If the weight average molecular weight is below the lower limit, the adhesion of the composition may be greatly deteriorated. If the weight average molecular weight exceeds the upper limit, the reactivity deteriorates, the curability decreases, and a decrease in residual adhesion or an increase in peeling force due to insufficient curing may be observed.
[0105] The dynamic viscosity of the component (B) at 25° C. measured by an Ostwald viscometer is preferably 2 mm 2 / s~500mm 2 / s, more preferably 2 mm 2 / s~300mm 2 / s, and more preferably 5mm 2 / s~200mm 2 / s. The dynamic viscosity at 25°C is less than 2mm 2 / s, the reactivity is good due to the small molecular weight, but the adhesion to the substrate may deteriorate. 2 / s, the reactivity is deteriorated, the curing property is reduced, and a reduction in the residual adhesion rate or an increase in the peeling force due to insufficient curing may be observed.
[0106] Regarding the amount of component (B), the ratio of the number of Si-H groups in component (B) to the number of alkenyl groups in component (A) is 1 to 5, preferably an amount equivalent to 1.2 to 3. When the amount of component (B) is too small, the curability and adhesion of the composition are insufficient. When the amount is too large, the amount of remaining Si-H groups increases, so the peeling force increases. The Si-H groups decrease over time, so the peeling force changes greatly over time.
[0107] [(C) ingredient]
[0108] (C) Platinum group metal catalysts can use existing catalysts used as addition reaction catalysts. Examples of the platinum group metal catalysts include platinum, palladium, rhodium, and ruthenium catalysts. Platinum catalysts are particularly preferred. Examples of platinum catalysts include platinum silica-alumina, platinum alumina-halogen, platinum rhodium and other platinum compounds, complexes of platinum and vinyl siloxane, alcohol solutions or aldehyde solutions of chloroplatinic acid, complex salts of chloroplatinic acid and various olefins, complexes of chloroplatinic acid and vinyl siloxane, etc.
[0109] The amount of component (C) is the catalyst amount, and the concentration of the platinum group metal used to provide a hardened film for release paper or release film is usually 60 mass ppm to 500 mass ppm in the organopolysiloxane composition. In contrast, the amount of the platinum group metal catalyst in the present invention is 1 mass ppm to 100 mass ppm in terms of the mass of the platinum group metal relative to the total mass of the composition. It is preferably 3 mass ppm to 60 mass ppm, more preferably 5 mass ppm to 40 mass ppm, and most preferably 10 mass ppm to 30 mass ppm. As for the organopolysiloxane composition of the present invention, as described above, even if the amount of platinum group metal catalyst is small, it is fully hardened and can provide a hardened film with good physical properties. When the amount of catalyst is less than the lower limit, the addition reaction does not proceed, and a lot of unreacted functional groups remain, so it is impossible to form a sufficient hardened film. In addition, if the upper limit is exceeded, it may sometimes react with moisture or a control agent, or the usable time may be shortened and hardened during operation.
[0110] [(D) ingredient]
[0111] The organopolysiloxane composition of the present invention may contain (D) an addition reaction control agent as required. The addition reaction control agent controls the catalytic activity of the platinum group metal catalyst and may be a conventional control agent. Examples thereof include organic nitrogen compounds, organic phosphorus compounds, acetylene compounds, oxime compounds, and organic chlorine compounds. More specifically, examples include acetylene alcohols such as 1-ethynyl-1-cyclohexanol, 3-methyl-1-butyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-pentyn-3-ol, and 2-phenyl-3-butyn-2-ol; acetylene compounds such as 3-methyl-3-pentene-1-yne and 3,5-dimethyl-3-hexene-1-yne; reaction products of acetylene compounds such as 1,1-dimethylpropynyloxytrimethylsilane with alkoxysilanes, siloxanes, or hydrogensilanes; vinylsiloxanes such as tetramethylvinylsiloxane rings; organic nitrogen compounds such as benzotriazole and other organic phosphorus compounds; oxime compounds; maleic acid compounds such as diallyl maleate; and organic chlorine compounds.
[0112] The amount of component (D) is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of component (A). By mixing within the range, the addition hardening reaction can be well controlled. When mixing, if too little, the usable time becomes shorter, and hardening may occur during operation. If too much, no addition reaction is performed, and therefore a hardened film may not be formed.
[0113] [Other ingredients]
[0114] In addition to the above-mentioned components (A) to (D), other components prepared in addition reaction curing compositions for conventional release papers or release films may be mixed into the organopolysiloxane composition of the present invention within a range that does not impair the effects of the present invention. For example, organic solvents, high molecular weight linear organopolysiloxanes other than components (A) to (C) for the purpose of imparting slip properties, silicone resins having aromatic groups other than components (A) to (C) for the purpose of adjusting release strength, silicone resins (resins), and silica may be mentioned.
[0115] As the organic solvent, it is preferred to use an organic solvent (not including a siloxane solvent) soluble in an organopolysiloxane, such as toluene, hexane, xylene, methyl ethyl ketone (also known as 2-butanone); a low-viscosity cyclic siloxane such as octamethyltetrasiloxane and decamethylpentasiloxane, M 2 D t (M, D are the same as those in formula (1); t is 0 to 200, preferably 1 to 50) or the like straight chain siloxane; M 2+ u D t T u (M, D, T are the same as those in the formula (1); t is 0 to 200, preferably 1 to 50, and u is 1 to 10, preferably 1 to 3) or other branched siloxanes or other organopolysiloxanes (siloxane solvents).
[0116] The amount of the organic solvent is preferably 3 to 50 times, more preferably 8 to 30 times the total mass of the component (A) and the component (B).
[0117] The organopolysiloxane composition of the present invention is obtained by mixing the above-mentioned components (A) to (C) and, if necessary, the component (D) or the arbitrary components in a predetermined amount. The obtained organopolysiloxane composition preferably has a dynamic viscosity of 10 mm / s at 25° C. as measured by an Oswald viscometer. 2 / s~2000mm 2 / s, more preferably 15mm 2 / s~1000mm 2 / s.
[0118] The organopolysiloxane composition of the present invention is applied to various substrates and cured to provide release paper, release film, etc. For example, after being applied to a sheet substrate such as paper or plastic film by a coating roller (three-roller, five-roller, gravure roller, planographic gravure roller, etc.), it is heated and cured by a conventional method to form a silicone cured film on one side of the sheet substrate, thereby obtaining release paper, release sheet, etc.
[0119] Examples of the paper substrate include glassine paper, polyethylene laminated paper, polyvinyl alcohol resin coated paper, clay coated paper, etc. Examples of the plastic film substrate include films of polyesters such as polyethylene, polypropylene, and polyethylene terephthalate.
[0120] The amount of the organopolysiloxane composition applied to the substrate may be an amount sufficient to form a silicone cured film on the surface of the sheet-like substrate, for example, 0.1 g / m 2 ~5.0g / m 2 Too much coating may sometimes lead to a decrease in peeling performance. The heat curing conditions vary depending on the type of substrate or the coating amount, but a cured film can be formed on the substrate by heating at 80°C to 200°C, preferably 100°C to 180°C for 1 to 60 seconds, preferably 2 to 30 seconds.
[0121] Example
[0122] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0123] Furthermore, the weight average molecular weight listed below is 29 The viscosity was measured by Si-NMR (measurement solvent: deuterated chloroform). The viscosity was measured by a rotational viscometer at 25°C (mPa·s). The dynamic viscosity was measured by an Owas viscometer at 25°C (mm 2 / s).
[0124] The components used in Examples and Comparative Examples are as follows.
[0125] (A)Ingredients
[0126] In the following, M is R 3 SiO 1 / 2 、M Vi For R 2 PSiO 1 / 2 、D is R 2 SiO 2 / 2 , D Vi RPSiO 2 / 2 , D A RASiO 2 / 2 、T is RSiO 3 / 2 . R is methyl and P is vinyl.
[0127] 1) Methyl polysiloxane (1) having two vinyl groups in one molecule and an average of 0.05 acrylic groups represented by the following average formula:
[0128] M Vi 2 D 150 D A0.05
[0129] Where A is CH 2 =CHCO(CH 2 ) 3 -, ethylene value is 0.0177 mol / 100g, viscosity is 413mPa·s, and weight average molecular weight is 11294.6.
[0130] 2) Methyl polysiloxane (2) having two vinyl groups in one molecule and an average of 0.1 acrylic groups represented by the following average formula:
[0131] M Vi 2 D 150 D A 0.1
[0132] Where A is CH 2 =CHCO(CH 2 ) 3 -, ethylene value is 0.0177 mol / 100g, viscosity is 415 mPa·s, and weight average molecular weight is 11303.2.
[0133] 3) Methyl polysiloxane (3) having two vinyl groups in one molecule and an average of 2.5 acrylic groups represented by the following average formula:
[0134] M Vi 2 D 220 D A 2.5
[0135] Where A is CH 2 =CHCO(CH 2 ) 3 -, ethylene value is 0.0118 mol / 100 g, viscosity is 1082 mPa·s, and weight average molecular weight is 16896.
[0136] 4) Methyl polysiloxane (4) having two vinyl groups and an average of one acrylic group in one molecule represented by the following average formula:
[0137] M Vi 3 D 150 D A 1 T 1
[0138] Where A is CH 2 =CHCO(CH 2 ) 3-, ethylene value is 0.0258 mol / 100g, viscosity is 258mPa·s, and weight average molecular weight is 11618.
[0139] 5) Methyl polysiloxane (5) represented by the following average formula, having two vinyl groups in the side chain and an average of 0.1 acrylic groups
[0140] M 2 D Vi 2 D 148 D A 0.1
[0141] Where A is CH 2 =CHCO(CH 2 ) 3 -, ethylene value is 0.0174 mol / 100g, viscosity is 418 mPa·s, and weight average molecular weight is 11303.2.
[0142] 6) Methyl polysiloxane (6) having two vinyl groups in one molecule and an average of 0.1 methacrylic groups represented by the following average formula:
[0143] M Vi 2 D 150 D A ' 0.1
[0144] Where A' is CH 2 =C(CH 3 )CO(CH 2 ) 3 -, ethylene value is 0.0177 mol / 100 g, viscosity is 416 mPa·s, and weight average molecular weight is 11304.6.
[0145] (B) Ingredients
[0146] Methyl hydrogen polysiloxane (7) represented by the following average formula
[0147] M 2 D H 100
[0148] In the above, M is R' 3 SiO 1 / 2 , D H R′HSiO 2 / 2 R' is methyl, and both ends of the molecular chain have trimethylsilyl groups. The Si-H group content is 1.62 mol / 100g, and the dynamic viscosity is 35 mm 2 / s. The weight average molecular weight is 6162.
[0149] Other added ingredients (comparative example)
[0150] 1) Methyl polysiloxane (8) represented by the following average formula, having vinyl groups at both ends and no (meth)acrylic group
[0151] M Vi 2 D 150
[0152] Where M Vi For R 2 PSiO 1 / 2 , D is R 2 SiO 2 / 2 , R is methyl, P is CH 2 =CH-, ethylene value is 0.0177 mol / 100 g, viscosity is 405 mPa·s, and weight average molecular weight is 11286.
[0153] 2) Methyl polysiloxane (9) having two vinyl groups in one molecule and an average of 10 acrylic groups represented by the following average formula:
[0154] M Vi 2 D 150 D A 10
[0155] M in the formula Vi For R 2 PSiO 1 / 2 , D is R 2 SiO 2 / 2 , D A RASiO 2 / 2 , R is methyl, A is CH 2 =CHCO(CH 2 ) 3 -, P is CH 2 =CH-, ethylene value is 0.0154 mol / 100g, viscosity is 427mPa·s, and weight average molecular weight is 13006.
[0156] 3) Methyl polysiloxane (10) having acrylic groups at both ends represented by the following average formula:
[0157] M A 2 D 5
[0158] M in the formula A For R 2 ASiO 1 / 2 、D is R 2SiO 2 / 2 , R is methyl, A is CH 2 =CHCO(CH 2 ) 3 -, viscosity is 7mPa·s. Weight average molecular weight is 728.
[0159] [Example 1]
[0160] The components were mixed according to the formulation described in Table 1 below to prepare an addition reaction-curable organopolysiloxane composition.
[0161] That is, (A) 100 parts by mass of the methyl polysiloxane (1), (B) 1.97 parts by mass of the methyl hydrogen polysiloxane (7), and (D) 0.3 parts by mass of 1-ethynyl-1-cyclohexanol were added and stirred until uniform, and then (C) a complex of platinum and vinyl siloxane was added in an amount of 20 ppm by mass in terms of the mass of platinum atoms relative to the total mass of the composition and stirred until uniform. The obtained product had a dynamic viscosity of 393 mm 2 H / Vi (the ratio of the number of Si-H groups in the component (B) to the number of alkenyl groups in the component (A) (the same applies hereinafter)) was 1.8.
[0162] [Example 2]
[0163] As shown in Table 1 below, Example 1 was repeated except that 100 parts by mass of the methyl polysiloxane (2) was used as the component (A) to obtain a 2-hydroxy-2-methyl-1-isopropyl siloxane having a dynamic viscosity of 395 mm 2 / s, H / Vi=1.8.
[0164] [Example 3]
[0165] As shown in Table 1 below, Example 1 was repeated except that 100 parts by mass of the methyl polysiloxane (3) was used as the component (A) and 1.97 parts by mass of the methyl hydrogen polysiloxane (7) was used as the component (B) to obtain a 2-hydroxy-1-methyl-1 ... 2 / s, H / Vi=1.8 organopolysiloxane composition.
[0166] [Example 4]
[0167] As shown in Table 1 below, Example 1 was repeated except that 100 parts by mass of the methyl polysiloxane (4) was used as the component (A) and 2.87 parts by mass of the methyl hydrogen polysiloxane (7) was used as the component (B) to obtain a 244 mm2 mol mol polysiloxane having a dynamic viscosity of 244 mm2. 2 / s, H / Vi=1.8.
[0168] [Example 5]
[0169] As shown in Table 1 below, Example 1 was repeated except that 100 parts by mass of the methyl polysiloxane (5) was used as the component (A) and 1.639 parts by mass of the methyl hydrogen polysiloxane (7) was used as the component (B) to obtain a 2-hydroxy-1-methyl-1 ... 2 / s, H / Vi=1.8.
[0170] [Example 6]
[0171] As shown in Table 1 below, Example 1 was repeated except that 50 parts by mass of the methyl polysiloxane (3) and 50 parts by mass of the methyl polysiloxane (8) were used as the component (A), and 1.51 parts by mass of the methyl hydrogen polysiloxane (7) was used as the component (B) to prepare a 2-hydroxy-1-methyl-1-propene-1-yl siloxane having a dynamic viscosity of 646 mm 2 / s, H / Vi=1.8.
[0172] [Example 7]
[0173] As shown in Table 1 below, Example 1 was repeated except that 100 parts by mass of the methyl polysiloxane (6) was used as the component (A) to prepare a 2-hydroxy-1-methyl-1-isopropyl siloxane having a dynamic viscosity of 396 mm 2 / s, H / Vi=1.8.
[0174] [Example 8]
[0175] As shown in Table 1 below, Example 1 was repeated except that 15 ppm by mass of the complex of platinum and vinyl siloxane (C) was used in terms of the mass of platinum atoms relative to the total mass of the composition to obtain a 2-hydroxy-2-nitropropene-2-ol having a dynamic viscosity of 395 mm 2 / s, H / Vi=1.8.
[0176] [Comparative Example 1]
[0177] As shown in Table 1 below, Example 1 was repeated except that 100 parts by mass of the methyl polysiloxane (8) containing vinyl groups at both ends was used instead of the component (A) to obtain a cellulose ester having a dynamic viscosity of 386 mm 2 / s, H / Vi=1.8.
[0178] [Comparative Example 2]
[0179] As shown in Table 2 below, Example 1 was repeated except that 100 parts by mass of methyl polysiloxane (9) containing vinyl groups at both ends and acrylic groups in the side chain was used instead of the component (A) and the amount of the methyl hydrogen polysiloxane (B) (7) was changed to 1.71 parts by mass to obtain a 2-hydroxy-1-methyl-1-methyl-2-thiophene (1-hydroxy-1-methyl-2-thiophene) having a dynamic viscosity of 408 mm2 / s, H / Vi=1.8.
[0180] [Comparative Example 3]
[0181] As shown in Table 2 below, in addition to the composition of Comparative Example 1, 1 part by mass of an organopolysiloxane M having acrylic groups at both ends was further added. A 2 D 5 (10) and repeat Comparative Example 1 to obtain a product having a dynamic viscosity of 388 mm 2 / s, H / Vi=1.8.
[0182] [Comparative Example 4]
[0183] As shown in Table 2 below, Comparative Example 1 was repeated except that 1 part by mass of acrylic acid (11) was further added to the composition of Comparative Example 1 to obtain a cellulose ester having a dynamic viscosity of 393 mm 2 / s, H / Vi=1.8.
[0184] [Reference Example 1]
[0185] As shown in Table 2 below, 100 parts by mass of methylpolysiloxane (8) containing vinyl groups at both ends, 1.97 parts by mass of methylhydrogenpolysiloxane (B) (H / Vi=1.8), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol as the component (D) were added in the same manner as in Comparative Example 1, and stirred to uniformity. Then, a complex of platinum and vinylsiloxane (C) was added to give 100 ppm by mass in terms of the mass of platinum atoms relative to the total mass of the composition, and stirred until uniformity was achieved.
[0186] The obtained product has a dynamic viscosity of 387 mm 2 / s of organopolysiloxane composition.
[0187] The organopolysiloxane compositions obtained above were subjected to the following evaluations.
[0188] 〔Peeling force〕
[0189] The organopolysiloxane composition was coated on the metal roller of the RI tester (manufactured by IHI Machinery Systems Co., Ltd.), and the two rollers were rotated for 45 seconds to stretch uniformly. Thereafter, the composition was transferred from the rubber roller to the glass paper ASP (manufactured by Ahlstrom-munksjo, containing catalyst poison). The glass paper to which the composition was transferred was heated in a hot air dryer at 120° C. for 30 seconds to obtain a glass paper having a thickness of 0.9 g / m 2 ~1.1g / m 2After aging for 24 hours at 25°C, TESA-7475 tape (tesa UK Ltd) was attached to the surface of the cured film of the release paper (the side transferred from the rubber roller) and cut into 2.5 cm × 18 cm size. The paper was sandwiched between glass plates and aged at 25°C and 70 g / cm 2 Under load, and 70℃, 20g / cm 2 The test piece was aged for 24 hours at room temperature under a load of . After aging, one end of the test piece was peeled off, and the end of the substrate of the tape was stretched in a direction of 180 degrees relative to the cellophane at a peeling speed of 0.3 m / min. At this time, the force required to peel off the tape (i.e., "peeling force") (N / 25 mm) was measured using a tensile tester (Shimadzu Corporation AGS-50G model).
[0190] 〔Residual bonding rate〕
[0191] The TESA-7475 tape after the peeling force measurement was attached to a polyester film, and a 2 kg roller was moved back and forth once to apply a load. After leaving it for 30 minutes, one end of the TESA-7475 tape was peeled off, and the end was stretched in a direction forming an angle of 180 degrees relative to the polyester film. The force required to peel the tape at a peeling speed of 0.3 m / min (hereinafter referred to as "peeling force A", N / 25 mm) was measured.
[0192] As a blank, an unused TESA-7475 tape was attached to a polyester film, and a 2 kg roller was reciprocated once to apply a load in the same manner as described above. After leaving it for 30 minutes, one end of the TESA-7475 tape was peeled off, and the end was stretched in a direction at an angle of 180 degrees relative to the polyester film. The force required to peel off the tape at a peeling speed of 0.3 m / min (hereinafter referred to as "peeling force B", N / 25 mm) was measured.
[0193] The residual adhesion rate (%) was calculated by (value of peel force A) / (value of peel force B)×100.
[0194] (hardening)
[0195] Each organopolysiloxane composition was coated on a metal roller of a testing machine. The two rollers including the metal roller and the rubber roller were rotated in contact for 45 seconds to uniformly stretch the organopolysiloxane composition, and then the composition was transferred from the rubber roller to a Korean glass paper. The polyethylene laminated paper to which the organopolysiloxane composition was transferred was heated in a hot air dryer at 120°C for 30 seconds to obtain a 0.9 g / m thick paper. 2 ~1.1g / m 2Remove the release paper from the dryer, immediately rub the hardened film surface 10 times with the index finger, apply red magic ink, and observe the ink concentration or hardened film state.
[0196] The results were evaluated based on the following indices and are shown in Tables 1 and 2.
[0197] · If the finger marks appear deep, "×"
[0198] · The finger marks are light and are marked as "△"
[0199] · "ο" means that the fingerprints are almost invisible.
[0200] In the same manner as in the case of the peeling force measurement, a polyethylene terephthalate film with a thickness of 36 μm was overlapped on the surface of the cured film of the organopolysiloxane composition formed on the surface of the glass paper, and after being pressed at room temperature and under a pressure of 0.98 MPa for 20 hours, the polyethylene terephthalate film was removed from the cured film. An oily ink (trade name: Magic Ink, manufactured by Teranishi Chemical Industry Co., Ltd.) was applied to the surface of the polyethylene terephthalate film in contact with the cured film, and the silicone migration was evaluated based on the repellency of the ink.
[0201] The results were evaluated based on the following indicators and are shown in Tables 1 and 2.
[0202] No ink rejection (no or very little silicone migration) is "ο"
[0203] "×" indicates ink repellency (more silicone migration)
[0204] [Tightness]
[0205] The organopolysiloxane composition was transferred onto glass paper by the same method as the evaluation method of curability, and heated in a hot air dryer at 120°C for 30 seconds to obtain a release paper. The release paper was stored in a constant temperature and humidity chamber at 60°C and 90%RH for 1 day, and then the hardened film surface was rubbed 10 times with the index finger by the same method as the curability, and the red magic ink was applied to observe the ink concentration and the state of the hardened film.
[0206] The results were evaluated based on the following indicators and are shown in Tables 1 and 2.
[0207] · If the finger marks appear deep, "×"
[0208] · The finger marks are light and are marked as "△"
[0209] ・If the fingerprints are barely visible, it is marked as "○"
[0210]
[0211] [Table 2]
[0212]
[0213] As shown in Table 1, Reference Example 1 is a conventional addition reaction curing type organopolysiloxane composition, and the platinum concentration of the catalyst (C) is as high as 100 mass ppm. Since the curing reaction of the composition is fully carried out, the curability, silicone migration and adhesion are good, the peeling force is low, the residual adhesion rate is high, and it has good peeling characteristics.
[0214] Comparative Example 1 is a composition in which the platinum concentration of the catalyst (C) is set to 20 mass ppm in the composition of Reference Example 1. In this case, the organopolysiloxane composition does not harden during the heating treatment at 120°C for 30 seconds and becomes oily. That is, the hardening is insufficient. In addition, after aging at 25°C for 1 day, the hardening is also insufficient, and the finger marks are clear after wiping the coated surface. In addition, due to the large amount of migration, the hardening property and silicone migration are poor.
[0215] In addition, as shown in Table 2, Comparative Examples 3 and 4 are compositions in which 1 part by mass of siloxane (10) or acrylic acid having acrylic groups at both ends is formulated into the composition of Comparative Example 1. The composition contains siloxane or acrylic acid containing acrylic groups, but the curing property and adhesion are poor, and the silicone migration is as poor as that of Comparative Example 1. In addition, the peeling force is higher than that of Reference Example 1, and the residual adhesion rate is also low. Comparative Example 2 is a composition in which 100 parts by mass of methyl polysiloxane (9) having vinyl groups at both ends and acrylic groups on the side chains is formulated. The siloxane has an average of 10 acrylic groups in one molecule. The composition contains siloxane containing vinyl and acrylic groups, but the curing property and adhesion are poor, and the silicone migration is as poor as that of Comparative Example 1. In addition, the peeling force is higher than that of Reference Example 1, and the residual adhesion rate is also low.
[0216] In contrast, as shown in Table 1, Examples 1 to 8 are organopolysiloxane compositions containing methylpolysiloxane having vinyl groups at both ends and a specific amount of acrylic groups in the side chains. In these Examples 1 to 8, the vinyl-containing organopolysiloxane having a specific amount of acrylic groups or methacrylic groups is used as the (A) component, and the composition is sufficiently hardened despite the low platinum concentration of the (C) catalyst. Therefore, even if the coated surface of the hardened film is wiped, almost no finger marks are left, and the amount of silicone transfer is also small. In addition, the peeling force and the residual adhesion rate are the same as those of Reference Example 1. Therefore, by containing the (A) component of the present application, the hardenability of the composition is improved, and the addition reaction can be carried out at a low platinum concentration.
[0217] In particular, the number of D units of the methylpolysiloxane (3) used in Example 3 is 220, and it contains 2.5 siloxane units having an acrylic group. In addition, the molecular weight of the methylpolysiloxane (5) used in Example 5 is the same as that of the methylpolysiloxane (2), and it has 2 vinyl groups on the side chain. Even with a composition containing such a methylpolysiloxane, the curability and adhesion are good. In addition, the composition of Example 6 is a composition that uses a methylpolysiloxane (3) having an acrylic group and a vinyl group and a methylpolysiloxane (8) having no acrylic group but a vinyl group. In the composition, the curability is also good and the amount of silicone transfer is also small. In addition, the peel force and the residual adhesion rate are the same as those of Reference Example 1. Therefore, even with an existing composition containing a vinyl-containing organic polysiloxane, by containing the (A) component of the present application, the addition reaction is fully promoted with a small amount of platinum catalyst.
[0218] That is, by blending the component (A) of the present invention, even if the platinum concentration of the platinum group metal catalyst (C) is as low as less than 100 mass ppm, the composition can be sufficiently cured and can obtain the same peeling properties as when cured at 100 mass ppm.
[0219] The organopolysiloxane composition of the present invention can be cured sufficiently to form a hardened film having the same release force as the existing addition type composition, although the amount of platinum group metal catalyst is small, and is suitable as a composition for providing a hardened film for release paper and release film. The organopolysiloxane composition of the present invention can be cured even under conditions that have been difficult to cure before, and the manufacturing cost can be greatly reduced due to the small amount of platinum group metal catalyst. In addition, even substrates containing catalyst poison can be cured by addition reaction.
Claims
1. An addition reaction curing type organopolysiloxane composition comprising the following components (A) to (C), (A) an organopolysiloxane having two or more silicon-bonded alkenyl groups in one molecule, an average of 0.01 to 2.9 (meth)acrylic groups, and a weight average molecular weight of 3,000 to 300,000 (B) an organohydrogenpolysiloxane having two or more silicon-bonded hydrogen atoms, i.e., Si—H groups, in one molecule: the ratio of the number of Si—H groups in the component (B) to the number of alkenyl groups in the component (A) is 1 to 5, and (C) Platinum group metal catalyst: The content of the platinum group metal is 1 to 100 ppm by mass relative to the total mass of the composition. 2 . The addition reaction-curable organopolysiloxane composition according to claim 1 , further comprising 0.01 to 5 parts by mass of a reaction control agent (D) based on 100 parts by mass of the component (A). 3 .
3. The addition reaction-curable organopolysiloxane composition according to claim 1 or 2, wherein The component (A) has the (meth)acrylic group in a side chain.
4. The addition reaction-curable organopolysiloxane composition according to claim 1 or 2, wherein The amount of the component (C) is such that the platinum group metal content is 5 to 40 ppm by mass relative to the total mass of the composition. 5 . The addition reaction-curing organopolysiloxane composition according to claim 1 , which is used for release paper or release film. 6 . A release paper comprising a film comprising a cured product of the addition reaction-curing organopolysiloxane composition according to claim 1 . 7 . A release film comprising a film comprising a cured product of the addition reaction-curing organopolysiloxane composition according to claim 1 .
Citation Information
Patent Citations
Radiationncurable silicone release composition
JP1979162787A
Silicone dissociable coating composition
JP2009513740A
Curable organopolysiloxane composition
JP1978118453A