Catalysts for exhaust gas purification

By forming a high proportion of high aspect ratio pores in the low-porosity catalyst coating layer, the problems of catalyst coating layer thickness and catalytic performance are solved, and high-efficiency catalytic performance and low pressure loss are achieved when the catalyst coating amount is increased.

CN115702042BActive Publication Date: 2024-10-29CATALER CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180042502.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-08
Publication Date
2024-10-29
Estimated Expiration
2041-06-08

AI Technical Summary

Technical Problem

Existing catalyst coating layers with high porosity have problems such as increased thickness and large pressure loss when the catalyst coating amount increases, or the catalytic performance cannot be fully exerted when the coating amount decreases.

Method used

By forming a high proportion of high aspect ratio pores with an equivalent circular diameter of 2 to 50 μm and an aspect ratio of 5 or more in the low porosity catalyst coating layer, the thickness of the catalyst coating layer is ensured to be between 25 and 150 μm. The porosity ranges from 1.5 to 8.0% to optimize catalyst distribution and gas diffusivity.

Benefits of technology

It is achieved that even when the catalyst coating amount increases, the thickness of the catalyst coating layer is thin, which can exert higher catalytic performance, reduce pressure loss, and at the same time improve gas diffusivity and the contact opportunities between catalytic active points and gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003998337660000201
    Figure BDA0003998337660000201
Patent Text Reader

Abstract

A catalyst for purifying exhaust gas, comprising a substrate and a catalyst coating layer containing catalyst particles formed on the surface of the substrate, wherein the average thickness of the catalyst coating layer is in the range of 25 to 150 μm, the porosity of the cross section of the catalyst coating layer determined by scanning electron microscope (SEM) observation is in the range of 1.5 to 8.0 volume %, 60 to 90 volume % of the entire voids in the catalyst coating layer are composed of high aspect ratio pores having an equivalent circle diameter of pores in the range of 2 to 50 μm and an aspect ratio of 5 or more in a cross-sectional image of the cross section of the catalyst coating layer perpendicular to the flow direction of the exhaust gas of the substrate, the average aspect ratio of the high aspect ratio pores is in the range of 10 to 50, and a precious metal is loaded on the entire catalyst coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an exhaust gas-purifying catalyst, and more particularly, to an exhaust gas-purifying catalyst including a catalyst coating layer formed on a surface of a substrate. Background Art

[0002] In the past, as exhaust gas purification catalysts installed in automobiles, etc., in order to purify harmful components such as harmful gases (hydrocarbons (HC), carbon monoxide (CO), nitrogen oxides (NOx)) contained in the exhaust gas, three-way catalysts, oxidation catalysts, NOx storage reduction catalysts, etc. have been developed.

[0003] For example, International Publication No. 2016 / 136560 (Patent Document 1) discloses an exhaust gas purification catalyst, which comprises a substrate and a catalyst coating layer containing catalyst particles formed on the surface of the substrate, wherein the average thickness of the catalyst coating layer is in the range of 25 to 160 μm, the porosity of the catalyst coating layer measured by the water weight method is in the range of 50 to 80 volume %, and 0.5 to 50 volume % of the entire voids of the catalyst coating layer are composed of high aspect ratio pores having an equivalent circle diameter of 2 to 50 μm and an aspect ratio of 5 or more in a cross-sectional image of a cross section of the catalyst coating layer perpendicular to the flow direction of the exhaust gas of the substrate, and the average aspect ratio of the high aspect ratio pores is in the range of 10 to 50. In addition, Patent Document 1 states that the exhaust gas purification catalyst exhibits excellent catalytic performance even in a high-load region with a high gas flow rate.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2016 / 136560 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, in a catalyst coating layer with a high porosity, when the amount of catalyst coating is increased, there is a problem that the catalyst coating layer becomes thicker and the pressure loss becomes larger. In addition, in a catalyst coating layer with a high porosity, when the catalyst coating layer is thinned, the amount of catalyst coating is reduced, so there is a problem that sufficient catalytic performance cannot be exerted. In addition, when the porosity of the catalyst coating layer is reduced in order to thin the thickness of the catalyst coating layer with an increased amount of catalyst coating, there is a problem that sufficient catalytic performance cannot be exerted.

[0009] The present invention has been made in view of the above-mentioned problems in the prior art, and an object of the present invention is to provide an exhaust gas purifying catalyst which can exhibit high catalytic performance by reducing the thickness of the catalyst coating layer even when the amount of catalyst coating is increased.

[0010] Methods used to solve problems

[0011] The present inventors have repeatedly conducted intensive studies to achieve the above-mentioned purpose, and as a result, have found that by forming high aspect ratio pores having a specific equivalent circle diameter and a specific aspect ratio in a catalyst coating layer having a low porosity at a high ratio relative to the overall voids of the above-mentioned catalyst coating layer, it is possible to obtain a catalyst for purifying exhaust gas that is thin in thickness and can exhibit high catalytic performance even when the catalyst coating amount is increased, thereby completing the present invention.

[0012] That is, the exhaust gas purification catalyst of the present invention comprises a substrate and a catalyst coating layer containing catalyst particles formed on the surface of the substrate, the average thickness of the above-mentioned catalyst coating layer is in the range of 25 to 150 μm, the porosity of the cross section of the above-mentioned catalyst coating layer obtained by scanning electron microscope (SEM) observation is in the range of 1.5 to 8.0 volume %, 60 to 90 volume % of the entire voids in the above-mentioned catalyst coating layer are composed of high aspect ratio pores having an equivalent circle diameter of pores in the range of 2 to 50 μm and an aspect ratio of 5 or more in a cross-sectional image of the cross section of the catalyst coating layer perpendicular to the flow direction of the exhaust gas of the above-mentioned substrate, the average aspect ratio of the above-mentioned high aspect ratio pores is in the range of 10 to 50, and the above-mentioned catalyst coating layer is loaded with a precious metal as a whole.

[0013] In the exhaust gas-purifying catalyst of the present invention, the porosity of the catalyst coating layer is preferably in the range of 1.6 to 7.0 volume %.

[0014] In the exhaust gas purifying catalyst of the present invention, preferably, 70-90% by volume of the entire voids in the catalyst coating layer are constituted by the high aspect ratio pores, and the average aspect ratio of the high aspect ratio pores is in the range of 10-35.

[0015] Furthermore, in the exhaust gas-purifying catalyst of the present invention, it is preferred that the coating amount of the catalyst coating layer is in the range of 50 to 300 g / L per unit volume of the substrate.

[0016] It should be noted that the reason why the catalyst for exhaust gas purification of the present invention has a thin catalyst coating layer and can exert a higher catalytic performance even when the amount of catalyst coating is increased is not necessarily clear, but the inventors speculate as follows. That is, the catalyst for exhaust gas purification of the present invention has a catalyst coating layer with a low porosity. The catalyst coating layer with a low porosity is dense and thin, so it can suppress pressure loss, but in the previous dense catalyst coating layer, the diffusion of gas into the interior of the layer is insufficient, so it is impossible to exert a full catalytic performance. On the other hand, it is speculated that in the catalyst for exhaust gas purification of the present invention, in such a dense catalyst coating layer, the above-mentioned high aspect ratio pores are formed in a high proportion relative to the overall voids. Therefore, compared with the previous dense catalyst coating layer, the diffusion of gas into the interior of the layer is excellent, and the precious metal (catalytic active site) loaded on the inside of the catalyst coating layer has an increased chance of contact with the gas, thereby being able to exert a higher catalytic performance.

[0017] Effects of the Invention

[0018] According to the present invention, it is possible to obtain an exhaust gas purifying catalyst which can exhibit high catalytic performance while having a thin catalyst coating layer even when the catalyst coating amount is increased. DETAILED DESCRIPTION

[0019] Hereinafter, the present invention will be described in detail based on preferred embodiments of the present invention.

[0020] The exhaust gas purification catalyst of the present invention comprises a substrate and a catalyst coating layer containing catalyst particles formed on the surface of the substrate, the average thickness of the catalyst coating layer is in the range of 25 to 150 μm, the porosity of the cross section of the catalyst coating layer obtained by scanning electron microscope (SEM) observation is in the range of 1.5 to 8.0 volume %, 60 to 90 volume % of the total voids in the catalyst coating layer are composed of high aspect ratio pores having an equivalent circle diameter of pores in the range of 2 to 50 μm and an aspect ratio of 5 or more in a cross-sectional image of the cross section of the catalyst coating layer perpendicular to the flow direction of the exhaust gas of the substrate, the average aspect ratio of the high aspect ratio pores is in the range of 10 to 50, and the catalyst coating layer as a whole is loaded with a precious metal.

[0021] (Base material)

[0022] As the substrate in the exhaust gas purification catalyst of the present invention, there is no particular limitation, and a known substrate that can be used as a substrate for the exhaust gas purification catalyst can be listed, among which a honeycomb-shaped substrate is preferred. As such a honeycomb-shaped substrate, there is no particular limitation, and a known honeycomb-shaped substrate that can be used as a substrate for the exhaust gas purification catalyst can be listed, among which a honeycomb-shaped monolithic substrate (honeycomb filter, high-density honeycomb, etc.) is preferred. In addition, the material of such a substrate is not particularly limited, and a substrate composed of ceramics such as cordierite, silicon carbide, silicon dioxide, alumina, and mullite, and a substrate composed of metals such as stainless steel containing chromium and aluminum can be listed, among which cordierite is preferred from the perspective of cost.

[0023] (Catalyst coating layer)

[0024] The catalyst coating layer in the exhaust gas purification catalyst of the present invention is formed on the surface of the substrate and contains catalyst particles, preferably composed of catalyst particles. There is no particular limitation on the catalyst particles forming the catalyst coating layer as long as they have exhaust gas purification performance. Examples thereof include a catalyst particle formed of aluminum oxide (Al 2 O 3 , aluminum oxide), cerium oxide (CeO 2 , cerium dioxide), zirconium oxide (ZrO 2 , zirconium dioxide), silicon oxide (SiO 2 , silicon dioxide), yttrium oxide (Y 2 O 3 , yttrium trioxide), neodymium oxide (Nd 2 O 3 ) or their composite oxides, etc., on catalyst substrate particles (oxide particles (preferably porous oxide particles)) on which a noble metal is supported. These catalyst particles may be used alone or in combination of two or more.

[0025] It should be noted that the “composed of catalyst particles” of the above-mentioned catalyst coating layer means that the above-mentioned catalyst coating layer is composed only of catalyst particles or mainly of catalyst particles, and contains other components within the scope that does not impair the effect of the present invention. As other components, other metal oxides, additives, etc. used as catalyst coating layers for such purposes can be listed, for example, alkali metals such as potassium (K), sodium (Na), lithium (Li), cesium (Cs), alkaline earth metals such as barium (Ba), calcium (Ca), strontium (Sr), rare earth elements such as lanthanum (La), yttrium (Y), cerium (Ce), transition metals such as iron (Fe), etc. can be listed. These components can be used alone or in combination of two or more.

[0026] As the above-mentioned precious metal, there is no particular limitation, and examples thereof include platinum (Pt), palladium (Pd), rhodium (Rh), gold (Au), silver (Ag), iridium (Ir), and ruthenium (Ru). One of these precious metals may be used alone, or two or more may be used in combination. In addition, among these precious metals, from the viewpoint of catalytic performance, Pt, Rh, Pd, Ir, and Ru are preferred, and Pt, Rh, and Pd are particularly preferred. In the exhaust gas purification catalyst of the present invention, by making such precious metals loaded on the entire catalyst coating layer, a higher catalytic performance can be exerted. On the other hand, the exhaust gas purification catalyst in which the precious metal is loaded on a part of the catalyst substrate particles in the catalyst coating layer cannot exert sufficient catalytic performance.

[0027] In the exhaust gas purification catalyst of the present invention, the coating amount of the catalyst coating layer (the coating amount of the catalyst substrate particles) is preferably in the range of 50 to 300 g / L per unit volume of the substrate, more preferably in the range of 50 to 250 g / L, and particularly preferably in the range of 50 to 200 g / L. When the coating amount of the catalyst coating layer is less than the lower limit, the catalytic activity of the catalyst particles cannot be fully obtained, and thus there is a tendency that the catalytic performance cannot be fully exerted. On the other hand, when the upper limit is exceeded, the catalyst coating layer becomes thicker, and thus there is a tendency that the pressure loss increases and the fuel efficiency deteriorates.

[0028] In addition, in the exhaust gas purification catalyst of the present invention, the coating amount of the above-mentioned noble metal is preferably in the range of 0.05 to 10 g / L per unit volume of the above-mentioned substrate, more preferably in the range of 0.1 to 10 g / L, and particularly preferably in the range of 0.1 to 5 g / L. When the coating amount of the above-mentioned noble metal is less than the above-mentioned lower limit, the catalytic activity cannot be fully obtained, and there is a tendency that sufficient catalytic performance cannot be exerted. On the other hand, when it exceeds the above-mentioned upper limit, the catalytic activity is saturated, and there is a tendency that the cost increases.

[0029] The catalyst coating layer in the exhaust gas purification catalyst of the present invention needs to have an average thickness in the range of 25 to 150 μm. When the average thickness of the catalyst coating layer is less than the lower limit, the catalytic activity of the catalyst particles cannot be fully obtained, and therefore the catalytic performance cannot be fully exerted. On the other hand, when the upper limit is exceeded, the pressure loss when the exhaust gas passes through becomes large, and the catalytic performance cannot be fully exerted. In addition, from the perspective of the balance between pressure loss, catalytic performance and durability, the average thickness of the catalyst coating layer is preferably in the range of 50 to 100 μm, and particularly preferably in the range of 70 to 90 μm. It should be noted that the average thickness of the catalyst coating layer can be obtained by the following method: observe the radial cross-section of the substrate of the catalyst coating layer using a scanning electron microscope, an optical microscope, etc., and measure the thickness of the catalyst coating layer at 10 randomly extracted locations in the obtained microscope photograph, and average them.

[0030] In addition, the above-mentioned catalyst coating layer in the exhaust gas purification catalyst of the present invention needs to have a porosity in the range of 1.5 to 8.0 volume %. When the porosity of the above-mentioned catalyst coating layer is less than the above-mentioned lower limit, the diffusion of the gas into the inside of the above-mentioned catalyst coating layer is reduced, and therefore the catalytic performance cannot be fully exerted. On the other hand, when it exceeds the above-mentioned upper limit, the coating amount of the above-mentioned catalyst particles becomes less, so the catalytic activity cannot be fully obtained, and the catalytic performance cannot be fully exerted. In addition, from the viewpoint of the balance between gas diffusivity and catalytic activity, the porosity of the above-mentioned catalyst coating layer is preferably in the range of 1.6 to 7.0 volume %, and particularly preferably in the range of 3.0 to 7.0 volume %. It should be noted that the porosity of the above-mentioned catalyst coating layer can be obtained by the following method: using a scanning electron microscope to observe the cross section of the substrate of the above-mentioned catalyst coating layer in the flow direction of the exhaust gas, for the obtained SEM image, using the difference in brightness between the pores and the catalyst component, using commercially available image analysis software (for example, two-dimensional image analysis software "WinROOF" manufactured by Mitani Shoji Co., Ltd.) to perform binarization processing, extract the pores, for more than three shooting fields of view, calculate the ratio of the area occupied by the pore part relative to the shooting field of view, and average them. In addition, there is no particular limitation on the shape of the voids, for example, it can be any one of spherical, elliptical, cylindrical, rectangular (prism), disc, channel shape and shapes similar to them. In addition, such voids include micropores with an equivalent circle diameter of less than 2 μm in the cross section, high aspect ratio pores with an equivalent circle diameter of 2 μm or more in the cross section and an aspect ratio of 5 or more, and pores with an equivalent circle diameter of 2 μm or more in the cross section and an aspect ratio of less than 5.

[0031] In addition, the catalyst coating layer in the exhaust gas purification catalyst of the present invention requires that 60 to 90% by volume of the entire voids be composed of high aspect ratio pores having an equivalent circle diameter of 2 to 50 μm in a cross-sectional image of a cross section of the catalyst coating layer perpendicular to the flow direction of the exhaust gas of the substrate and an aspect ratio of 5 or more. When the proportion of the high aspect ratio pores in the entire voids is less than the lower limit, the gas diffusibility into the inside of the catalyst coating layer is reduced, so that the catalytic performance cannot be fully exerted. On the other hand, when it exceeds the upper limit, the proportion of gas that directly passes through the catalyst coating layer without contacting the catalytic active point increases, and the catalytic performance cannot be fully exerted. In addition, from the viewpoint of the balance between the gas diffusibility and the contact efficiency with the catalytic active point, the proportion of the high aspect ratio pores in the entire voids is preferably in the range of 70 to 90% by volume, and particularly preferably in the range of 75 to 89% by volume. It should be noted that the proportion of the above-mentioned high aspect ratio pores in the overall voids can be calculated by the following method: the porosity generated by the high aspect ratio pores in the above-mentioned catalyst coating layer is measured according to the method recorded in International Publication No. 2016 / 136560, and the porosity generated by the high aspect ratio pores is divided by the porosity of the above-mentioned catalyst coating layer (porosity generated by the high aspect ratio pores / porosity of the catalyst coating layer).

[0032] In addition, the above-mentioned catalyst coating layer in the exhaust gas purification catalyst of the present invention requires that the average aspect ratio of the above-mentioned high aspect ratio pores is in the range of 10 to 50. When the average aspect ratio of the above-mentioned high aspect ratio pores is less than the above-mentioned lower limit, the connectivity of the pores cannot be fully obtained. On the other hand, when it exceeds the above-mentioned upper limit, the proportion of gas that does not contact the catalytic active points and directly passes through the catalyst coating layer increases, and the catalytic performance cannot be fully exerted. In addition, from the perspective of taking into account the diffusibility of the gas and the contact efficiency with the catalytic active points, the average aspect ratio of the above-mentioned high aspect ratio pores is preferably in the range of 10 to 35, and particularly preferably in the range of 10 to 30. It should be noted that the average aspect ratio of the above-mentioned high aspect ratio pores can be obtained according to the method described in International Publication No. 2016 / 136560.

[0033] [Catalysts for exhaust gas purification]

[0034] The exhaust gas purification catalyst of the present invention comprises the above-mentioned substrate and the above-mentioned catalyst coating layer containing the above-mentioned catalyst particles formed on the surface of the substrate. It should be noted that the exhaust gas purification catalyst of the present invention can be used in combination with other catalysts. As other catalysts, there are no particular restrictions, and known catalysts can be listed (for example, in the case of automobile exhaust gas purification catalysts, oxidation catalysts, NOx reduction catalysts, NOx storage reduction catalysts (NSR catalysts), lean NOx capture catalysts (LNT catalysts), NOx selective reduction catalysts (SCR catalysts), etc.). These other catalysts can be used alone or in combination of two or more.

[0035] (Method for producing exhaust gas purifying catalyst)

[0036] The exhaust gas purification catalyst of the present invention can be manufactured, for example, by the following method. That is, first, the catalyst substrate particles having an average particle size of 0.5 to 4 μm (hereinafter referred to as "catalyst substrate particles A"), the catalyst substrate particles having an average particle size of 4 to 15 μm (hereinafter referred to as "catalyst substrate particles B"), a precious metal raw material and a pore-forming material are mixed to prepare a catalyst slurry, the catalyst slurry is applied to the surface of the substrate to form a catalyst slurry layer, the catalyst slurry layer is calcined, and the pore-forming material is removed, thereby obtaining the exhaust gas purification catalyst of the present invention having the catalyst coating layer formed on the substrate.

[0037] (Catalyst slurry preparation)

[0038] In the method for producing the exhaust gas purification catalyst, the catalyst substrate particles A having an average particle size of 0.5 to 4 μm and the catalyst substrate particles B having an average particle size of 4 to 15 μm are used. Thus, a dense catalyst coating layer having a porosity within the above range can be formed. On the other hand, when only the catalyst substrate particles A are used, the catalyst coating layer is easily shrunk, and there is a tendency that the catalyst coating layer is easily peeled off. On the other hand, when only the catalyst substrate particles B are used, the catalyst coating layer becomes thicker, so the pressure loss when the exhaust gas passes through becomes larger, and there is a tendency that the catalytic performance cannot be fully exerted. In addition, as the average particle size of the catalyst substrate particles A and B, from the viewpoint of being able to form a thinner and denser catalyst coating layer, the average particle size of the catalyst substrate particles A is preferably in the range of 1.0 to 3.0 μm, and the average particle size of the catalyst substrate particles B is preferably in the range of 4.0 to 7.0 μm.

[0039] As the mixing ratio of the catalyst substrate particles A and the catalyst substrate particles B, the mass ratio (A / B) is preferably in the range of 1 / 10 to 10 / 1, more preferably in the range of 1 / 5 to 5 / 1, and particularly preferably in the range of 1 / 3 to 3 / 1. When the mass ratio (A / B) is less than the lower limit, the catalyst coating layer becomes thicker, and therefore, the pressure loss when the exhaust gas passes through becomes larger, and there is a tendency that the catalytic performance cannot be fully exerted. On the other hand, when it exceeds the upper limit, there is a tendency that the catalyst coating layer is easily peeled off.

[0040] There are no particular restrictions on the precious metal raw materials used in the method for producing the above-mentioned exhaust gas purification catalyst, and examples thereof include solutions obtained by dissolving salts (e.g., acetates, carbonates, nitrates, ammonium salts, citrates, dinitrodiamine salts, etc.) of precious metals (e.g., Pt, Rh, Pd, Ru, etc. or their compounds) or their complexes (e.g., tetraamine complexes) in solvents such as water and alcohol. The content of the above-mentioned precious metal raw materials in the above-mentioned catalyst slurry is not particularly limited, and can be appropriately set according to the loading amount of the precious metal in the catalyst coating layer. It is preferably in the range of 0.1 to 10 parts by mass, more preferably in the range of 0.1 to 5 parts by mass, and particularly preferably in the range of 0.1 to 3 parts by mass, relative to 100 parts by mass of the total amount of the above-mentioned catalyst substrate particles A and the above-mentioned catalyst substrate particles B, in terms of metal conversion.

[0041] The pore-forming material used in the method for producing the above-mentioned exhaust gas purification catalyst is not particularly limited as long as it is a substance that can be removed by the calcination treatment described later, and examples thereof include fibrous organic substances such as polyethylene terephthalate (PET) fibers, acrylic fibers, nylon fibers, rayon fibers, and cellulose fibers. One of these fibrous organic substances can be used alone, or two or more can be used in combination. In addition, among these fibrous organic substances, PET fibers and nylon fibers are preferred from the perspective of the balance between processability and calcination temperature. By making the catalyst slurry contain such a pore-forming material and removing the pore-forming material by a subsequent calcination treatment, a void having the same shape as that of the pore-forming material can be formed in the catalyst coating layer. The voids thus formed become diffusion paths for the exhaust gas, and a higher catalytic performance is exerted even in a dense catalyst coating layer.

[0042] The average diameter of such a pore-forming material is preferably in the range of 1.7 to 8.0 μm, more preferably in the range of 2.0 to 6.0 μm, and particularly preferably in the range of 2.0 to 5.0 μm. When the average diameter of the pore-forming material is less than the lower limit, the equivalent circle diameter of the cross section of the high aspect ratio pores becomes smaller, and the diffusibility of the gas into the catalyst coating layer decreases, so there is a tendency that sufficient catalytic performance cannot be exerted. On the other hand, when it exceeds the upper limit, the equivalent circle diameter of the cross section of the high aspect ratio pores becomes larger, so the proportion of gas that directly passes through the catalyst coating layer without contacting the catalytic active point increases, and there is a tendency that sufficient catalytic performance cannot be exerted.

[0043] In addition, the average length of the pore-forming material is preferably in the range of 15 to 150 μm, more preferably in the range of 15 to 120 μm, and particularly preferably in the range of 20 to 120 μm. When the average length of the pore-forming material is less than the lower limit, the average aspect ratio of the high aspect ratio pores becomes smaller, and there is a tendency that the connectivity of the pores cannot be sufficiently obtained. On the other hand, when it exceeds the upper limit, the average aspect ratio of the high aspect ratio pores becomes larger, and the proportion of gas that directly passes through the catalyst coating layer without contacting the catalytic active sites increases, and there is a tendency that sufficient catalytic performance cannot be exerted.

[0044] In addition, the average aspect ratio of the pore-forming material is preferably in the range of 9 to 50, more preferably in the range of 9 to 35, and particularly preferably in the range of 9 to 30. When the average aspect ratio of the pore-forming material is less than the lower limit, the average aspect ratio of the high aspect ratio pores becomes smaller, and there is a tendency that the connectivity of the pores cannot be fully obtained. On the other hand, when it exceeds the upper limit, the average aspect ratio of the high aspect ratio pores becomes larger, and the proportion of gas that directly passes through the catalyst coating layer without contacting the catalytic active point increases, and there is a tendency that sufficient catalytic performance cannot be exerted. It should be noted that the average aspect ratio of such a pore-forming material is defined as "average length / average diameter". Here, the "length of the pore-forming material" is set to the straight line distance connecting the starting point and the end point of the pore-forming material. The average length can be obtained by measuring the lengths of 50 or more pore-forming materials randomly extracted and averaging. In addition, the average diameter can be obtained by measuring the diameters of 50 or more pore-forming materials randomly extracted and averaging.

[0045] The content of the pore-forming material in the catalyst slurry is preferably in the range of 0.5 to 4.5 parts by mass, more preferably in the range of 0.6 to 4.0 parts by mass, and particularly preferably in the range of 1.5 to 3.5 parts by mass, relative to 100 parts by mass of the total amount of the catalyst substrate particles A and the catalyst substrate particles B. When the content of the pore-forming material is less than the lower limit, the proportion of the high aspect ratio pores in the entire void becomes smaller, and the diffusibility of the gas into the catalyst coating layer decreases, so there is a tendency that the catalytic performance cannot be fully exerted. On the other hand, when the upper limit is exceeded, the proportion of the gas that directly passes through the catalyst coating layer without contacting the catalytic active point increases, and there is a tendency that the catalytic performance cannot be fully exerted.

[0046] There is no particular limitation on the method for preparing the catalyst slurry. For example, the catalyst substrate particles A, the catalyst substrate particles B, the noble metal raw material and the pore-forming material may be mixed. A known mixing method may be used as appropriate. There is no particular limitation on the mixing conditions as long as the pore-forming material can be uniformly dispersed and mixed in the catalyst slurry. For example, the stirring speed is preferably in the range of 100 to 400 rpm and the processing time is 30 minutes or more.

[0047] In addition, as the mixing order of each component, it is necessary to mix at least the above-mentioned precious metal raw material with the above-mentioned catalyst substrate particles A and the above-mentioned catalyst substrate particles B. Thus, a catalyst coating layer loaded with precious metals in the entire layer can be formed, which can exert higher catalytic performance. Specifically, it can be listed as follows: a method of mixing the above-mentioned precious metal raw material in a dispersion containing the above-mentioned catalyst substrate particles A and the above-mentioned catalyst substrate particles B, and mixing the above-mentioned pore-forming material after loading the above-mentioned precious metal; a method of mixing the above-mentioned precious metal raw material after mixing the above-mentioned pore-forming material in a dispersion containing the above-mentioned catalyst substrate particles A and the above-mentioned catalyst substrate particles B; a method of mixing the above-mentioned precious metal raw material and the above-mentioned pore-forming material in a dispersion containing the above-mentioned catalyst substrate particles A and the above-mentioned catalyst substrate particles B at the same time; a method of mixing the above-mentioned catalyst substrate particles A, the above-mentioned catalyst substrate particles B and the above-mentioned pore-forming material in a solution containing the above-mentioned precious metal raw material; etc. On the other hand, when the above-mentioned precious metal raw material is mixed with one of the above-mentioned catalyst substrate particles A or the above-mentioned catalyst substrate particles B and loaded, sufficient catalytic performance cannot be exerted.

[0048] (Catalyst slurry layer formation)

[0049] Next, the catalyst slurry prepared in this way is applied to the surface of the substrate to form a catalyst slurry layer. There are no particular restrictions on the coating method, and known methods such as a method of immersing the substrate in the catalyst slurry for coating (immersion method), a water washing coating method, and a method of pressing the catalyst slurry using a press-in means can be cited.

[0050] In such a method for coating the catalyst slurry, the total amount of the coating amount of the catalyst substrate particles A and the catalyst substrate particles B is preferably in the range of 50 to 300 g / L per unit volume of the substrate, more preferably in the range of 50 to 250 g / L, and particularly preferably in the range of 50 to 200 g / L. When the coating amount of the catalyst slurry is less than the lower limit, the catalytic activity of the catalyst particles cannot be fully obtained, and thus there is a tendency that the catalytic performance cannot be fully exerted. On the other hand, when it exceeds the upper limit, the catalyst coating layer becomes thicker, the pressure loss increases, and there is a tendency that the fuel efficiency deteriorates.

[0051] In addition, the coating amount of the above-mentioned precious metal raw material is preferably in the range of 0.05 to 10 g / L per unit volume of the above-mentioned substrate in terms of metal conversion, more preferably in the range of 0.1 to 10 g / L, and particularly preferably in the range of 0.1 to 5 g / L. When the coating amount of the above-mentioned precious metal raw material is less than the above-mentioned lower limit, the catalytic activity cannot be fully obtained, and there is a tendency that sufficient catalytic performance cannot be exerted. On the other hand, when it exceeds the above-mentioned upper limit, the catalytic activity is saturated, and there is a tendency that the cost increases.

[0052] In addition, the coating amount of the pore-forming material is preferably in the range of 0.25 to 13.5 g / L, more preferably in the range of 0.3 to 10 g / L, and particularly preferably in the range of 0.75 to 7 g / L, relative to the unit volume of the substrate. When the coating amount of the pore-forming material is less than the lower limit, the proportion of the high aspect ratio pores in the entire void becomes smaller, and the diffusibility of the gas into the catalyst coating layer decreases, so there is a tendency that the catalytic performance cannot be fully exerted. On the other hand, when it exceeds the upper limit, the proportion of the high aspect ratio pores in the entire void becomes larger, and the proportion of the gas that directly passes through the catalyst coating layer without contacting the catalytic active point increases, and there is a tendency that the catalytic performance cannot be fully exerted.

[0053] (Firing treatment)

[0054] Next, the catalyst slurry layer thus formed is subjected to a calcination treatment to remove the above-mentioned pore-forming material, thereby obtaining the exhaust gas purification catalyst of the present invention having the above-mentioned catalyst coating layer containing the above-mentioned high aspect ratio pores in a specified proportion formed on the above-mentioned substrate. The calcination temperature is preferably 300 to 800°C, and more preferably 400 to 700°C. When the above-mentioned calcination temperature is less than the above-mentioned lower limit, there is a tendency for the above-mentioned pore-forming material to remain. On the other hand, when the above-mentioned upper limit is exceeded, there is a tendency for the precious metal to be sintered. In addition, the calcination time varies depending on the above-mentioned calcination temperature and cannot be generalized. It is preferably more than 20 minutes, and more preferably 30 minutes to 2 hours. In addition, there is no particular restriction on the atmosphere in such a calcination treatment, and it is preferably air or nitrogen (N 2 ) and other inactive gases.

[0055] Example

[0056] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0057] (Example 1)

[0058] First, yttria-containing zirconium oxide particles (yttria-containing zirconium oxide powder (ZrO 2 Content: 80 mass%, Y 2 O 3 Content: 20 mass %)) 50 g of particles prepared by crushing in advance to have an average particle size of 2.5 μm), cerium oxide-zirconia solid solution particles (cerium oxide-zirconia solid solution powder (CeO 2 Content: 20 mass%, ZrO 2 Content: 80 mass %)) 50 g of particles prepared in advance by crushing to an average particle size of 2.0 μm), lanthanum oxide-containing alumina particles (lanthanum oxide-containing alumina powder (Al 2 O 3 Content: 96 mass%, La 2 O 3 Content: 4 mass %), 50 g of particles (pre-crushed and prepared in a manner to have an average particle size of 6.0 μm), 10 ml of a rhodium nitrate solution containing 0.45 g of rhodium (Rh) as a precious metal raw material in terms of metal conversion, further added with zirconium oxide balls (average diameter: 3 mm), using a stirred ball mill (manufactured by Mitsui Mining Co., Ltd.), stirring treatment was carried out under the conditions of a stirring speed of 300 rpm and a treatment time of 30 minutes, to obtain a dispersion containing the above-mentioned yttria-containing zirconium oxide particles, the above-mentioned cerium oxide-zirconium oxide solid solution particles and the above-mentioned lanthanum oxide-containing aluminum oxide particles in a mass ratio of 1:1:1.

[0059] Next, 1.5 g of polyethylene terephthalate fibers (PET fibers, average diameter: 4 μm, average length: 60 μm, average aspect ratio: 15) as a pore-forming material were added to the dispersion, and a propeller stirrer (manufactured by Azowan Co., Ltd.) was used to carry out stirring treatment under the conditions of a stirring speed of 200 rpm and a treatment time of 60 minutes to obtain a catalyst slurry containing 0.3 parts by mass of rhodium and 1.0 parts by mass of the above-mentioned PET fibers relative to 100 parts by mass of the total amount of the above-mentioned yttrium oxide-containing zirconium oxide particles, the above-mentioned cerium oxide-zirconium oxide solid solution particles and the above-mentioned lanthanum oxide-containing aluminum oxide particles.

[0060] Next, the catalyst slurry was washed and applied to a cordierite monolithic honeycomb substrate (manufactured by Japan Gaishi Co., Ltd., diameter: 30 mm, length: 50 mm, volume: 35 ml, cell shape: square, cell density: 400 cells / inch) 2 , wall thickness: 4 mil), and dried in the air at 120° C. for 2 hours. The coating and drying were repeated to form a catalyst slurry layer containing 50 g / L of the yttria-containing zirconia particles, 50 g / L of the ceria-zirconia solid solution particles, 50 g / L of the lanthanum oxide-containing alumina particle catalyst, 0.45 g / L of rhodium, and 1.5 g / L of the PET fiber per 1 L of the honeycomb substrate.

[0061] Then, the catalyst slurry layer is calcined in the atmosphere at 500°C for 2 hours to remove the above-mentioned PET fiber, and at the same time, a catalyst for exhaust gas purification is obtained, wherein a catalyst coating layer is formed on the inner wall surface of the compartment of the above-mentioned honeycomb substrate, containing 50 g / L of the above-mentioned yttria-containing zirconium oxide particles, 50 g / L of the above-mentioned cerium oxide-zirconium oxide solid solution particles, 50 g / L of the above-mentioned lanthanum oxide-containing alumina particle catalyst per 1L of the above-mentioned honeycomb substrate, and rhodium is loaded at 0.45 g / L on the entire layer.

[0062] (Example 2)

[0063] A catalyst slurry containing 0.3 parts by mass of rhodium and 2.5 parts by mass of the PET fibers per 100 parts by mass of the total amount of the yttria-containing zirconia particles, the ceria-zirconia solid solution particles, and the lanthanum oxide-containing alumina particles was prepared in the same manner as in Example 1 except that the amount of the PET fibers added was changed to 3.75 g. Using the catalyst slurry, a catalyst slurry containing 50 g / L of the yttria-containing zirconia particles, 50 g / L of the ceria-zirconia solid solution particles, and 100 parts by mass of the total amount of the yttria-containing zirconia particles, the ceria-zirconia solid solution particles, and the lanthanum oxide-containing alumina particles was formed on the honeycomb substrate. A catalyst slurry layer comprising 50 g / L of zirconium oxide solid solution particles, 50 g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide, 0.45 g / L of rhodium, and 3.75 g / L of the above-mentioned PET fiber is further obtained, and a catalyst coating layer is formed on the inner wall surface of the compartment of the above-mentioned honeycomb substrate, which contains 50 g / L of the above-mentioned yttria-containing zirconium oxide particles, 50 g / L of the above-mentioned cerium oxide-zirconium oxide solid solution particles, 50 g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide per 1 L of the above-mentioned honeycomb substrate, and rhodium is loaded on the entire layer at 0.45 g / L.

[0064] (Comparative Example 1)

[0065] The same operation as in Example 1 was performed except that the PET fiber was not added to prepare a catalyst slurry containing 0.3 parts by mass of rhodium relative to 100 parts by mass of the total amount of the yttria-containing zirconia particles, the ceria-zirconia solid solution particles, and the lanthanum oxide-containing alumina particles. The catalyst slurry was used in the same manner as in Example 1 to form a catalyst slurry containing 50 g / L of the yttria-containing zirconia particles, 50 g / L of the ceria-zirconia solid solution particles, and 100 g / L of the total amount of the yttria-containing zirconia particles, the ceria-zirconia solid solution particles, and the lanthanum oxide-containing alumina particles on the honeycomb substrate. A catalyst slurry layer comprising 50 g / L of body particles, 50 g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide, and 0.45 g / L of rhodium is further obtained, and a catalyst coating layer is formed on the inner wall surface of the compartment of the above-mentioned honeycomb substrate, which contains 50 g / L of the above-mentioned yttria-containing zirconia particles, 50 g / L of the above-mentioned cerium oxide-zirconia solid solution particles, 50 g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide per 1L of the above-mentioned honeycomb substrate, and rhodium is loaded on the entire layer at 0.45 g / L.

[0066] (Comparative Example 2)

[0067] A catalyst slurry containing 0.3 parts by mass of rhodium and 5.0 parts by mass of the PET fibers per 100 parts by mass of the total amount of the yttria-containing zirconia particles, the ceria-zirconia solid solution particles, and the lanthanum oxide-containing alumina particles was prepared in the same manner as in Example 1 except that the amount of the PET fibers added was changed to 7.5 g. Using the catalyst slurry, a catalyst slurry containing 50 g / L of the yttria-containing zirconia particles, 50 g / L of the ceria-zirconia solid solution particles, and 100 parts by mass of the total amount of the lanthanum oxide-containing alumina particles was formed on the honeycomb substrate. A catalyst slurry layer comprising 50 g / L of zirconium oxide solid solution particles, 50 g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide, 0.45 g / L of rhodium, and 7.5 g / L of the above-mentioned PET fiber is further obtained, and a catalyst coating layer is formed on the inner wall surface of the compartment of the above-mentioned honeycomb substrate, which contains 50 g / L of the above-mentioned yttria-containing zirconium oxide particles, 50 g / L of the above-mentioned cerium oxide-zirconium oxide solid solution particles, 50 g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide per 1 L of the above-mentioned honeycomb substrate, and rhodium is loaded on the entire layer at 0.45 g / L.

[0068] (Comparative Example 3)

[0069] First, 20 ml of a rhodium nitrate solution containing 0.9 g of rhodium (Rh) as a precious metal raw material was impregnated into yttria-containing zirconium oxide particles (yttria-containing zirconium oxide powder (ZrO 2 Content: 80 mass%, Y 2 O 3 The mixture was added with 100 g of particles (pre-crushed to give an average particle size of 2.5 μm) and then dried at 110° C. in the air for 12 hours and further calcined at 500° C. in the air for 3 hours to obtain yttria-containing zirconia particles loaded with rhodium (rhodium loading amount relative to 100 parts by mass of yttria-containing zirconia particles: 0.9 parts by mass).

[0070] Next, 50 g of the above-mentioned rhodium-loaded yttria-containing zirconium oxide particles and cerium oxide-zirconia solid solution particles (the cerium oxide-zirconia solid solution powder (CeO 2 Content: 20 mass%, ZrO 2 Content: 80 mass %)) 50 g of particles prepared in advance by crushing to an average particle size of 2.0 μm), lanthanum oxide-containing alumina particles (lanthanum oxide-containing alumina powder (Al 2 O 3 Content: 96 mass%, La 2 O 3The mixture was stirred at a speed of 300 rpm and for 30 minutes using a stirred ball mill to obtain a dispersion containing the above-mentioned rhodium-loaded yttria-containing zirconia particles, the above-mentioned cerium oxide-zirconia solid solution particles and the above-mentioned lanthanum oxide-containing alumina particles in a mass ratio of 1:1:1.

[0071] Next, 3.75 g of polyethylene terephthalate fibers (PET fibers, average diameter: 4 μm, average length: 60 μm, average aspect ratio: 15) as a pore-forming material were added to the dispersion, and a propeller stirrer (manufactured by Azowan Co., Ltd.) was used to carry out stirring treatment under the conditions of a stirring speed of 200 rpm and a treatment time of 60 minutes to obtain a catalyst slurry containing 2.5 parts by mass of the above-mentioned PET fibers relative to 100 parts by mass of the total amount of the above-mentioned rhodium-loaded yttria-containing zirconium oxide particles, the above-mentioned cerium oxide-zirconia solid solution particles, and the above-mentioned lanthanum oxide-containing alumina particles.

[0072] Next, except for using the catalyst slurry, the same operation as in Example 1 was performed to form a catalyst slurry layer containing 50 g / L of the above-mentioned rhodium-loaded yttria-containing zirconium oxide particles, 50 g / L of the above-mentioned cerium oxide-zirconia solid solution particles, 50 g / L of the above-mentioned lanthanum oxide-containing alumina particle catalyst, and 3.75 g / L of the above-mentioned PET fiber per 1L of the above-mentioned honeycomb substrate, and further to obtain an exhaust gas purification catalyst having a catalyst coating layer formed on the inner wall surface of the compartment of the above-mentioned honeycomb substrate containing 50 g / L of the above-mentioned rhodium-loaded yttria-containing zirconium oxide particles, 50 g / L of the above-mentioned cerium oxide-zirconia solid solution particles, and 50 g / L of the above-mentioned lanthanum oxide-containing alumina particle catalyst per 1L of the above-mentioned honeycomb substrate. It should be noted that the rhodium loading amount in the above-mentioned catalyst slurry layer and the above-mentioned catalyst coating layer is 0.45 g / L per 1L of the above-mentioned honeycomb substrate.

[0073] (Comparative Example 4)

[0074] Instead of the yttria-containing zirconium oxide particles having an average particle size of 2.5 μm, yttria-containing zirconium oxide powder (ZrO 2 Content: 80 mass%, Y 2 O 3 Yttria-containing zirconium oxide particles prepared by pulverizing in advance to have an average particle size of 5.0 μm were used instead of the above-mentioned cerium oxide-zirconia solid solution particles having an average particle size of 2.0 μm, and cerium oxide-zirconia solid solution powder (CeO 2 Content: 20 mass%, ZrO2 The catalyst slurry containing 0.3 parts by mass of rhodium and 2.5 parts by mass of the PET fiber is prepared in the same manner as in Example 2, with respect to 100 parts by mass of the total amount of the yttria-containing zirconia particles, the cerium oxide-zirconia solid solution particles and the lanthanum oxide-containing alumina particles. The catalyst slurry is used in the same manner as in Example 2, with respect to each 1L of the honeycomb substrate, to form a catalyst slurry containing 0.3 parts by mass of rhodium and 2.5 parts by mass of the PET fiber. The catalyst slurry layer comprises 50g / L of the above-mentioned cerium oxide-zirconia solid solution particles, 50g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide, 0.45g / L of rhodium, and 3.75g / L of the above-mentioned PET fiber, and further obtains a catalyst for exhaust gas purification having a catalyst coating layer formed on the inner wall surface of the compartment of the above-mentioned honeycomb substrate, which contains 50g / L of the above-mentioned yttria-containing zirconium oxide particles, 50g / L of the above-mentioned cerium oxide-zirconia solid solution particles, 50g / L of the above-mentioned alumina particle catalyst containing lanthanum oxide per 1L of the above-mentioned honeycomb substrate, and rhodium is loaded on the entire layer at 0.45g / L.

[0075] <Average thickness of catalyst coating layer>

[0076] The obtained exhaust gas purification catalyst was embedded in epoxy resin, the embedded material was cut along the radial direction of the honeycomb substrate, the obtained cross section was ground, and observed using a scanning electron microscope ("S-4800" manufactured by Hitachi High-Technologies Corporation) (measurement magnification: 1300 times). In the obtained SEM image, the thickness of the catalyst coating layer at 10 randomly extracted locations was measured, and the average thickness of the catalyst coating layer was calculated by averaging them. The results are shown in Table 1.

[0077] <Porosity of Catalyst Coating Layer>

[0078] The obtained catalyst for exhaust gas purification was cut along the flow direction of the exhaust gas of the honeycomb substrate, the obtained cross section was ground, and observed using a scanning electron microscope ("S-4800" manufactured by Hitachi High-Technologies Co., Ltd.) (output: 15 kV, measurement magnification: 3000 times). For the obtained SEM image, the difference in brightness between the pores and the catalyst component was used to perform binarization processing using commercially available image analysis software (two-dimensional image analysis software "WinROOF" manufactured by Mitani Shoji Co., Ltd.), extract the pores, and calculate the ratio of the area occupied by the pore portion relative to the shooting field of view (30 μm in length and 40 μm in width). The ratio of the area occupied by such pores is calculated for more than 3 fields of view, and the average value is used as the porosity of the catalyst coating layer. The results are shown in Table 1.

[0079] <Average aspect ratio of high aspect ratio pores>

[0080] The equivalent circle diameter and aspect ratio of each pore in the catalyst coating layer of the obtained exhaust gas purification catalyst were measured according to the method described in International Publication No. 2016 / 136560, and the average aspect ratio of pores (high aspect ratio pores) with an equivalent circle diameter in the range of 2 to 50 μm and an aspect ratio of 5 or more was obtained. The results are shown in Table 1.

[0081] <Porosity due to high aspect ratio pores>

[0082] The porosity caused by the high aspect ratio pores in the catalyst coating layer of the obtained exhaust gas purifying catalyst was measured according to the method described in International Publication No. 2016 / 136560. The results are shown in Table 1.

[0083] <Ratio of high aspect ratio pores in total voids>

[0084] The ratio of high aspect ratio pores to the total voids was calculated by dividing the porosity of the high aspect ratio pores by the porosity of the catalyst coating layer (= porosity of high aspect ratio pores / porosity of the catalyst coating layer).

[0085] <NOx purification rate>

[0086] First, the stoichiometric model gas [NO (3000 ppm) + C 3 H 6 (1000ppmC)+N 2 (balance)] (3 minutes) and lean model gas [NO (3000ppm) + C 3 H 6 (500ppmC)+N 2 (balance)] (1 minute) The obtained exhaust gas purifying catalyst was flowed for 50 hours while alternately switching, and a durability test was carried out.

[0087] Under the conditions of temperature 550°C and space time SV = 170,000 / s, the rich model gas [NO (3000ppm) + C 3 H 6 (3300ppmC)+N 2 The NOx purification rate was calculated by measuring the NO concentration in the catalyst inlet gas and the catalyst outlet gas through the exhaust gas purification catalyst after the durability test. The results are shown in Table 1.

[0088] [Table 1]

[0089]

[0090] *1 Particle 1: Zirconia particles containing yttria

[0091] Particle 2: Cerium oxide-zirconia solid solution particles

[0092] Particle 3: Alumina particles containing lanthanum oxide

[0093] *2 Addition amount relative to 100 parts by mass of the total amount of particles 1 to 3

[0094] As shown in Table 1, the exhaust gas purifying catalysts (Examples 1-2) having a catalyst coating layer with a predetermined porosity and containing high aspect ratio pores at a predetermined ratio have a higher NOx purification rate than the exhaust gas purifying catalyst (Comparative Example 1) having a catalyst coating layer without high aspect ratio pores and a porosity less than a predetermined range. This is considered to be because the high aspect ratio pores are present in the catalyst coating layer in the exhaust gas purifying catalysts of Examples 1-2, so the gas is sufficiently diffused into the inside of the catalyst coating layer, while the high aspect ratio pores are not present in the catalyst coating layer in the exhaust gas purifying catalyst of Comparative Example 1, so the gas is not diffused into the inside of the catalyst coating layer.

[0095] In addition, it can be seen that the exhaust gas purification catalyst (Comparative Example 2) having a catalyst coating layer in which the proportion of high aspect ratio pores in the entire void is greater than a predetermined range has a lower NOx purification rate than the exhaust gas purification catalyst (Examples 1-2) having a catalyst coating layer containing high aspect ratio pores at a predetermined ratio. This is believed to be because the proportion of gas that directly passes through the catalyst coating layer without contacting the catalytic active site increases in the exhaust gas purification catalyst of Comparative Example 2, and the catalytic performance is not fully exerted.

[0096] In addition, it is known that the exhaust gas purification catalyst having a catalyst coating layer in which the precious metal is not supported on the entire layer (Comparative Example 3) has a lower NOx purification rate than the exhaust gas purification catalyst having the precious metal supported on the entire layer (Examples 1 and 2). This is considered to be because, in the exhaust gas purification catalyst of Comparative Example 3, even if the gas is sufficiently diffused into the inside of the catalyst coating layer, the catalytic effect is not fully exerted in the part where the precious metal is not supported.

[0097] In the exhaust gas purifying catalyst (Comparative Example 4) having a catalyst coating layer with a porosity greater than the predetermined range, the catalyst coating layer was thick. This is probably because even if the porosity is large, there are few opportunities for gas to contact the catalytic active sites.

[0098] Industrial Applicability

[0099] As described above, according to the present invention, a catalyst for purifying exhaust gas can be obtained which has a thin catalyst coating layer and can exhibit high catalytic performance even when the amount of catalyst coating is increased. Therefore, the catalyst for purifying exhaust gas of the present invention is particularly useful as a catalyst for purifying harmful components such as NOx contained in the gas exhausted from an internal combustion engine such as an automobile engine.

Claims

1. An exhaust gas purification catalyst comprising a substrate and a catalyst coating layer containing catalyst particles formed on a surface of the substrate, The average thickness of the catalyst coating layer is in the range of 25 to 150 μm. The porosity of the cross section of the catalyst coating layer determined by scanning electron microscopy is in the range of 1.5 to 8.0 volume %, 60 to 90% by volume of the entire voids in the catalyst coating layer are composed of high aspect ratio pores having an equivalent circle diameter of 2 to 50 μm and an aspect ratio of 5 or more in a cross-sectional image of a cross section of the catalyst coating layer perpendicular to the exhaust gas flow direction of the substrate, The average aspect ratio of the high aspect ratio pores is in the range of 10 to 50, The entire catalyst coating layer is loaded with a precious metal.

2. The exhaust gas purification catalyst according to claim 1, wherein The porosity of the catalyst coating layer is in the range of 1.6 to 7.0 volume %.

3. The exhaust gas purification catalyst according to claim 1 or 2, wherein: 70 to 90% by volume of the entire voids in the catalyst coating layer are constituted by the high aspect ratio pores, and the average aspect ratio of the high aspect ratio pores is in the range of 10 to 35.

4. The exhaust gas purification catalyst according to claim 1 or 2, wherein: The coating amount of the catalyst coating layer is in the range of 50 to 300 g / L per unit volume of the substrate.

Citation Information

Patent Citations

  • Catalyst support and manufacturing method therefor

    CN103796758A

  • Exhaust gas purification catalyst

    CN107427826A

  • Exhaust gas purification catalyst, manufacturing method therefor, and exhaust gas purification method using same

    WO2016136560A1