Feeding method and feeding system of propylene polymerization catalyst, polypropylene and preparation method thereof
By mixing the propylene polymerization catalyst with liquid propylene and performing metering, transportation and stirring control during the buffering process in the feeding system, the problem of uneven components and pipe blockage caused by catalyst sedimentation is solved, and the polymerization of the catalyst components is realized. The uniformity in the reactor and the stability of the process conditions improve the molecular structure and production efficiency of polypropylene.
Patent Information
- Application Number
- CN202110945969.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-08-17
AI Technical Summary
The suspension of existing propylene polymerization catalysts easily settles during the feeding process, resulting in uneven catalyst components, affecting the uniformity of the polymerization reaction and the stability of process parameters, and easily causing blockage of the feeding pipeline, affecting the normal operation of the device.
The propylene polymerization catalyst and liquid phase propylene are mixed evenly, and the components of the catalyst premix are ensured to be uniform through metering, transportation and stirring control during the buffering process, and the temperature and pressure are adjusted in the buffer tank to make them consistent with the conditions of the polymerization reactor , the feed system design includes batching tanks, metering tanks, diaphragm metering pumps, conveying pipelines and buffer tanks, with agitators and temperature and pressure regulators installed to ensure uniform catalyst components and stable conditions.
It achieves the uniformity of the catalyst components in the polymerization reactor, reduces the impact of the feeding process on the polymerization reaction, avoids pipe blockage, improves the uniformity of the molecular structure and comprehensive performance of polypropylene, and enhances production efficiency.
Smart Images

Figure CN115703055B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer preparation, and in particular relates to a feeding method and system of a propylene polymerization catalyst and a method for preparing polypropylene using the method and system. Background Art
[0002] The catalyst for propylene polymerization is generally prepared by premixing the catalyst with propylene to form a catalyst suspension, and then adding the catalyst suspension to the propylene polymerization reactor to participate in the polymerization reaction. However, since the catalyst is a solid powder, the suspension prepared with propylene is easy to settle. In the actual production process, many problems are often caused by the feeding method of the suspension. For example, the catalyst feed amount may fluctuate within a certain range due to the sedimentation of the catalyst, making the catalyst components entering the reactor at different times uneven and making the polymerization reaction of propylene uneven. In severe cases, the polymerization reactor may be locally overheated and agglomerated, which has a significant impact on the normal operation of the device; it may also cause part of the catalyst powder to accumulate in the feed pipeline due to the sedimentation of the catalyst, resulting in blockage of the catalyst feed pipeline. Furthermore, due to the above factors, the process parameters of the catalyst entering the polymerization reactor are unstable, making the process control of the polymerization reaction more difficult. In this way, in the polymerization reaction of propylene, especially in the preparation of high-performance polypropylene with a designable molecular structure, the final molecular structure of the product is unevenly distributed and has a large difference from the molecular structure of the designed product, thereby affecting the performance and quality of the final product.
[0003] In the existing literature reports, many researchers hope to solve this technical problem. For example, some people set up circulation pumps and circulation pipelines for metering tanks to keep the components of the suspension uniform by circulation; some people improve the dispersion degree of the suspension by designing a special structure of the metering tank to keep the components of the suspension uniform; however, these research results can only alleviate the sedimentation of the suspension to a certain extent, and can only ensure that the components of the catalyst suspension in the metering tank are uniform, while it is difficult to avoid the sedimentation of the material during the transportation of the catalyst suspension into the feed pipeline, and it is impossible to ensure that the components of the suspension entering the polymerization reactor are uniform and the conditions are stable, and it is also difficult to avoid pipeline blockage. Summary of the invention
[0004] Based on the above, the main purpose of the present invention is to provide a feeding method and a feeding system for a propylene polymerization catalyst. The feeding method provided by the present invention makes the catalyst components introduced into the polymerization reactor uniform and the temperature and pressure consistent with those of the polymerization reactor, minimizes the influence of the catalyst feeding process on the polymerization reaction, controls the process conditions of the polymerization reaction, obtains high-performance polypropylene with designable molecular structure, improves the uniformity and comprehensive performance of the product molecular structure, and can also avoid the blockage of the feed pipeline, improve market efficiency, and thus is more suitable for practical use.
[0005] To this end, the present invention provides a feeding method of a propylene polymerization catalyst, which comprises the following steps:
[0006] 1) uniformly mixing a propylene polymerization catalyst and liquid propylene to obtain a catalyst premix liquid;
[0007] 2) the catalyst premix liquid is metered, conveyed and buffered in sequence and then introduced into a propylene polymerization reactor to participate in a propylene polymerization reaction, wherein the components of the catalyst premix liquid are controlled to be uniform during the metering, conveying and buffering processes, and the temperature of the catalyst premix liquid during the buffering process is controlled to be the same as the temperature when participating in the propylene polymerization reaction.
[0008] In the feeding method of the present invention, it is preferred that the metering process includes stirring and circulating the catalyst premix in a metering tank and accurately metering it by a diaphragm metering pump.
[0009] In the feeding method of the present invention, it is preferred that the conveying process uses a pipeline provided with a stirrer.
[0010] In the feeding method of the present invention, it is preferred that the buffering process includes stirring and circulating the catalyst premix in a buffer tank, and then adjusting the temperature of the catalyst premix and the pressure in the buffer tank.
[0011] To this end, the present invention also provides a feeding system for a propylene polymerization catalyst, which comprises a batching tank, a metering tank, a diaphragm metering pump, a conveying pipeline and a buffer tank connected in sequence, wherein the buffer tank is connected to a propylene polymerization reaction device, and a stirrer is respectively arranged in the batching tank, the metering tank, the conveying pipeline and the buffer tank, and a temperature controller and a pressure regulator are also arranged in the buffer tank; preferably, the stirrer arranged in the conveying pipeline is a slanted-paddle stirrer, and the slanted-paddle stirrer is composed of two straight blades, and the two blades are folded 45° to 60° in opposite directions.
[0012] Specifically, a stirrer is provided on the delivery pipeline connecting the diaphragm metering pump and the buffer tank, so as to keep the components of the catalyst premix liquid uniform during the delivery process.
[0013] In the feeding system of the present invention, preferably, the metering tanks include at least two, and further preferably, the metering tanks are connected in parallel.
[0014] In the feeding system described in the present invention, preferably, a protective valve is provided between the metering tank and the diaphragm metering pump; further preferably, the diaphragm metering pump is a stroke-adjustable diaphragm metering pump.
[0015] In the feeding system of the present invention, preferably, a plurality of agitators are provided in the conveying pipeline, and further preferably, the distance between adjacent agitators is less than 2m.
[0016] To this end, the present invention also provides a method for preparing high-impact and high-gloss polypropylene, which comprises the following steps:
[0017] 1) using the above-mentioned feeding method to pass the catalyst premixed liquid into a loop reactor to carry out a first polymerization with a first olefin monomer;
[0018] 2) The catalyst premix solution is introduced into a horizontal reactor by the above-mentioned feeding method to carry out a second polymerization with the product obtained in step 1) and a second olefin monomer.
[0019] The preparation method described in the present invention is preferably that the first polymerization includes a prepolymerization reaction and a liquid phase bulk polymerization reaction occurring in sequence; the reaction temperature of the prepolymerization reaction is 10-40°C, the reaction pressure is 2.8-4.1Mpa, and the reaction time is 3-5min; the reaction temperature of the liquid phase bulk polymerization reaction is 60-80°C, and the reaction pressure is 2.7-4.0Mpa.
[0020] In the preparation method of the present invention, it is preferred that, during the prepolymerization reaction, the first olefin monomer is propylene; and during the first polymerization process, the mass concentration of the propylene polymerization catalyst in the catalyst premix is ≥50%.
[0021] In the preparation method of the present invention, it is preferred that the propylene polymerization catalyst comprises a main catalyst and a co-catalyst; wherein,
[0022] The main catalyst comprises a magnesium compound carrier, a transition metal halide, an alcohol having 2 to 15 carbon atoms and an electron donor, and the molar ratio of the four is 1: (1-40): (0.01-10): (0.01-10);
[0023] The cocatalyst comprises an organic aluminum compound; the organic aluminum compound comprises an alkyl aluminum and / or an alkyl aluminum hydrolyzate alkyl aluminumoxane;
[0024] In terms of molar ratio, the ratio of the transition metal halide to the organic aluminum compound is 1:(10-500).
[0025] In the preparation method of the present invention, it is preferred that the electron donor is selected from at least one of an organophosphorus compound, an organosilane, cyclohexylmethyldimethoxysilane, dicyclopentyldimethoxysilane, and an electron donor as shown in Formula I:
[0026]
[0027] In Formula I, R1 and R6 are each independently selected from C1-C 12 Straight chain alkyl, C3-C 12 Branched alkyl, C3-C 15 Cycloalkyl, C3-C 15 R2, R3, R4, R5 are each independently selected from H atoms, halogen, C1-C 12 Straight chain alkyl, C3-C 12 branched alkyl, C3-C8 cycloalkyl, C6-C 15 Aryl, C6-C 15 wherein R2 and R3, R3 and R4, R4 and R5 are independently connected to form a ring or not.
[0028] The preparation method of the present invention is preferably that, during the liquid phase bulk polymerization reaction, the first olefin monomer is propylene or an olefin mixture, the olefin mixture is composed of propylene with a molar percentage of ≥96% and other olefins with a molar percentage of ≤4%, and the other olefins are ethylene and / or butene.
[0029] In the preparation method of the present invention, it is preferred that, in the liquid phase bulk polymerization process, the amount of the catalyst used is 0.02-0.10% by mass of the liquid phase propylene in the first olefin monomer.
[0030] In the preparation method described in the present invention, it is preferred that the liquid phase bulk polymerization reaction adopts a polymerization reaction loop tube, and the polymerization reaction loop tube includes a plurality of polymerization loop tube units connected in parallel, and the polymerization loop tube unit includes a plurality of annular reaction tubes connected in series.
[0031] In the preparation method of the present invention, preferably, the polymerization reaction loop pipe is connected in series with the horizontal reactor.
[0032] In the preparation method of the present invention, preferably, the second olefin monomer is at least two of ethylene, propylene and butene; further preferably, the molar percentage of ethylene in the second olefin monomer is ≤60%.
[0033] In the preparation method of the present invention, preferably, the reaction temperature of the second polymerization is 60-80°C, and the reaction pressure is 2.0-3.0Mpa. Further preferably, the reaction temperature of the second polymerization is 65-75°C, and the reaction pressure is 2.4-2.5Mpa.
[0034] In the preparation method of the present invention, it is preferred that, in the second polymerization process, the amount of the catalyst in the catalyst premix is 0.02-0.10% by mass of the second olefin monomer.
[0035] In the preparation method of the present invention, preferably, the first polymerization further comprises the step of adding a first auxiliary agent, wherein the first auxiliary agent comprises a molecular weight regulator; and the second polymerization further comprises the step of adding a second auxiliary agent, wherein the second auxiliary agent comprises a molecular weight regulator.
[0036] In the preparation method described in the present invention, it is preferred that a horizontal stirring shaft is provided in the horizontal reactor, and a plurality of stirring paddles are provided on the horizontal stirring shaft.
[0037] In the preparation method described in the present invention, it is preferred that the horizontal reactor is divided into a gasification separation zone and a gas phase polymerization reaction zone along the feeding direction; a partition is arranged between the gasification separation zone and the gas phase polymerization reaction zone; and a gap is arranged between one end of the partition and the side wall of the horizontal reactor.
[0038] To this end, the present invention also provides a high-impact and high-gloss polypropylene prepared by the above method, characterized in that the room temperature impact strength is ≥60KJ / m according to ASTM D256 standard test. 2 ; Its low temperature impact strength ≥50KJ / m 2 ; According to GB / T8807 standard, its glossiness is ≥85%.
[0039] By means of the above technical scheme, the feeding method and system of the propylene polymerization catalyst, the method for preparing polypropylene using the method and system, and the polypropylene prepared by the preparation method proposed in the present invention have at least the following advantages:
[0040] 1. The feeding method of propylene polymerization catalyst proposed by the present invention comprises the following steps: firstly, the propylene polymerization catalyst is uniformly mixed with liquid propylene to obtain a catalyst premix liquid; in order to solve the technical problem that the catalyst premix liquid is easy to settle, resulting in uneven components and blocking the feeding pipeline, stirring is provided at each link through which the catalyst premix liquid flows to keep the components uniform all the time, thereby ensuring that the catalyst components entering the polymerization reactor are uniform and will not block the feeding pipeline;
[0041] 2. The feed system of the propylene polymerization catalyst proposed by the present invention enables intermittent catalyst batching to continuously feed the polymerization reactor by designing metering tanks connected in parallel; and by arranging an agitator of a pipeline structure on the delivery pipeline, it avoids the catalyst from being deposited in the feed pipeline and clogging the pipeline, thereby reducing production failures and improving production efficiency;
[0042] 3. The feed system of the propylene polymerization catalyst proposed in the present invention, by designing a buffer tank, makes the catalyst introduced into the polymerization reactor have uniform components, and the temperature and pressure are consistent with those in the polymerization reactor, thereby minimizing the influence of the feed process on the polymerization reaction process conditions, and providing a guarantee for the preparation of high-performance polypropylene with designable molecular structure;
[0043] 4. The feed system of the propylene polymerization catalyst proposed by the present invention can accurately measure the amount of catalyst introduced into the polymerization reactor by installing a diaphragm metering pump on the pipeline, thereby minimizing the influence of the feed process on the polymerization reaction process conditions, and providing a guarantee for the preparation of high-performance polypropylene with designable molecular structure;
[0044] 5. The method for preparing polypropylene proposed in the present invention prepares high-impact and high-gloss polypropylene by combining the use of a loop reactor for liquid-phase bulk polymerization of propylene and a horizontal reactor for impact copolymerization of propylene, thereby overcoming the defects of the prior art, obtaining polypropylene with good impact resistance and high gloss, and broadening the application range of polypropylene;
[0045] 6. The method for preparing polypropylene proposed by the present invention has a designable target molecular structure, and the ratio of olefin monomers can be adjusted within a wide range, thereby obtaining polypropylene with a high ethylene content;
[0046] 7. The method for preparing polypropylene proposed by the present invention accurately controls the molecular weight and molecular weight distribution of the homopolymer or random copolymer by reacting in a loop reactor; and then fully mixes the materials in the horizontal reactor without axial backmixing and in the radial direction, so that the residence time of each reaction material in the reactor is basically the same, thereby controlling the consistency of its molecular structure and improving the performance stability of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 It is a process flow diagram of a feeding method of a propylene polymerization catalyst of the present invention;
[0048] Figure 2 It is a structural schematic diagram of a feeding system of the propylene polymerization catalyst of the present invention.
[0049] Among them, 1. batching tank, 2. metering tank, 3. diaphragm metering pump, 4. agitator in the pipeline, 5. buffer tank, 6. polymerization reactor;
[0050] 21. The first metering tank, 22. The second metering tank. DETAILED DESCRIPTION
[0051] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0052] The present invention provides a feeding method of propylene polymerization catalyst, as shown in the following Figure 1 As shown, it includes the following steps:
[0053] S1 catalyst preparation: uniformly mixing the propylene polymerization catalyst and liquid propylene to obtain a catalyst premix liquid;
[0054] S2 Catalyst metering: The catalyst premix is stirred and circulated in a metering tank and accurately metered by a diaphragm metering pump and transported to a buffer tank;
[0055] S3 catalyst feed buffer: stirring and circulating the catalyst premix in the buffer tank and adjusting the temperature of the premix and the pressure in the buffer tank;
[0056] S4 Propylene polymerization reaction: The catalyst premix liquid after being stabilized in the buffer tank is introduced into the polymerization reactor for propylene polymerization reaction.
[0057] The propylene polymerization catalyst is uniformly mixed with liquid propylene to obtain a catalyst premix liquid; then the catalyst premix liquid is sequentially metered, conveyed and buffered before being introduced into a propylene polymerization reactor to participate in a propylene polymerization reaction, wherein the components of the metered, conveyed and buffered premix liquid are controlled to be uniform, and the pressure and temperature of the buffered premix liquid are controlled to be in the same range as the pressure and temperature of the propylene polymerization reaction; the catalyst premix liquid is sequentially metered, conveyed and buffered before being introduced into a propylene polymerization reactor to participate in a propylene polymerization reaction, wherein the components of the metered, conveyed and buffered premix liquid are controlled to be uniform, and the temperature of the buffered premix liquid is controlled to be in the same range as the temperature of the propylene polymerization reaction.
[0058] In order to avoid the problems caused by catalyst sedimentation, the technical solution of the present invention improves the feeding method of the propylene polymerization catalyst. First, the propylene polymerization catalyst is evenly mixed with liquid propylene to obtain a catalyst premix liquid; then, the catalyst premix liquid is continuously stirred in a metering tank, a conveying pipeline and a buffer tank to keep the premix liquid in a uniform state of components. At the same time, the temperature condition of the buffer tank is controlled to be consistent with the process conditions of the first step of the polymerization reactor, thereby reducing the influence of the catalyst feeding on the polymerization reaction process conditions, achieving stable control of the polymerization reaction conditions, and controlling the molecular structure and performance of the polymerization product.
[0059] Preferably, the metering includes stirring and circulating the catalyst premix in a metering tank and accurately metering the catalyst premix by a diaphragm metering pump.
[0060] The diaphragm metering pump uses a specially designed and processed flexible diaphragm to replace the piston, and realizes reciprocating motion under the action of the driving mechanism to complete the suction-discharge process. Due to the isolation effect of the diaphragm, the isolation between the metered fluid and the driving lubrication mechanism can be achieved in structure.
[0061] Preferably, an agitator with a pipeline structure is provided on the pipeline used for transportation.
[0062] The pipe structure agitator can force convection and uniform mixing of liquid and gas medium. It is composed of two straight blades, and the radial liquid flow velocity generated is relatively small. The two blades of the oblique blade agitator are bent 45° or 60° in opposite directions, thereby generating axial liquid flow.
[0063] Preferably, the buffering includes stirring and circulating the catalyst premix in a buffer tank and adjusting the temperature of the premix and the pressure in the buffer tank.
[0064] The present invention also provides a feeding system for propylene polymerization catalyst, as shown in the attached Figure 2 As shown, it includes:
[0065] A batching tank 1 is provided with a stirrer for uniformly mixing the propylene polymerization catalyst with the liquid propylene to obtain a catalyst premix liquid;
[0066] A metering tank 2, the inlet of which is connected to the outlet of the batching tank 1; a stirrer is provided in the metering tank 2 to keep the catalyst premix liquid uniform in composition;
[0067] A diaphragm metering pump 3, whose inlet is connected to the outlet of the metering tank 2, is used to meter the catalyst premix liquid;
[0068] A buffer tank 5, whose inlet is connected to the outlet of the diaphragm metering pump 3, and whose outlet is connected to the polymerization reactor 6; the buffer tank 5 is provided with an agitator, a temperature controller and a pressure regulator; the agitator is used to keep the catalyst premix liquid uniform in composition; the temperature controller and the pressure regulator are used to adjust the temperature of the catalyst premix liquid and the pressure in the buffer tank respectively;
[0069] The agitator 4 of the pipeline structure is arranged in the delivery pipeline connecting the diaphragm metering pump 3 and the buffer tank 5, and is used to keep the components of the catalyst premix liquid uniform during the delivery process.
[0070] Preferably, the metering tank 2 comprises at least two metering tanks connected in parallel, as shown in the attached Figure 2 As shown, the metering tank 2 includes a first metering tank 21 and a second metering tank 22 which are connected in parallel to each other.
[0071] Preferably, a protective valve is provided between the metering tank 2 and the diaphragm metering pump 3 .
[0072] Preferably, the diaphragm metering pump 3 is a stroke-adjustable diaphragm metering pump.
[0073] Preferably, a plurality of agitators 4 are provided in the conveying pipeline; and the distance between two adjacent agitators 4 is less than 2 m.
[0074] The agitator of the pipeline structure, its agitator device includes a stirring shaft that is arranged through the mixing pipe, the stirring shaft is detachably mounted with a stirring impeller, and one end of the stirring shaft extends out of the mixing pipe and is connected to a driving device. The two mixing pipes are arranged in parallel along the longitudinal direction, and expansion pipes are respectively arranged at the bottom ends of the two mixing pipes, and a connecting elbow is arranged between the bottom ends of the two expansion pipes; the diameter of the expansion pipe is larger than the diameter of the mixing pipe and the connecting elbow. The driving device includes a driving motor, and the driving motor is installed above the mixing pipe through a bracket.
[0075] The present invention also provides a method for preparing high-impact and high-gloss polypropylene, which comprises the following steps:
[0076] 1) obtaining a catalyst premix according to the aforementioned feeding method;
[0077] 2) introducing the catalyst premix into a loop reactor according to the aforementioned feeding method to carry out a first polymerization with a first olefin monomer;
[0078] 3) According to the aforementioned feeding method, the catalyst premix solution is introduced into a horizontal reactor to carry out a second polymerization with the product obtained in step 2) and a second olefin monomer.
[0079] In the loop reactor, the first olefin monomer undergoes liquid phase bulk polymerization; a first auxiliary agent may be added during the first polymerization; the first auxiliary agent refers to various auxiliary agents required in the first polymerization, for example, including molecular weight regulators, etc.; in the horizontal reactor, the second olefin monomer undergoes gas phase copolymerization with the product obtained in step 2) to generate a propylene copolymer; a second auxiliary agent may be added during the second polymerization; the second auxiliary agent refers to various auxiliary agents required in the second polymerization, for example, including molecular weight regulators, etc.
[0080] During the polymerization process, sometimes the properties of materials in different stages vary greatly, and the requirements for reaction conditions are also different. For example, in the early stage of polymerization, the material system has low viscosity, high heat release, and easy flow, while in the later stage of polymerization, it is often the opposite, and it is hoped that the low molecular weight substances generated can be removed while the reaction is ongoing. At this time, the use of a horizontal reactor can achieve better results.
[0081] Preferably, the first polymerization comprises a prepolymerization reaction and a liquid phase bulk polymerization reaction occurring sequentially.
[0082] The loop reactor comprises a prepolymerization loop and a liquid phase bulk polymerization loop connected in series. Propylene and a catalyst are first introduced into the prepolymerization loop to cause a prepolymerization reaction to occur, thereby obtaining a catalyst-containing slurry with a certain degree of polymerization, thereby adjusting the reaction control ability of the subsequent liquid phase bulk polymerization.
[0083] The catalyst-containing slurry obtained from the prepolymerization reaction, as well as the first olefin monomer and the first auxiliary agent with a designed formula are introduced into the polymerization reaction loop to carry out a liquid phase bulk polymerization reaction to obtain a polymer slurry with a certain degree of polymerization.
[0084] Preferably, in the prepolymerization reaction, the first olefin monomer is propylene; and the mass concentration of the catalyst component is ≥50%.
[0085] Preferably, the reaction temperature of the prepolymerization reaction is 10-40° C., the reaction pressure is 2.8-4.1 MPa, and the reaction time is 3-5 min.
[0086] Preferably, the propylene polymerization catalyst comprises a main catalyst and a co-catalyst; wherein the main catalyst comprises a magnesium compound carrier, a transition metal halide, an alcohol having 2 to 15 carbon atoms and an electron donor; the molar ratio of the magnesium compound carrier, the transition metal halide, the alcohol having 2 to 15 carbon atoms and the electron donor is 1:(1-40):(0.01-10):(0.01-10); the co-catalyst comprises an organoaluminum compound; in terms of molar ratio, the amount of the transition metal halide in the main catalyst to the organoaluminum compound in the co-catalyst is 1:(10-500).
[0087] Preferably, the electron donor is selected from at least one of an organophosphorus compound, an organosilane, cyclohexylmethyldimethoxysilane, dicyclopentyldimethoxysilane, and an electron donor having the following structure:
[0088]
[0089] In the formula, R1 and R6 are each independently selected from C1-C 12 Straight chain alkyl, C3-C 12 Branched alkyl, C3-C 15 Cycloalkyl, C3-C 15 R2, R3, R4, R5 are each independently selected from H atoms, halogen, C1-C 12 Straight chain alkyl, C3-C 12 branched alkyl, C3-C8 cycloalkyl, C6-C 15 Aryl, C6-C 15wherein R2 and R3, R3 and R4, R4 and R5 are independently connected to form a ring or not.
[0090] Preferably, the organoaluminum compound comprises alkylaluminum and / or alkylaluminoxane which is the hydrolysis product of alkylaluminum.
[0091] The catalyst is used for homopolymerization or copolymerization of olefin monomers, and the olefin monomers can be any one or more of ethylene, C3-C20 α-olefins or C3-C20 polar olefin monomers.
[0092] Specifically, the olefin polymerization catalyst used in the technical solution of the present invention can effectively catalyze ethylene homopolymerization, propylene homopolymerization, ethylene and α-olefin copolymerization, propylene and α-olefin copolymerization, ethylene and polar olefin monomer copolymerization or propylene and polar olefin monomer copolymerization, and the catalyst has high catalytic activity. Among them, α-olefin is C3-C20 olefin, preferably propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 3-methyl-1-butene, 4-methyl-1-pentene, styrene, α-methylstyrene and norbornene.
[0093] Preferably, in the liquid phase bulk polymerization reaction, the first olefin is propylene; or, the first olefin monomer is composed of propylene with a molar percentage of ≥96% and ethylene and / or butene with a molar percentage of ≤4%.
[0094] The liquid phase bulk polymerization can be either homopolymerization or copolymerization. In actual production, the formula can be designed and determined according to the performance requirements of the product to be produced. The raw material slurry, liquid propylene and hydrogen are mixed to form a liquid phase polymerization raw material; the liquid phase polymerization raw material is sent to a polymerization reaction loop reactor to carry out propylene liquid phase bulk homopolymerization to obtain a polypropylene slurry; the polypropylene slurry is continuously fed into a horizontal gas phase polymerization reactor to carry out propylene gas phase homopolymerization in the propylene slurry to obtain a product containing a propylene homopolymer. Alternatively, the liquid phase polymerization raw material is fed into a polymerization reaction loop reactor for liquid phase random copolymerization with ethylene to obtain a copolymer slurry; wherein the ethylene feed amount is less than 5% of the liquid phase propylene by mass (this is because ethylene is a non-condensable gas, and when the content in the loop reactor is high, it may be difficult to fuse with propylene into a uniform phase, and there is also a greater safety risk); the copolymer slurry is continuously fed into a gas phase polymerization reactor, so that the ethylene and propylene in the copolymer slurry are subjected to gas phase random copolymerization or gas phase impact copolymerization to obtain a product containing a propylene-ethylene random copolymer or an impact ethylene-propylene copolymer. The specific reaction can be designed according to actual production needs to design the feed ratio and process parameters to obtain a polymer of the target structure. The product containing a propylene homopolymer or a product containing a propylene-ethylene random / impact copolymer obtained by the technical solution of the present invention is subjected to gas-solid separation, the separated solid is dried to obtain polypropylene or a propylene-ethylene copolymer, and the separated gas is subjected to propylene and hydrogen recovery.
[0095] When the first olefin monomer is selected from propylene only, the product obtained by polymerization in the loop reactor is a polypropylene homopolymer. When the first olefin monomer is selected from a mixture of propylene and ethylene, the product obtained by polymerization in the loop reactor is an ethylene-propylene random copolymer. Since ethylene is a non-condensable gas, when its addition amount is large, there is a problem of pressure load in the reactor on the one hand, and a problem of high reaction heat during ethylene polymerization on the other hand, resulting in that the content of ethylene in the loop reactor cannot be large, otherwise the reaction conditions of the polymerization reaction system will be difficult to control.
[0096] Preferably, in the liquid phase bulk polymerization reaction, the amount of the catalyst used is 0.02 to 0.10% by mass of the liquid phase propylene.
[0097] The amount of the catalyst used can be determined according to actual production needs and the structure and properties of the target polymer.
[0098] Preferably, the amount of the catalyst is 0.02-0.03%, 0.03-0.04%, 0.04-0.05%, 0.05-0.06%, 0.06-0.07%, 0.07-0.08%, 0.08-0.09% and 0.09-0.10% of the mass of liquid propylene.
[0099] Preferably, the first polymerization in step 2) further comprises the step of adding a first auxiliary agent; the first auxiliary agent comprises a molecular weight regulator.
[0100] The molecular weight regulator is hydrogen, which is also called a chain transfer agent. In the actual production process, the process of using hydrogen to adjust the melt index of the polymer without using a degradation agent makes the molecular weight of the polymer smaller and the melt index higher. Hydrogen is used as a chain transfer agent for the polymerization reaction. It is dissolved in the liquid phase propylene and enters two loop reactors for chain transfer reaction, so that the melt index of the polymer product is significantly improved. At the same time, the product has the characteristics of being non-toxic and tasteless.
[0101] In the liquid phase bulk polymerization, the concentration of hydrogen can be adjusted within a wide range according to the molecular weight of the polymer to be produced. By volume, the hydrogen concentration is ≤20%; hydrogen concentration is ≤10%; hydrogen concentration is ≤5%; hydrogen concentration is ≤1%; hydrogen concentration is ≤0.8%; hydrogen concentration is ≤0.6%; hydrogen concentration is ≤0.4%; hydrogen concentration is ≤0.2%.
[0102] Preferably, the reaction temperature of the liquid phase bulk polymerization reaction is 60-80° C., and the reaction pressure is 2.7-4.0 MPa.
[0103] The polymerization in the loop reactor is liquid phase polymerization, and its polymerization temperature is basically maintained at about 70°C. Since the vaporization temperature of olefin monomers is low, at this reaction temperature, it needs to be maintained under certain pressure conditions to make the reaction system a liquid phase medium. The use of a loop reactor for homopolymerization or random copolymerization can, on the one hand, increase the concentration of monomers in the liquid phase medium, thereby increasing the polymerization activity of the catalyst; on the other hand, the loop reactor has a small diameter, a large specific surface area, and fast heat transfer, which is particularly suitable for the conduction of exothermic reaction heat of the polymerization reaction, which is conducive to the stable maintenance of the reaction system conditions and has good reaction controllability for highly exothermic reactions. In liquid phase bulk polymerization, the liquid circulates and reacts in the loop tube, which is a process of full mixing of materials, and the reaction materials are fully in contact, so the materials react more thoroughly, so the homopolymerization or random copolymerization in this step has a very high conversion rate, which can achieve a great increase in production.
[0104] The liquid phase bulk polymerization occurs in liquid phase propylene, and hydrogen is used as a molecular weight regulator to carry out bulk polymerization. Propylene homopolymers or copolymers of propylene and ethylene, C4 and C4 α-olefins above are generated. The polymerization conditions of the liquid phase bulk polymerization are: polymerization pressure of 2.2-6.5Mpa, polymerization temperature of 55-95°C. Preferably, the polymerization pressure is 2.7-4.0Mpa, and the polymerization temperature is 60-80°C. The hydrogen concentration is determined according to the molecular weight of the polymer required to be produced by the liquid phase bulk polymerization.
[0105] In actual production, the molecular weight of polymers produced by liquid phase bulk polymerization is generally smaller than that of polymers produced by gas phase bulk polymerization. The polymers produced by liquid phase bulk polymerization account for 20% to 90% of the total polymer amount.
[0106] Preferably, the loop reactor comprises a polymerization reaction loop in which a liquid phase bulk polymerization reaction occurs, which comprises a polymerization loop unit; the polymerization loop unit comprises one or more annular tubes connected in series.
[0107] The one or more annular tubes connected in series constitute a polymeric annular tube unit.
[0108] In one embodiment of the present invention, the polymerization reaction loop can be a single loop, or two or more loops connected in series. The reaction conditions in each loop are designed according to actual needs, and the reaction conditions in each loop can be independently controlled, thereby controlling the structure and molecular weight of the polymer. The monomer and catalyst conditions in each loop can be the same or different, and the product obtained can be a homopolymer of a single olefin monomer or a random copolymer of multiple olefin monomers; the obtained product can be a unimodal polymer, a bimodal polymer or a multimodal polymer.
[0109] Preferably, the polymerization reaction loop comprises a plurality of polymerization loop units connected in parallel.
[0110] The loop tube reactor comprises a prepolymerization loop tube and a polymerization reaction loop tube, wherein the loop tubes are connected in series or in parallel, and can be flexibly designed according to different technical purposes in actual production.
[0111] The loop reactor is divided into two zones, one zone is a prepolymerization zone, and the other zone is a liquid phase bulk polymerization reaction zone; the loops between the two zones are connected in series, and the slurry prepolymerized in the prepolymerization zone is transported to the polymerization reaction zone through a pipeline for liquid phase bulk polymerization. The prepolymerization zone includes a loop, into which the first olefin monomer and the catalyst are introduced for prepolymerization; the liquid phase bulk polymerization zone includes a loop, into which the prepolymerization product, the first olefin monomer and the first auxiliary agent are introduced to continue the bulk homopolymerization reaction to obtain a propylene homopolymer or an ethylene-propylene random copolymer.
[0112] In one embodiment of the present invention, the loop reactor is composed of a plurality of loops, including a prepolymerization loop and a plurality of polymerization loop units connected in parallel. The reaction conditions of each polymerization loop unit are individually designed and controlled, and polymers of various polymerization structures and molecular weights can be designed and manufactured according to actual needs.
[0113] In the technical solution of the present invention, the liquid phase bulk polymerization of olefins adopts a loop reactor, the loop is fully mixed, and several loops are connected in series similar to several stirred kettles in series. Compared with kettle-type bulk polymerization, the loop has a large heat transfer area and a high single-pass conversion rate; in the loop bulk polymerization, polymer particles are suspended in propylene liquid, and there is good heat transfer between the polymer and propylene; a cooling jacket is used to remove the reaction heat, the heat transfer area per unit volume is large, and the heat transfer coefficient is large. Generally speaking, the overall heat transfer coefficient of the loop reactor can be as high as 1600w / (m 2 .℃); the polymer slurry concentration in the loop reactor is high, generally >50% (mass fraction), the reactor has a high single-pass conversion rate, and the single-pass conversion rate of homopolymerized propylene can reach 50% to 65%. Furthermore, in addition to improving the heat transfer capacity of the system, the advantage of the loop is to enhance the mass transfer effect. The slurry in the annular tube reactor is circulated at high speed by an axial flow pump, and the fluid flow rate can reach 7m / s; if the circulation ratio is high enough, the fluid in the annular tube can be close to ideal full mixing, and the distribution of comonomers, catalysts, etc. in the entire reactor is more uniform; on the one hand, the isotacticity of the polymer can be improved, and on the other hand, the polymerization reaction conditions are easy to control and can be controlled very accurately, so that the product quality is stable, and it is not easy to produce hot spots, not easy to stick to the wall, and the energy consumption of the axial flow pump is also low; while in the stirred tank, especially the large stirred tank, there will always be dead zones in the system, and the structure of the manufactured polymer is uneven and the performance is unstable; further, the fluid in the annular tube should be close to a piston-type fluid, which can greatly reduce the short circuit of the catalyst and increase the residence time of the catalyst under the transportation of the axial flow pump, while the fluid in the kettle reactor is fully mixed, which can easily cause the catalyst to short-circuit.
[0114] Preferably, the polymerization reaction loop is connected in series with the horizontal reactor.
[0115] The discharge of the loop reactor is directly introduced into the horizontal reactor, and the monomers do not need to be gasified with steam. The liquid monomers are gasified by the heat of the gas phase polymerization reaction, which reduces the steam consumption. The single-pass conversion rate of the reaction is high, which can reach more than 80%, and the circulating amount of the monomers is small.
[0116] The polypropylene preparation method of the present invention is a continuous process. The homopolymer or random copolymer obtained from the loop reactor can be introduced into the horizontal reactor for further copolymerization without flash evaporation or the like.
[0117] The horizontal reactor is a continuous reactor. Materials are continuously input from one end of the reactor, and products are continuously output from the other end of the reactor until a certain conversion rate is reached, and the chemical reaction is completed in the flow. As the materials move in the reactor, the concentration gradually decreases and the reaction rate gradually decreases. Multiple stirring paddles can be set in the horizontal reactor, and each stirring paddle is separated by a partition, so that the flow condition of the material in the reactor is similar to that of a multi-stage series stirring reactor, thereby reducing the number of equipment and the installation height.
[0118] In addition to meeting the requirements of general reactors, the horizontal reactor has the following special requirements: first, the materials can be fully mixed radially in the reactor, without axial mixing, and as close to plug flow as possible; second, according to the polymerization kinetics theory, in order to achieve a predetermined degree of polymerization, small molecules generated in the system should be removed as much as possible, so the reaction materials should be spread out as much as possible in the reactor to form a large-area film, increase the evaporation surface area, and the evaporation surface area can be continuously updated.
[0119] In the prior art, the gas phase polymerization reactor generally used in conjunction with the loop tube is mostly a gas phase fluidized bed reactor, and the fluidized bed is a fully mixed reactor, so the residence time of various materials in the reactor varies greatly, resulting in relatively large differences between individual polymer powders in the reactor. When producing copolymer products, the residence time of some materials is very short, making their content in the comonomer very low; theoretically, the copolymer product obtained therefrom may contain 100% homopolymer particles, and the structure and distribution of various components in the copolymer are also difficult to control, which will affect the performance of the copolymer product to a certain extent.
[0120] In the technical solution of the present invention, a horizontal reactor is used for gas phase bulk polymerization. Compared with a gas phase fluidized bed reactor, the horizontal reactor has the advantages of high equipment efficiency, high catalyst utilization efficiency, uniform product comonomer content, and strong adaptability even when the comonomer content in the product is relatively high or the molecular weight of the polymer is very low, which may cause the powder to be somewhat sticky. Since the catalyst introduced into the horizontal reactor is a polypropylene powder that has been fully polymerized in the liquid phase bulk in the loop reactor, no hot spots generated by catalyst aggregation will occur in the horizontal reactor. Therefore, the horizontal reactor can be used for gas phase polymerization under a wide and high reaction pressure (2.1-3.0Mpa) and a wide reaction temperature (60-130°C) without generating hot spots or plasticized blocks, and the reaction is well controlled.
[0121] In one embodiment of the present invention, a plurality of polymerization ring tube units are connected in parallel, and the same or different polymerization reactions can be carried out in each polymerization ring tube unit; the products after polymerization are then simultaneously put into a horizontal reactor for gas phase copolymerization. When the same polymerization reaction is carried out in each polymerization ring tube unit, the technical solution of the present invention can improve the yield of polypropylene by connecting a plurality of polymerization ring tube units in parallel and then connecting them in series with a horizontal reactor, thereby overcoming the defect of small yield of the ring tube reactor. When different polymerization reactions are carried out in each polymerization ring tube unit, the technical solution of the present invention can design the structure and performance of the copolymer by connecting a plurality of polymerization ring tube units in parallel and then connecting them in series with a horizontal reactor, and can have the advantages of both the ring tube reactor and the horizontal reactor, the dispersion of various materials such as the catalyst is good, it is not easy to generate hot spots, the production efficiency is high, and polypropylene with excellent comprehensive performance can be obtained.
[0122] Preferably, the second olefin monomer is at least two of ethylene, propylene or butene.
[0123] The olefin monomer can be at least one of C2 to C12 olefin monomers. It should be noted that, for this preparation method, the olefin monomer is not specifically limited and can be selected according to actual needs after the target product is determined. The olefin monomer for gas phase bulk polymerization can be gas phase copolymerization of propylene and propylene, or propylene and ethylene, butene and α-olefins above butene to produce propylene homopolymer, or random copolymer, or impact copolymer.
[0124] Preferably, the molar percentage of ethylene in the second olefin monomer is ≤60%.
[0125] When preparing impact-resistant polypropylene, ethylene units can be introduced into polypropylene to improve its performance. The traditional physical blending modification method is gradually replaced by chemical copolymerization modification due to poor modification effect. The technical solution of the present invention obtains a product with good low-temperature impact resistance and high gloss by adjusting and optimizing olefin monomers, for example, copolymerization of ethylene, propylene and butene.
[0126] The process flow of the present invention is as follows: propylene and auxiliary agents such as catalysts are sequentially put into a prepolymerization loop for prepolymerization, liquid phase bulk polymerization is carried out in a polymerization reaction loop, and then the propylene is put into a horizontal reactor for gas phase bulk polymerization for homopolymerization or copolymerization. When producing impact copolymers, the prepolymerization loop and the polymerization reaction loop produce propylene homopolymers with relatively small molecular weight, and the horizontal reactor produces propylene and ethylene or alpha olefin copolymers with relatively large molecular weight.
[0127] The reaction in the horizontal reactor is mainly gas phase bulk polymerization of propylene and ethylene, C4 and C4 α-olefins above; when producing impact copolymers, polymers with relatively large molecular weight are produced in the horizontal reactor. The technical scheme of the present invention adopts a step-by-step polymerization process combining liquid phase bulk polymerization in a loop reactor with gas phase bulk polymerization in a horizontal reactor to carry out propylene homopolymerization and copolymerization of propylene and ethylene, C4 and C4 α-olefins above, and can produce polypropylene homopolymers and copolymers with adjustable molecular weight distribution in a wide range.
[0128] Preferably, the reaction temperature of the second polymerization is 60-80°C, and the reaction pressure is 2.0-3.0 MPa. More preferably, the reaction temperature of the second polymerization is 65-75°C, and the reaction pressure is 2.4-2.5 MPa.
[0129] When producing impact-resistant copolymers, the temperature of the gas phase bulk polymerization needs to be controlled above the dew point and below the softening point of the polymer, generally 60 to 80°C, preferably between 65 and 75°C.
[0130] Since the catalyst of the polymerization reaction is added to the reaction system during the liquid phase bulk polymerization in the loop reactor, it undergoes preliminary polymerization in the prepolymerization loop and continues chain growth in the subsequent liquid phase bulk polymerization. Therefore, the polymer slurry introduced into the horizontal reactor contains polypropylene powder after polymerization growth. Therefore, even at an operating pressure of up to 3.0 MPa and an operating temperature above the dew point, the copolymerization reaction in the horizontal reactor will not generate hot spots due to the aggregation of the catalyst to generate plasticized blocks.
[0131] Preferably, the amount of the catalyst used in the second polymerization is 0.02-0.10% by mass of the second olefin.
[0132] The amount of the catalyst used can be determined according to actual production needs and the structure and properties of the target polymer.
[0133] Preferably, the amount of the catalyst used is 0.02-0.03%, 0.03-0.04%, 0.04-0.05%, 0.05-0.06%, 0.06-0.07%, 0.07-0.08%, 0.08-0.09% and 0.09-0.10% of the mass of the second olefin.
[0134] Preferably, the second polymerization in step 3) further comprises the step of adding a first auxiliary agent; the second auxiliary agent comprises a molecular weight regulator.
[0135] In gas phase bulk polymerization, hydrogen is also used as a molecular weight regulator for polymerization, and the concentration of hydrogen can be adjusted within a wide range according to the molecular weight of the polymer to be produced. Generally, the hydrogen concentration in the second polymerization is slightly less than the hydrogen concentration in the first polymerization, and the specific value is determined according to the molecular structure and performance of the product to be produced. By adjusting and changing the concentration of hydrogen, the molecular weight and structure of the polymer obtained in the loop reactor and the horizontal reactor can be controlled.
[0136] In the gas phase bulk polymerization, the type of catalyst used is the same as the catalyst used in the first polymerization, and the amount of the catalyst used can be adjusted within a wide range according to the molecular weight of the polymer to be produced.
[0137] Preferably, the horizontal reactor is provided with a transverse stirring shaft, and a plurality of stirring paddles are provided on the stirring shaft.
[0138] Preferably, the shape of the stirring paddle is selected from T-shaped, rectangular, wedge-shaped and open-shaped.
[0139] In the horizontal reactor propylene polymerization process, agglomeration is one of the hidden dangers that seriously affects the long-term stable operation of the device and the quality of the product. According to a large amount of research data analysis, when the agitator uses a blade paddle for stirring, the degree of back-mixing of the materials in the reactor is the largest, which is closest to full mixed flow, which is not conducive to the consistent control of the residence time of the materials in the reactor, and also makes the quality control of the polymer more difficult. The obtained copolymer structure is not uniform and the performance is unstable; while the use of T-shaped, rectangular, wedge-shaped and open-shaped paddles has better effects; the horizontal kettle stirring with a T-shaped paddle is preferred, at this time the degree of back-mixing of the materials in the reactor is the smallest, which is closest to the plug flow.
[0140] The technical solution of the present invention adopts a horizontal reactor and uses a T-shaped stirring paddle. This unique reactor makes the residence time distribution range of various material particles in the reactor very narrow, and copolymer products with very good rigidity and impact resistance can be produced. Further, this reactor close to plug flow can avoid the short circuit of the catalyst in the reactor. When ethylene is present in the second olefin, large-particle copolymers can be generated, rather than fine powder that may reduce the low-temperature impact strength of the copolymer in the homopolymer particles and form unnecessary colloids. Therefore, the very narrow reaction residence time distribution of this process can achieve the requirements of high-impact copolymers that can only be produced by multiple fully mixed reactor homopolymer reactors. In addition, due to the unique reactor design, the product transition time of this process is very short. In theory, the transition time of the product is 2 / 3 shorter than that of a continuous stirred reactor or a fluidized bed reactor, so product switching is easy and there are few transition products.
[0141] Preferably, the horizontal reactor comprises a gasification separation zone and a gas phase polymerization reaction zone in sequence from the feed direction to the discharge direction; a partition is arranged between the gasification separation zone and the gas phase polymerization reaction zone; and a gap is arranged between one end of the partition and the side wall of the horizontal reactor.
[0142] In the technical solution of the present invention, the polymer slurry obtained from the loop reactor does not need to be subjected to treatments such as flash evaporation and degassing, and can be directly introduced into the horizontal reactor.
[0143] The horizontal reactor can be divided into a plurality of polymerization zones with different polymerization temperatures and gas phase components by partitions, each having an independent external circulation cooling system. The circulating gas and condensate can be returned to the bottom of the horizontal reactor together. The catalyst entering can be a slurry that has been prepolymerized and slurry polymerized with propylene.
[0144] The horizontal reactor uses propylene flash evaporation to remove heat. Liquid propylene is sprayed into the reactor from various feed points in a way that keeps the reactor bed dry. After the liquid propylene is vaporized, the partial pressure of its monomer is less than its dew point pressure and is sufficient to remove the reaction heat. During operation, the feed rate of liquid propylene and its vaporization in the reactor must be strictly controlled to ensure a balance between the dryness of the reactor and the reaction temperature range.
[0145] A gasification separation zone is set at the material inlet end of the horizontal reactor. The polymer slurry produced by the loop reactor first enters the gasification separation zone of the horizontal reactor. In this zone, the liquid phase in the slurry is gasified due to the action of polymerization heat, and most of the hydrogen and part of the propylene are separated and leave the horizontal reactor. After separating and removing most of the hydrogen and part of the propylene, the polypropylene powder enters the gas phase polymerization reaction zone through the gap between the partition and the side wall of the horizontal reactor. The polymerization reaction in the gas phase polymerization reaction zone can be carried out at a set hydrogen concentration and a set ratio of propylene to comonomer, producing a homopolymer or copolymer with a higher molecular weight than liquid phase bulk polymerization.
[0146] The gas phase polymerization zone can be an integral area, or it can be divided into several gas phase polymerization sub-zones by setting a partition inside it. The horizontal reactor with gas phase polymerization sub-zones has a reaction effect equivalent to several gas phase polymerization kettles connected in series, and the reaction conditions of each zone can be independently controlled, which can realize flexible product design and product production through one device.
[0147] Furthermore, the horizontal reactors may be connected in series. When multiple horizontal reactors are connected in series, the gasification separation zone may be arranged only in the first horizontal reactor connected to the loop reactor.
[0148] When multiple horizontal reactors are connected in series, the molecular weight of the polymer polymerized in the gas phase gradually increases starting from the first horizontal reactor connected to the loop reactor; however, as required, the molecular weight of the generated copolymer can also be controlled to be the same as that of the polymer polymerized in the first horizontal reactor.
[0149] The horizontal reactor and the supporting devices for the operation of the horizontal reactor are collectively referred to as the gas phase reaction zone. Specifically, in the gasification separation zone, the horizontal reactor of the present invention is provided with a polymer slurry inlet for receiving the polymer slurry introduced from the loop reactor or the extractor; it is also provided with an exhaust port for discharging the separated gasified propylene gas and hydrogen; if necessary, a propylene quenching liquid inlet for lowering the reactor temperature can also be provided, through which the propylene quenching liquid can be sprayed at any time, and the temperature of the reactor can be adjusted by gasification and heat removal of the cold liquid propylene. In the gas phase polymerization zone, the horizontal reactor is also provided with the following external supporting devices, including an external circulation condenser, a condensate tank, a condensate reflux pump, a circulating fan for non-condensable gas, etc. During gas phase homopolymerization, the condensate and non-condensable gas can be returned to the gas phase polymerization zone; however, when producing copolymer products, the condensate and non-condensable gas are not allowed to return to the gasification separation zone to avoid affecting the reaction conditions of the gas phase polymerization zone.
[0150] The above method can prepare products with various structures and properties according to product design, such as the ethylene content in the gas phase copolymerization can be adjusted arbitrarily within the range of ≤50%. The structure and properties of the polymer obtained by the technical solution of the present invention can be designed, and different designs can be made according to actual needs in actual operation to obtain products that meet various needs.
[0151] The present invention also provides a high-impact and high-gloss polypropylene prepared according to the above method, and the room temperature impact strength thereof is ≥60KJ / m according to ASTM D256 standard test. 2 ; Its low temperature impact strength ≥50KJ / m 2 ; According to GB / T 8807 standard, its glossiness shall be ≥85%.
[0152] In the detection method, the low temperature is -20°C.
[0153] The preparation method of the invention adopts a process method of liquid phase bulk polymerization in a loop reactor combined with gas phase bulk polymerization in a horizontal reactor. At the same time, under the condition of the presence of a suitable catalyst, the polymer structure can be designed according to actual needs. The generated polypropylene particles are large and uniform, spherical, and the molecular weight distribution can be adjusted to be wide or narrow. The product has high crystallinity and good optical properties. The copolymerized ethylene content and the distribution in the ethylene copolymer are fine and uniform, and have good low-temperature impact resistance.
[0154] The present invention also provides an application of high-impact and high-gloss polypropylene prepared according to the above method.
[0155] The following is further described in detail by specific embodiments:
[0156] Example 1
[0157] The feeding system adopted in this embodiment includes: a batching tank 1, in which an agitator is arranged; a metering tank 2 (including a first metering tank 21 and a second metering tank 22 connected in parallel), whose inlet is connected to the outlet of the batching tank 1; a diaphragm metering pump 3, whose inlet is connected to the outlet of the metering tank 2; a buffer tank 5, whose inlet is connected to the outlet of the diaphragm metering pump 3, and whose outlet is connected to a polymerization reactor 6; the buffer tank 5 is provided with an agitator, a temperature controller and a pressure regulator; an agitator 4 with a pipeline structure is arranged in the conveying pipeline between the diaphragm metering pump 3 and the buffer tank 5, so as to keep the catalyst premix liquid in the conveying process uniform in composition. Two sets of buffer tanks 5 of the feeding system are arranged, one set is connected to the prepolymerization loop pipe to make its composition uniform and adjust its temperature with the temperature of the prepolymerization loop pipe; the other set is connected to the horizontal reactor to make its composition uniform and adjust its temperature with the temperature of the horizontal kettle.
[0158] The preparation method of high-impact high-gloss polypropylene is as follows: a prepolymerization loop tube, a polymerization reaction loop tube and a horizontal reactor are connected in series; the prepolymerization loop tube is a single loop tube; the polymerization reaction loop tube includes two polymerization reaction units connected in parallel; each polymerization reaction unit includes two loop tubes connected in series; a gas phase separation zone and a gas phase copolymerization reaction zone are arranged in the horizontal reactor; the polymerization reaction units are all connected to the inlet end (gas phase separation zone) of the horizontal reactor, and the specific preparation steps are as follows:
[0159] First, propylene and catalyst are introduced into the prepolymerization loop, the reaction temperature is controlled to be 10-12°C, the reaction pressure is 4.0-4.1Mpa, and the reaction is carried out for 5 minutes; wherein, in the catalyst, the molar ratio of the magnesium compound carrier, ferrous chloride, octanol and cyclic phosphate is 1:10:2:2; the co-catalyst is triethylaluminum; in terms of molar ratio, the amount of ferrous chloride and triethylaluminum is 1:100; and the mass concentration of the catalyst is 50%.
[0160] Ethylene and propylene are introduced as raw materials into a polymerization reaction loop; wherein the molar percentage of propylene is 96%, and the molar percentage of ethylene is 4%; the amount of catalyst used is 0.05% of the mass of liquid propylene; the reaction temperature is 70-72°C, and the reaction pressure is 3.2-3.3Mpa; hydrogen with a volume concentration of 1000ppm is introduced to control the reaction; and the reaction time in each loop is controlled to be 15min.
[0161] The obtained ethylene-propylene random copolymer is introduced into a horizontal reactor, and ethylene and propylene are continuously introduced into the horizontal reactor to carry out copolymerization reaction in the presence of a catalyst; wherein the volume percentage of propylene is 90%, and the volume percentage of ethylene is 10%; the reaction temperature is 73-75°C; the reaction pressure is 2.3-2.4Mpa; the catalyst is the same as the catalyst for liquid phase bulk polymerization, and its amount is 0.05% of the mass of the second olefin; hydrogen with a volume concentration of 800ppm is introduced to control the reaction, and a propylene polymer of ethylene-propylene rubber phase is obtained.
[0162] The performance of the product obtained in this example was tested. Its impact strength was tested according to ASTM D256 standard, and the room temperature impact strength was 68.8 KJ / m 2 , low temperature impact strength is 54KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 94.2%.
[0163] The infrared spectrum shows that the high gloss impact-resistant copolymer polypropylene resin of the present invention is different from ordinary propylene-ethylene random copolymer polypropylene and conventional impact-resistant copolymer polypropylene.
[0164] Example 2
[0165] The reactor is the same as in Example 1, and the specific preparation steps are as follows:
[0166] First, propylene and catalyst are introduced into a prepolymerization loop, and the reaction temperature is controlled to be 38-40° C., the reaction pressure is 2.8-2.9 MPa, and the reaction is carried out for 5 minutes. In the catalyst, the molar ratio of the magnesium compound carrier, titanium tetrachloride, 1-pentadecanol and cyclohexylmethyldimethoxysilane is 1:40:10:10; the co-catalyst includes tri-n-propylaluminum; the molar ratio of titanium tetrachloride to tri-n-propylaluminum is 1:10; and the mass concentration of the catalyst is 50%.
[0167] Ethylene and propylene are introduced as raw materials into a polymerization reaction loop; wherein the molar percentage of propylene is 96%, and the molar percentage of ethylene is 4%; the amount of catalyst used is 0.10% of the mass of liquid phase propylene; the reaction temperature is 60-62°C, and the reaction pressure is 3.9-4.0 MPa; hydrogen with a volume concentration of 1000 ppm is introduced to control the reaction; and the reaction time in each loop is controlled to be 15 min.
[0168] The obtained ethylene-propylene random copolymer is introduced into a horizontal reactor, and ethylene and propylene are continuously introduced into the horizontal reactor to carry out copolymerization reaction in the presence of a catalyst; wherein the volume percentage of propylene is 80%, and the volume percentage of ethylene is 20%; the reaction temperature is 65-67°C; the reaction pressure is 2.4-2.5Mpa; the catalyst is used as a catalyst for liquid phase bulk polymerization, and its dosage is 0.08% of the mass of the second olefin liquid; hydrogen with a volume concentration of 800ppm is introduced to control the reaction, and a propylene polymer of ethylene-propylene rubber phase is obtained. The catalyst is used as a catalyst for liquid phase bulk polymerization, and its dosage is 0.08% of the mass of the second olefin; the performance of the product obtained in this example is tested. Its impact strength is tested according to ASTM D256 standard, and the impact strength at room temperature is 66.7KJ / m 2 , low temperature impact strength is 60.2KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 94.0%.
[0169] Example 3
[0170] The reactor is the same as in Example 1, and the specific preparation steps are as follows:
[0171] First, propylene and catalyst are introduced into the prepolymerization loop, the reaction temperature is controlled to be 20-22°C, the reaction pressure is 3.5-3.6Mpa, and the reaction is carried out for 3 minutes; wherein, in the catalyst, the molar ratio of the magnesium compound carrier, cupric chloride, n-hexanol and dicyclopentyldimethoxysilane is 1:1:0.01:0.01; the co-catalyst is triethylaluminum; in terms of molar ratio, the amount of cupric chloride and triethylaluminum is 1:500; and the mass concentration of the catalyst is 60%.
[0172] Ethylene and propylene are introduced as raw materials into a polymerization reaction loop; wherein the molar percentage of propylene is 96%, and the molar percentage of ethylene is 4%; the amount of catalyst used is 0.08% of the mass of liquid phase propylene; the reaction temperature is 78-80°C, and the reaction pressure is 2.7-2.8Mpa; hydrogen with a volume concentration of 1000ppm is introduced to control the reaction; and the reaction time in each loop is controlled to be 15min.
[0173] The obtained ethylene-propylene random copolymer is introduced into a horizontal reactor, and ethylene and propylene are continuously introduced into the horizontal reactor to carry out copolymerization reaction in the presence of a catalyst; wherein the volume percentage of propylene is 70%, and the volume percentage of ethylene is 30%; the reaction temperature is 60-62° C.; the reaction pressure is 2.9-3.0 MPa; the catalyst is the same as the catalyst for liquid phase bulk polymerization, and its amount is 0.10% of the mass of the second olefin; hydrogen with a volume concentration of 800 ppm is introduced to control the reaction, and a propylene polymer of ethylene-propylene rubber phase is obtained.
[0174] The performance of the product obtained in this example was tested. Its impact strength was tested according to ASTM D256 standard, and the room temperature impact strength was 69.0 KJ / m 2 , low temperature impact strength is 68.8KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 93.2%.
[0175] Example 4
[0176] The reactor is the same as in Example 1, and the specific preparation steps are as follows:
[0177] First, propylene and catalyst are introduced into the prepolymerization loop, the reaction temperature is controlled to be 20-22°C, the reaction pressure is 3.5-3.6Mpa, and the reaction is carried out for 5 minutes; wherein, in the catalyst, the molar ratio of the magnesium compound carrier, cobalt chloride, n-hexanol and dicyclopentyldimethoxysilane is 1:10:2:2; the co-catalyst is triethylaluminum; in terms of molar ratio, the amount of cupric chloride and triethylaluminum is 1:100; and the mass concentration of the catalyst is 50%.
[0178] Ethylene and propylene are introduced as raw materials into a polymerization reaction loop; wherein the molar percentage of propylene is 96%, and the molar percentage of ethylene is 4%; the amount of catalyst used is 0.05% of the mass of liquid propylene; the reaction temperature is 70-72°C, and the reaction pressure is 3.2-3.3Mpa; hydrogen with a volume concentration of 1000ppm is introduced to control the reaction; and the reaction time in each loop is controlled to be 15min.
[0179] The obtained ethylene-propylene random copolymer is introduced into a horizontal reactor, and ethylene and propylene are continuously introduced into the horizontal reactor to carry out copolymerization reaction in the presence of a catalyst; wherein the volume percentage of propylene is 60%, and the volume percentage of ethylene is 40%; the reaction temperature is 72-74° C.; the reaction pressure is 2.4-2.5 MPa; the catalyst is used as a catalyst for liquid phase bulk polymerization, and its amount is 0.08% of the mass of the second olefin; hydrogen with a volume concentration of 800 ppm is introduced to control the reaction, and a propylene polymer of ethylene-propylene rubber phase is obtained.
[0180] The performance of the product obtained in this example was tested. Its impact strength was tested according to ASTM D256 standard, and the room temperature impact strength was 67.5 KJ / m 2 , low temperature impact strength is 71.3KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 91.0%.
[0181] Example 5
[0182] The reactor is the same as in Example 1, and the specific preparation steps are as follows:
[0183] First, propylene and catalyst are introduced into the prepolymerization loop, the reaction temperature is controlled to be 20-22° C., the reaction pressure is 3.5-3.6 MPa, and the reaction is carried out for 5 minutes; wherein, in the catalyst, the molar ratio of the magnesium compound carrier, titanium tetrachloride, n-hexanol and dicyclopentyldimethoxysilane is 1:10:2:2; the co-catalyst is triethylaluminum; in terms of molar ratio, the amount of cupric chloride and triethylaluminum is 1:500; and the mass concentration of the catalyst is 50%.
[0184] Ethylene and propylene are introduced as raw materials into a polymerization reaction loop; wherein the molar percentage of propylene is 96%, and the molar percentage of ethylene is 4%; the amount of catalyst used is 0.05% of the mass of liquid propylene; the reaction temperature is 70-72°C, and the reaction pressure is 3.2-3.3Mpa; hydrogen with a volume concentration of 1000ppm is introduced to control the reaction; and the reaction time in each loop is controlled to be 15min.
[0185] The obtained ethylene-propylene random copolymer is introduced into a horizontal reactor, and ethylene and propylene are continuously introduced into the horizontal reactor to carry out copolymerization reaction in the presence of a catalyst; wherein the volume percentage of propylene is 50%, and the volume percentage of ethylene is 50%; the reaction temperature is 72-74° C.; the reaction pressure is 2.4-2.5 MPa; the catalyst is used as a catalyst for liquid phase bulk polymerization, and its amount is 0.08% of the mass of the second olefin; hydrogen with a volume concentration of 800 ppm is introduced to control the reaction, and a propylene polymer of ethylene-propylene rubber phase is obtained.
[0186] The performance of the product obtained in this example was tested. Its impact strength was tested according to ASTM D256 standard, and the room temperature impact strength was 65.8 KJ / m 2 , low temperature impact strength is 73.2KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 89.0%.
[0187] Example 6
[0188] The reactor is the same as in Example 1, and the specific preparation steps are as follows:
[0189] First, propylene and catalyst are introduced into the prepolymerization loop, the reaction temperature is controlled to be 20-22°C, the reaction pressure is 3.5-3.6Mpa, and the reaction is carried out for 5 minutes; wherein, in the catalyst, the molar ratio of the magnesium compound carrier, titanium tetrachloride, n-hexanol and dicyclopentyldimethoxysilane is 1:10:2:2; the co-catalyst is triethylaluminum; in terms of molar ratio, the amount of cupric chloride and triethylaluminum is 1:100; and the mass concentration of the catalyst is 50%.
[0190] Ethylene and propylene are introduced as raw materials into a polymerization reaction loop; wherein the molar percentage of propylene is 96%, and the molar percentage of ethylene is 4%; the amount of catalyst used is 0.05% of the mass of liquid propylene; the reaction temperature is 70-72°C, and the reaction pressure is 3.2-3.3Mpa; hydrogen with a volume concentration of 1000ppm is introduced to control the reaction; and the reaction time in each loop is controlled to be 15min.
[0191] The obtained ethylene-propylene random copolymer is introduced into a horizontal reactor, and ethylene and propylene are continuously introduced into the horizontal reactor to carry out copolymerization reaction in the presence of a catalyst; wherein the volume percentage of propylene is 40%, and the volume percentage of ethylene is 60%; the reaction temperature is 72-74° C.; the reaction pressure is 2.4-2.5 MPa; the catalyst is used as a catalyst for liquid phase bulk polymerization, and its amount is 0.08% of the mass of the second olefin; hydrogen with a volume concentration of 800 ppm is introduced to control the reaction, and a propylene polymer of ethylene-propylene rubber phase is obtained.
[0192] The performance of the product obtained in this example was tested. Its impact strength was tested according to ASTM D256 standard, and the room temperature impact strength was 65.4 KJ / m 2 , low temperature impact strength is 74.8KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 86.5%.
[0193] Example 7
[0194] The reactor is the same as in Example 1, and the specific preparation steps are as follows:
[0195] First, propylene and catalyst are introduced into the prepolymerization loop, the reaction temperature is controlled to be 20-22°C, the reaction pressure is 3.5-3.6Mpa, and the reaction is carried out for 5 minutes; wherein, in the catalyst, the molar ratio of the magnesium compound carrier, titanium tetrachloride, n-hexanol and dicyclopentyldimethoxysilane is 1:10:2:2; the co-catalyst is triethylaluminum; in terms of molar ratio, the amount of cupric chloride and triethylaluminum is 1:100; and the mass concentration of the catalyst is 50%.
[0196] Propylene is introduced as raw material into the polymerization reaction loop; the catalyst dosage is 0.05% of the mass of liquid propylene; the reaction temperature is 70-72°C, and the reaction pressure is 3.2-3.3Mpa; hydrogen with a volume concentration of 1000ppm is introduced to control the reaction; the reaction time in each loop tube is controlled to be 15min.
[0197] The obtained ethylene-propylene random copolymer is introduced into a horizontal reactor, and ethylene and propylene are continuously introduced into the horizontal reactor to carry out copolymerization reaction in the presence of a catalyst; wherein the volume percentage of propylene is 50%, and the volume percentage of ethylene is 50%; the reaction temperature is 72-74° C.; the reaction pressure is 2.4-2.5 MPa; the catalyst is used as a catalyst for liquid phase bulk polymerization, and its amount is 0.08% of the mass of the second olefin; hydrogen with a volume concentration of 800 ppm is introduced to control the reaction, and a propylene polymer of ethylene-propylene rubber phase is obtained.
[0198] The performance of the product obtained in this example was tested. Its impact strength was tested according to ASTM D256 standard, and the room temperature impact strength was 66.2 KJ / m 2 , low temperature impact strength is 76.0KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 86.8%.
[0199] From the test data of the above embodiments, it can be seen that with the increase of ethylene content in the copolymer, its room temperature impact resistance shows a trend of increasing first and then decreasing; although the content of the rubber phase increases very high, its room temperature impact strength only fluctuates in a small range of 65 to 69Mpa, indicating that the influence of the rubber phase content on the room temperature impact resistance within this range is not obvious. The low temperature impact resistance of the product is significantly improved with the increase of the rubber phase content, which can reach 76.0KJ / m 2 , showing good low-temperature impact resistance; at the same time, with the increase of rubber phase content, the gloss of the product is not significantly affected.
[0200] Comparative Example 1
[0201] The formula and process parameters are the same as those in Example 2. The only difference is that the feed system proposed in the present invention is not used, but the suspension of propylene polymerization catalyst and liquid propylene is directly introduced into the polymerization reactor. The performance of the product obtained in this comparative example is tested. The impact strength is tested according to ASTM D256 standard, and the room temperature impact strength is 62KJ / m 2 , low temperature impact strength is 58KJ / m 2 ; The glossiness was tested according to GB / T 8807 standard and the result was 91%.
[0202] The propylene polymer of the present invention is prepared by homopolymerizing propylene and then performing gas phase impact copolymerization with propylene and ethylene, or by copolymerizing propylene and ethylene twice to generate random copolymerized polypropylene and impact copolymerized polypropylene respectively, and by controlling the polymerization process, the homopolymer or random copolymer is polymerized in a ring tube at the front stage of the polymerization, which is very beneficial to reducing the crystallinity of the continuous phase part, thereby improving the gloss of the product; at the same time, using the random copolymer as the continuous phase can further improve the compatibility of the continuous phase with the dispersed phase rubber phase, thereby obtaining a product with a more uniform and refined distribution of the dispersed phase, which is advantageous in that the rubber phase content can be further reduced without reducing the impact resistance, and the adverse effect on the rigidity of the product can be reduced.
[0203] In the propylene polymer described in the present invention, the ethylene content can be designed according to actual needs, and the ethylene content in the product can be adjusted within a large range. The propylene polymer can obtain a homopolymer or a random copolymer with a narrow molecular weight distribution through the process control of the loop reactor; and then copolymerization is carried out in a horizontal reactor. The retention time of the reaction materials in the horizontal reactor is basically the same, and the reaction time of various materials can be controlled to be uniform. The materials in the horizontal reactor are in plug flow motion, and the materials are fully back-mixed in the radial direction of the reactor, and there is no back-mixing in the axial direction, so that the reaction conditions at various locations in the reactor are basically the same, and the obtained copolymer has a narrow molecular weight distribution, and the size of the rubber dispersed phase is much smaller than that of the conventional impact-resistant copolymer polypropylene dispersed phase. The product rubber phase has a small size, good dispersibility, and uniform distribution, which can make the product achieve higher gloss and rigidity, and ensure the product's good impact resistance.
[0204] The feeding method and system of the propylene catalyst proposed in the present invention control the uniformity of the components of the catalyst suspension, and control the temperature of the catalyst premix and the pressure of the buffer before entering the polymerization reactor so that it is the same as the conditions of the polymerization reaction before entering the polymerization reactor, thereby minimizing the influence of the catalyst feeding process on the polymerization reaction, controlling the process conditions of the polymerization reaction, and further providing a guarantee for the preparation of high-performance polypropylene with designable molecular structure; it can be seen from the test data of the product performance of Comparative Example 1 and Example 2 that the feeding method has a good effect on improving the product performance. Furthermore, the feeding method and the feeding system perform stirring control on each link through which the catalyst premix flows, so that the catalyst premix is continuously in a state of uniform components, the catalyst will not settle during the transportation process, and the clogging of the feed pipeline is avoided, thereby reducing the probability of production failures and improving production efficiency.
[0205] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. A method for feeding a propylene polymerization catalyst, characterized in that: A feeding system using a propylene polymerization catalyst comprises a batching tank, a metering tank, a diaphragm metering pump, a conveying pipeline and a buffer tank which are connected in sequence, wherein the buffer tank is connected to a propylene polymerization reaction device, wherein the batching tank, the metering tank, the conveying pipeline and the buffer tank are respectively provided with a stirrer, wherein the buffer tank is also provided with a temperature controller and a pressure regulator; the stirrer provided in the conveying pipeline is an oblique-paddle stirrer, wherein the oblique-paddle stirrer is composed of two straight blades, and the two blades are folded 45° to 60° in opposite directions; a plurality of stirrers are provided in the conveying pipeline, and the distance between adjacent stirrers is less than 2m; The feeding method comprises the following steps: 1) uniformly mixing a propylene polymerization catalyst and liquid propylene to obtain a catalyst premix liquid; 2) the catalyst premix liquid is metered, conveyed and buffered in sequence and then introduced into a propylene polymerization reactor to participate in a propylene polymerization reaction, wherein the components of the catalyst premix liquid are controlled to be uniform during the metering, conveying and buffering processes, and the temperature of the catalyst premix liquid during the buffering process is controlled to be the same as the temperature during the propylene polymerization reaction; The conveying process uses a pipeline equipped with a stirrer; The buffering process includes stirring and circulating the catalyst premix in a buffer tank, and then adjusting the temperature of the catalyst premix and the pressure in the buffer tank; The metering process includes stirring and circulating the catalyst premix in a metering tank and accurately metering the catalyst premix by a diaphragm metering pump.
2. The method for feeding a propylene polymerization catalyst according to claim 1, characterized in that: The metering tanks include at least two, and the metering tanks are connected in parallel.
3. The method for feeding a propylene polymerization catalyst according to claim 1, characterized in that: A protective valve is arranged between the metering tank and the diaphragm metering pump; the diaphragm metering pump is a stroke-adjustable diaphragm metering pump.
4. A method for preparing high-impact and high-gloss polypropylene, characterized in that: It includes the following steps: 1) using the feeding method according to any one of claims 1 to 2 to pass the catalyst premixed liquid into a loop reactor to carry out a first polymerization with a first olefin monomer; The first polymerization includes a prepolymerization reaction and a liquid phase bulk polymerization reaction occurring sequentially; the reaction temperature of the prepolymerization reaction is 10-40°C, the reaction pressure is 2.8-4.1Mpa, and the reaction time is 3-5min; the reaction temperature of the liquid phase bulk polymerization reaction is 55-95°C, and the polymerization pressure is 2.2-6.5Mpa; During the prepolymerization reaction, the first olefin monomer is propylene; and during the first polymerization, the mass concentration of the propylene polymerization catalyst in the catalyst premix is ≥50%; In the liquid phase bulk polymerization process, the first olefin monomer is propylene or an olefin mixture, the olefin mixture is composed of propylene with a molar percentage of ≥96% and other olefins with a molar percentage of ≤4%, and the other olefins are ethylene and / or butene; 2) using the feeding method described in any one of claims 1 to 2 to pass the catalyst premixed liquid into a horizontal reactor for second polymerization with the product obtained in step 1) and a second olefin monomer; The second olefin monomer is at least two of ethylene, propylene and butene; the molar percentage of ethylene in the second olefin monomer is ≤60%; The reaction temperature of the second polymerization is 60-80°C and the reaction pressure is 2.0-3.0Mpa; In the second polymerization process, the amount of the catalyst in the catalyst premix is 0.02-0.10% by mass of the second olefin monomer.
5. The preparation method according to claim 4, characterized in that: The reaction temperature of the liquid phase bulk polymerization reaction is 60-80° C., and the reaction pressure is 2.7-4.0 MPa.
6. The preparation method according to claim 4, characterized in that: The propylene polymerization catalyst comprises a main catalyst and a co-catalyst; wherein, The main catalyst comprises a magnesium compound carrier, a transition metal halide, an alcohol having 2 to 15 carbon atoms and an electron donor, and the molar ratio of the four is 1: (1-40): (0.01-10): (0.01-10); The cocatalyst comprises an organic aluminum compound; the organic aluminum compound comprises an alkyl aluminum and / or an alkyl aluminum hydrolyzate alkyl aluminumoxane; In terms of molar ratio, the ratio of the transition metal halide to the organoaluminum compound is 1:(10-500).
7. The preparation method according to claim 6, characterized in that: The electron donor is selected from at least one of an organophosphorus compound, an organosilane, cyclohexylmethyldimethoxysilane, dicyclopentyldimethoxysilane, and an electron donor as shown in Formula I: In Formula I, R1 and R6 are each independently selected from C1-C 12 Straight chain alkyl, C3-C 12 Branched alkyl, C3-C 15 Cycloalkyl, C3-C 15 R2, R3, R4, R5 are each independently selected from H atoms, halogen, C1-C 12 Straight chain alkyl, C3-C 12 branched alkyl, C3-C8 cycloalkyl, C6-C 15 Aryl, C6-C 15 wherein R2 and R3, R3 and R4, R4 and R5 are independently connected to form a ring or not.
8. The preparation method according to claim 5, characterized in that: In the liquid phase bulk polymerization process, the amount of the catalyst used is 0.02 to 0.10% by mass of the liquid phase propylene in the first olefin monomer.
9. The preparation method according to claim 5, characterized in that: The liquid phase bulk polymerization reaction adopts a polymerization reaction loop tube, and the polymerization reaction loop tube includes a plurality of polymerization loop tube units connected in parallel, and the polymerization loop tube unit includes a plurality of annular reaction tubes connected in series.
10. The preparation method according to claim 9, characterized in that: The polymerization reaction loop pipe is connected in series with the horizontal reactor.
11. The preparation method according to claim 4, characterized in that: The reaction temperature of the second polymerization is 65-75° C., and the reaction pressure is 2.4-2.5 MPa.
12. The preparation method according to claim 4, characterized in that: The first polymerization further comprises the step of adding a first auxiliary agent, wherein the first auxiliary agent comprises a molecular weight regulator; the second polymerization further comprises the step of adding a second auxiliary agent, wherein the second auxiliary agent comprises a molecular weight regulator.
13. The preparation method according to claim 4, characterized in that: A horizontal stirring shaft is arranged in the horizontal reactor, and a plurality of stirring paddles are arranged on the horizontal stirring shaft.
14. The preparation method according to claim 4, characterized in that: The horizontal reactor is divided into a gasification separation zone and a gas phase polymerization reaction zone along the feeding direction; a partition is arranged between the gasification separation zone and the gas phase polymerization reaction zone; a gap is arranged between one end of the partition and the side wall of the horizontal reactor.
Citation Information
Patent Citations
Gas-phase polymerization of propylene
CN102030841A
Propylene polymerization production technology by loop reactor
CN102399333A
Polypropylene or propylene-ethylene copolymer preparation method
CN109776702A
Propylene polymerization method and propylene polymerization device
CN111116785A
Charge -in system of polypropylene catalyst
CN205275504U