Method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy and dealuminization
By performing thermal reduction of aluminum on fluorotitanate and electrolyzing in low-temperature molten salt, the difficulty of deoxygenation and high cost problems in the preparation of metal titanium in the prior art are solved, and efficient and low-cost titanium extraction is achieved, reducing the Environmental pollution and energy consumption.
Patent Information
- Application Number
- CN202110959613.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-08-20
AI Technical Summary
The prior art faces problems of deoxygenation difficulties, high investment costs of equipment, low environmental pollution and low efficiency when preparing metal titanium, especially the problems of deoxygenation difficulties have not been effectively solved.
The aluminum-thermal reduction of fluorotitanate was performed at 750℃-850℃ to form a spongy TiAl, TiAl3, AlTi3 alloy or mixture thereof, and electrolyzed aluminum in low-temperature molten salt, and the aluminum was heated by aluminum reduction method. Combined with low-temperature molten salt electrolysis method, the extraction of high-purity metal titanium is achieved.
This method significantly improves the deoxygenation rate, reduces preparation costs, reduces environmental pollution, shortens the process flow, and greatly reduces energy consumption through low-temperature electrolysis, improves current efficiency, and avoids the emergence of deoxygenation problems.
Smart Images

Figure CN115707798B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal smelting and extraction, and specifically relates to a method for smelting and extracting high-purity Ti metal materials, and in particular to a method for preparing metallic Ti based on low-temperature molten salt electrolytic dealuminization of titanium-aluminum alloys. Background Art
[0002] Titanium metal has excellent properties such as light weight, high strength, high hardness, and corrosion resistance. It is widely used in aerospace, military industry, marine industry, medical and petroleum, and has become one of the high-performance metal materials that are essential for the development of the 21st century. In recent years, my country's titanium sponge production has continued to grow. At present, my country's titanium production ranks first in the world. Titanium metal products and secondary processed titanium alloy products are mainly distributed in titanium profiles, titanium powders, forged titanium, and involve high value-added alloy materials.
[0003] At present, the method for preparing sponge titanium in domestic and foreign industries is mainly the magnesium thermal reduction of titanium tetrachloride (TiCl4) method (Kroll method). This process is relatively complex and energy-intensive, and has a great impact on the environment, thus limiting the further expansion and application of this process. Its principle is to reduce titanium tetrachloride to sponge titanium using metallic magnesium in a high-temperature environment filled with inert gas, remove the reduction product magnesium chloride (MgCl2) and excess reducing agent Mg by vacuum distillation, and then further process to obtain sponge-like metallic titanium. The Kroll method has many problems, such as complex process, long time cycle, serious environmental pollution, generation of corrosive gas, large equipment investment and high cost, and the storage and transportation of titanium tetrachloride are also very difficult.
[0004] At the same time, the method of preparing metallic titanium by molten salt electrolysis of titanium dioxide (TiO2) (FFC method), USTB method and PRP method have been widely studied and are considered by the field to be the most likely to replace the Kroll method. The FCC method uses calcium chloride (CaCl2) molten salt as the electrolyte and performs electrolysis at high temperature. When current passes through, the titanium ions in the cathode TiO2 gain electrons and undergo reduction; at the anode, the oxygen ions lose electrons and undergo oxidation reaction, and oxygen combines with carbon to generate CO2 that escapes the electrolytic cell, thereby obtaining metallic titanium. At present, the deoxidation efficiency of this method during the electrolysis process is extremely low. The USTB process uses titanium dioxide and carbon as raw materials for carbon thermal reduction at high temperature to prepare titanium oxide (TiC x O y ), using it as the anode for electrolysis in a high-temperature molten salt system, and obtaining high-purity titanium metal at the cathode. At present, this method is difficult to separate the metal and the molten salt, has a large impact on the environment and has low current utilization. The RPR method is different from the previous two methods. This method belongs to the metal thermal reduction method, and its principle is to use metal vapor to directly reduce the TiO2 in the raw material of the molded body. This method also has the problems of high cost, difficulty in deoxidation and low efficiency, so it is difficult to use in large-scale industrial production.
[0005] At present, many processes are faced with problems such as difficulty in deoxygenation, high equipment investment cost, environmental pollution, and low efficiency. In particular, there is no good solution to the problem of difficulty in deoxygenation. Summary of the invention
[0006] In view of the above problems existing in the prior art, the technical problem to be solved by the present invention is: how to provide a method for preparing metallic titanium with high deoxidation rate, high efficiency and low preparation cost.
[0007] In order to solve the above technical problems, the present invention adopts the following technical scheme: using metal aluminum powder as a reducing agent, in a corundum crucible with a lid, aluminothermic reduction of fluorotitanate is carried out for 0.5h-3.0h at 750℃-850℃ in an inert gas protection environment; after the reaction is sufficient, the lid of the corundum crucible is lifted, and the temperature is increased to 1050℃-1250℃ for evaporation to remove unreacted fluorotitanate, cryolite generated by the reaction, and other unreacted low-boiling impurities; after evaporation, a sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is obtained in the corundum crucible, and TiAl, TiAl3, AlTi3 or a mixture thereof is used to electrolytically remove aluminum in a low-temperature molten salt to obtain high-purity metallic Ti at the anode.
[0008] As an improvement, the fluorotitanate is sodium fluorotitanate or potassium fluorotitanate.
[0009] As an improvement, the low temperature molten salt composition is BMIC-AlCl3, wherein the molar ratio of BMIC to AlCl3 is 1:1-1:2
[0010] As an improvement, the molar ratio of BMIC to AlCl3 is 1:2.
[0011] As an improvement, in the electrolysis process, a copper sheet is used as a cathode, a sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is used as an anode, and a BMIC-AlCl3 low-temperature molten salt is used as an electrolyte.
[0012] As an improvement, the electrolysis temperature of the electrolysis process is 25°C-90°C.
[0013] As an improvement, the amount of the metal aluminum powder added is 2-4wt% more than the amount required to generate Ti, TiAl, TiAl3 or AlTi3.
[0014] Compared with the prior art, the present invention has at least the following advantages:
[0015] 1. The invention proposes to achieve the purpose of purifying metallic Ti by secondary refining of low-temperature molten salt electrolysis based on aluminothermic reduction of fluorotitanate (Na2TiF6 or K2TiF6). Sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is obtained by aluminothermic reduction of fluorotitanate as the anode, and low-temperature molten salt sealed with n-decane is used as the electrolyte for electrolysis. The Al at the anode loses electrons to become Al ions and enters the low-temperature molten salt. The Al ions obtain electrons at the cathode to form single Al precipitation, and high-purity metallic Al is obtained. The remaining part of the anode is metallic Ti. Compared with the traditional solution for preparing metallic Ti, the present invention shortens the process flow, greatly reduces the preparation cost, reduces environmental pollution, reduces investment costs, and avoids the emergence of deoxidation problems.
[0016] 2. The present invention combines aluminothermic reduction with low-temperature molten salt electrolysis. The aluminothermic reduction process can produce porous sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof, thereby increasing its specific surface area and improving the reaction efficiency of the second step electrolysis. When electrolyzing sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof in low-temperature molten salt, an extremely low cell voltage can be used to dissolve aluminum at the anode and precipitate at the cathode, thereby achieving the purpose of secondary refining of metallic Ti. The electrolysis process greatly reduces energy consumption, the current efficiency in the process is extremely high, and high temperature is not required. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The electrolysis process flow chart of the method of the present invention is shown in FIG.
[0018] Figure 2 This is a diagram of a low-temperature molten salt electrolysis device.
[0019] In the figure, 1- copper electrode clamp; 2- polytetrafluoroethylene sealing cover; 3- electrolytic cell; 4- n-decane; 5- cathode copper sheet; 6- anode titanium aluminum alloy sheet; 7- electrolyte. DETAILED DESCRIPTION
[0020] The present invention is described in further detail below.
[0021] The present invention uses metal aluminum to perform aluminothermic reduction on fluorotitanate (Na2TiF6 or K2TiF6) at 750°C-850°C, and reduces the fluorotitanate to a sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof, completely avoiding the presence of oxygen in the metal, and performs evaporation treatment under high temperature conditions after the reaction, and evaporates the unreacted fluorotitanate, the fluoroaluminate generated by the reaction, and other low-boiling impurities that are not completely reacted at high temperature to obtain a sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof. The generated sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is used as an anode, and a low-temperature molten salt (BMIC-AlCl3) is used as an electrolyte for electrolytic dealuminization, and n-decane (C 10 H 22 ) is liquid-sealed to isolate the low-temperature molten salt from the air. During the electrolysis process, the Al in the anode loses electrons and becomes Al ions that are freed into the electrolyte, and obtains electrons at the cathode to precipitate, thereby obtaining high-purity metallic Al on the cathode, and the titanium-aluminum alloy of the anode is left with high-purity metallic Ti after dealumination. The present invention fully combines the method of preparing TiAl, TiAl3, AlTi3 alloys or mixtures thereof by aluminothermic reduction of fluorotitanate and the method of dealumination by low-temperature molten salt electrolysis to prepare high-purity metallic Ti and obtain high-purity metallic Al as a byproduct. This method greatly reduces energy consumption and reduces production costs.
[0022] See also Figure 1 and Figure 2 , a method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy, using metal aluminum powder as a reducing agent, in a corundum crucible with a lid, aluminothermic reduction of fluorotitanate is performed for 0.5h-3.0h at 750℃-850℃ under an inert gas protection environment. In specific implementation, the temperature of aluminothermic reduction can be selected from 750℃, 760℃, 770℃, 780℃, 790℃, 800℃, 810℃, 820℃, 830℃, 840℃, 850℃; the reaction time can be selected from 0.5h, 0.8h, 1.0h, 1.2h, 1.5h, 1.8h, 2h, 2.2h, 2.5h, 2.8h or 3h.
[0023] After the reaction is sufficient, the lid of the corundum crucible is lifted, and the temperature is raised to 1050°C-1250°C for evaporation to remove the unreacted fluorotitanate, the cryolite generated by the reaction, and other low-boiling impurities that are not completely reacted; the temperature is raised to 1050°C-1250°C in order to evaporate other low-boiling substances except titanium aluminum alloy and aluminum, including the unreacted reactant fluorotitanate, fluoride, and the fluoroaluminate generated by the reaction. In specific implementation, the evaporation temperature can be selected from 1050°C, 1080°C, 1100°C, 1130°C, 1150°C, 1180°C, 1200°C or 1250°C.
[0024] After evaporation, a sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is obtained in a corundum crucible. The TiAl, TiAl3, AlTi3 alloy or a mixture thereof is used to electrolytically remove aluminum in a low-temperature molten salt, and high-purity metallic Ti is obtained at the anode.
[0025] In a specific implementation, the fluorotitanate is sodium fluorotitanate or potassium fluorotitanate.
[0026] The low-temperature molten salt composition is BMIC-AlCl3, wherein the molar ratio of BMIC to AlCl3 is 1:1-1:2. In specific implementation, the molar ratio of BMIC to AlCl3 can be selected as 1:1, 1:1.5 or 1:2, preferably 1:2. This type of molten salt is also called an ionic solution. This type of ionic liquid is extremely sensitive to water and cannot be placed directly in the atmospheric environment. During the electrolysis process, n-decane is used for liquid sealing in a vacuum glove box.
[0027] In the electrolysis process, the copper sheet is used as the cathode, the sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is used as the anode, and the BMIC-AlCl3 low-temperature molten salt is used as the electrolyte. When a DC voltage is applied, the Al on the anode is oxidized to become Al ions that enter the electrolyte, and the cathode obtains electrons to generate single Al precipitation, forming a relatively high-purity metal Al, and the remaining part of the anode is a relatively high-purity metal Ti.
[0028] The amount of the metal aluminum powder added is 2-4wt% more than the amount required to generate Ti, TiAl, TiAl3 or AlTi3. Specifically, the amount of the metal aluminum powder added is 2wt%, 2.2wt%, 2.5wt%, 2.8wt%, 3wt%, 3.2wt%, 3.5wt%, 3.8wt% or 4wt% more than the amount required to generate Ti, TiAl, TiAl3 or AlTi3.
[0029] The electrolysis temperature of the electrolysis process is 25°C-90°C. In specific implementation, the electrolysis temperature can be selected from 25°C, 35°C, 45°C, 55°C, 65°C, 75°C, 85°C or 90°C.
[0030] The present invention combines aluminothermic reduction with low-temperature molten salt electrolysis to reduce fluorotitanate to produce porous sponge-like TiAl, TiAl3 and AlTi3 alloys, thereby increasing their specific surface area and improving the reaction efficiency of the second step of electrolysis. In the electrolysis of sponge-like TiAl, TiAl3, AlTi3 alloys or mixtures thereof in low-temperature molten salt, extremely low current density and cell voltage can be used to dissolve aluminum at the anode and precipitate at the cathode, thereby achieving the purpose of secondary refining of metallic Ti. The electrolysis process greatly reduces energy consumption, the current efficiency in the process is also very high, and high temperature is not required. The specific reaction equation involved is:
[0031] 3Na2TiF6+4Al+6NaF=3Ti+4Na3AlF6
[0032] 3Na2TiF6+7Al+6NaF=3AlTi+4Na3AlF6
[0033] 3Na2TiF6+13Al+6NaF=3Ti Al3+4Na3AlF6
[0034] 3K2TiF6+4Al+6KF=3Ti+4K3AlF6
[0035] 3K2TiF6+7Al+6KF=3AlTi+4K3AlF6
[0036] 3K2TiF6+13Al+6KF=3Ti Al3+4K3AlF6
[0037] Al+7AlCl - 4=4Al2Cl - 7+3e -
[0038] 4Al2Cl - 7+3e - =Al+7AlCl - 4
[0039] In summary, the present invention can electrolytically dealuminate various types of titanium-aluminum alloys produced in the aluminothermic reduction process, not limited to one type of titanium-aluminum alloy, and the various titanium-aluminum alloys obtained by aluminothermic reduction are all sponge-like, providing greater favorable conditions for the second step of electrolysis, increasing the reaction area, improving the reaction efficiency, shortening the reaction time, and the byproduct cryolite after evaporation, crystallization and purification can continue to be used as a raw material for industrial aluminum electrolysis. In the low-temperature molten salt electrolysis process, an extremely low cell voltage is used to reduce energy loss, have a higher current efficiency, and greatly reduce production costs.
[0040] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy, characterized in that: Using aluminum powder as a reducing agent, in a corundum crucible with a lid, the fluorotitanate is subjected to aluminothermic reduction at 750°C-850°C in an inert gas protection environment for 0.5h-3.0h; After the reaction is sufficient, the lid of the corundum crucible is lifted, and the temperature is raised to 1050°C-1250°C for evaporation to remove the unreacted fluorotitanate, the cryolite generated by the reaction, and other unreacted low-boiling impurities; After evaporation, a sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is obtained in a corundum crucible. 3、 AlTi3 or its mixed alloy is electrolyzed in low-temperature molten salt to remove aluminum, and high-purity metallic Ti is obtained at the anode.
2. The method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy according to claim 1, characterized in that: The fluorotitanate is sodium fluorotitanate or potassium fluorotitanate.
3. The method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy according to claim 1 or 2, characterized in that: The low-temperature molten salt composition is BMIC-AlCl3, wherein the molar ratio of BMIC to AlCl3 is 1:1-1:
2.
4. The method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloys according to claim 3, characterized in that: The molar ratio of BMIC to AlCl3 is 1:
2.
5. The method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy according to claim 3, characterized in that: In the electrolysis process, the copper sheet is used as the cathode, the sponge-like TiAl, TiAl3, AlTi3 alloy or a mixture thereof is used as the anode, and the BMIC-AlCl3 low-temperature molten salt is used as the electrolyte.
6. The method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy according to claim 4, characterized in that: The electrolysis temperature of the electrolysis process is 25°C-90°C.
7. The method for preparing metal Ti based on low-temperature molten salt electrolysis of titanium-aluminum alloy according to claim 5, characterized in that: The amount of the metal aluminum powder added is 2-4wt% more than the amount required to generate TiAl, TiAl3 or AlTi3.