A high-adhesion Cu thin film electrode and preparation method thereof

By using the transition connection layer and segmented plating process in the Cu thin film electrode, the adhesion and firmness problems of the Cu thin film electrode in extremely cold environments are solved, and an electrode with high adhesion, low resistance value and good stability is achieved. , ensuring the normal operation of the electric heating window in extremely cold environments and the stability of multiple power-ups.

CN115710686BActive Publication Date: 2024-10-15HUBEI JIUZHIYANG INFRARED SYST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211572790.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-10-15
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

Existing Cu film electrodes are prone to cracks or film peeling in extremely cold and low-temperature environments, causing the electric heating window to be unable to be powered and heated normally. When welding leads, the film thickness is too large, resulting in excessive residual stress, affecting firmness and adhesion.

Method used

Cu thin film electrodes are prepared by vacuum evaporation. Through the transition connection layer and optimized coating process parameters, the Cu thin film is plated in three stages, combined with ion-assisted deposition and heat preservation treatment to reduce residual stress and improve adhesion and firmness.

Benefits of technology

The Cu thin film electrode with high adhesion, low resistance value and good stability is realized to ensure that the electric heating window is stable and reliable under multiple energizations, and the welding does not suffer from perforation or falling off, making it adaptable to extremely cold environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115710686B_ABST
    Figure CN115710686B_ABST
Patent Text Reader

Abstract

The invention discloses a Cu thin film electrode with high adhesion, which comprises, from bottom to top, an optical substrate, an electric heating film, a transition connection layer and a Cu thin film; the transition connection layer adopts a metal chromium film with a thickness of 12nm to 15nm; the metal thin film electrode obtained by the invention has excellent firmness and excellent adhesion of the film layer on the surface of the optical substrate; the film layer can be welded without perforation and shedding, has a low resistance value, is easy to connect leads on its surface by welding, is stable and reliable when powered on multiple times, and has good environmental adaptability; the shape and contour can be customized according to design requirements, and the plating of metal thin film electrodes of various shapes can be realized by designing a coating fixture with a suitable structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical films, and in particular relates to a high-adhesion Cu film electrode and a preparation method thereof. Background Art

[0002] When optoelectronic equipment is used in extremely cold and low-temperature environments, problems such as ice, frost and fog often occur on the outer surface of its optical window, which seriously affects the observation of optoelectronic equipment. Plating an electric heating film on the window surface and electrically heating the optical window can effectively solve the problems of ice, frost and condensation.

[0003] Metal electrodes are an important part of electrically heated optical components, and their function is to conduct electricity. Generally speaking, leads need to be made at both ends of the electrodes to connect to an external power supply to electrically heat the optical components. The metal electrodes need to meet two prerequisites: first, the adhesion between the metal electrode and the optical component substrate is high enough, and the firmness does not change after multiple power-ons; second, it has excellent electrical conductivity, with a resistance value of less than 1Ω.

[0004] At present, there are many ways to manufacture metal electrodes, among which vacuum evaporation of copper (Cu) thin film is a good choice. The conductivity of copper is second only to silver, and it has high resistance to electromigration and mechanical strength. It is one of the most commonly used metal materials in the field of micro-nano manufacturing and is considered to be the most promising metal wiring material in the field of integrated circuits in the 21st century. For metal electrodes used in optical windows, adhesion and firmness are one of the most important performance parameters of optical films, which determine the safety performance and service life of electrically heated optical windows. When the firmness of the metal film electrode is poor, cracks will appear or the electrode film will fall off under the pulling of external forces, resulting in the inability of the electrically heated window to be powered on and heated normally, and the heating function will fail. In addition, when the Cu film is used as an electrode, leads need to be welded at both ends. The Cu film needs to be strong and tensile, and the solder joints will not fall off. When the solder wire is pulled with a certain amount of force, the film will not fall off. The film thickness is usually in the micrometer range. When a thicker film is prepared by vacuum evaporation, when the thickness is in the micrometer range, the film will fall off when the residual stress of the film is too large. Physical vapor deposition is used to prepare thicker metal films. There are usually two preparation processes: evaporation and sputtering. Process parameters such as deposition rate, substrate temperature and auxiliary ion source parameters will seriously affect the residual stress of the film.

[0005] Based on the requirements of the electrically heated optical window for metal electrodes, how to prepare a Cu thin film electrode with high adhesion, high firmness, no perforation or shedding during film welding, low resistance and good stability has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] The purpose of the present invention is to provide a high-adhesion Cu thin film electrode and a preparation method thereof, to realize current convergence by vacuum evaporating a metal Cu thin film electrode of a certain thickness on an optical substrate, to realize low residual stress and high adhesion of the micron-level thin film by utilizing a transition connection layer and optimizing the coating process parameters, and to solve the difficult problems of high-quality electrodes of electrically heated optical elements with high firmness, no perforation or shedding of the film layer during welding, low resistance value, and good stability after multiple power-ons.

[0007] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0008] A high-adhesion Cu thin film electrode comprises, from bottom to top, an optical substrate, an electric heating film, a transition connection layer, and a Cu thin film; the transition connection layer is a metal chromium film with a thickness of 12nm to 15nm.

[0009] According to the above solution, the optical substrate is made of K9 tempered glass, sapphire or silicon.

[0010] According to the above scheme, the electric heating film selects a suitable technical path according to the working band required by the optical window, and specifically adopts ITO conductive film or metal grid electrode.

[0011] According to the above scheme, the Cu film has a thickness of 1100nm to 1300nm and is plated in three stages;

[0012] The first stage is low-rate deposition with ion source assistance, with a deposition rate of 0.4±0.1nm / s and a deposition thickness of (75±5)nm;

[0013] The second stage is a higher rate deposition with ion source assistance, the deposition rate is 1.5±0.1nm / s, and the deposition thickness is (225±10)nm;

[0014] In the third stage, no auxiliary ion source was added and high-rate deposition was performed. The deposition rate was 3.5±0.1nm / s and the deposition thickness was (900±50)nm.

[0015] According to the above scheme, the metal electrode film layer is kept warm for 1 hour after plating to release its stress aging.

[0016] The method for preparing the high-adhesion Cu thin film electrode comprises the following steps:

[0017] 1) According to the heating requirements of the optical element, an electric heating film is prepared on the surface of the substrate;

[0018] 2) After passing the test, it is cleaned and then put into the vacuum coating machine;

[0019] 3) Baking treatment: Turn on the upper and lower baking systems of the vacuum coating machine to perform high-temperature baking treatment on the optical parts. The baking temperature is set to 180°C and the insulation time is 2 hours;

[0020] 4) Ion beam cleaning: Oxygen and argon with a purity of not less than 99.99% are introduced into the Mark II ion source at the same time. The ion source parameters are: anode voltage of (180±5)V, anode current of (3±0.2)A, neutralization current of (16.5±0.2)A, argon flow rate of (5±0.2)sccm, oxygen flow rate of (7.5±0.2)sccm, and ion beam cleaning treatment time of not less than 10 minutes;

[0021] 5) Plating of transition connection layer: the ion-assisted anode voltage of Cr film is (175±5)V, the anode current is (3±0.2)A, the electron gun beam current is (42±2)mA, the working gas Ar flow rate is (10.0±0.5)sccm; the deposition rate is (0.20±0.02)nm / s, and the thickness is 12nm~15nm;

[0022] 6) Three-stage plating of micron-scale Cu film:

[0023] For the plating of the Cu connecting layer, the ion-assisted source was turned on, the ion-assisted anode voltage was (180±5) V, the anode current was (3±0.2) A, the deposition rate was (0.4±0.1) nm / s, and the deposition physical thickness was (75±5) nm;

[0024] For the plating of the Cu connecting layer, the ion-assisted source was turned on, the ion-assisted anode voltage was (180±5) V, the anode current was (3±0.2) A, the deposition rate was (1.5±0.1) nm / s, and the deposition physical thickness was (225±10) nm;

[0025] For the deposition of Cu film, the ion-assisted source was turned off, the deposition rate was (3.5±0.1)nm / s, and the deposition physical thickness was (900±50)nm;

[0026] 6) Keep warm for 1 hour and then remove.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The micron-scale Cu film prepared in three steps has low residual stress. The strong diffusion ability of the Cu film during high-temperature plating enables it to bond with a thinner metal film transition bonding layer that does not affect the power-on effect, further improving the adhesion between the film layers.

[0029] The metal film electrode has excellent firmness and excellent adhesion to the film layer on the surface of the optical substrate.

[0030] The metal film electrode can achieve film layer welding without perforation and shedding, has low resistance value, is easy to connect leads by welding on its surface, is stable and reliable when powered on multiple times, and has good environmental adaptability.

[0031] The shape and contour of the metal thin film electrode can be customized according to the design requirements, and the plating of metal thin film electrodes of various shapes can be achieved by designing a coating fixture with a suitable structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 : Schematic diagram of the structure of the high adhesion Cu thin film electrode of the present invention;

[0033] It includes an optical substrate 1, an electric heating film 2, a transition connection layer 3, and a Cu film 4. DETAILED DESCRIPTION

[0034] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0035] The specific embodiment of the present invention provides a high adhesion Cu thin film electrode, the structure of which is as follows Figure 1 As shown, an electric heating film 2, a transition connection layer 3 for enhancing the firmness of the metal electrode, and a Cu film 4 with a thickness of micrometers are deposited on an optical substrate 1. The electric heating film 2 generates heat during the power-on process of the optical element to increase the surface temperature of the optical element, and quickly defogs and defrosts the window surface; the transition connection layer 3 uses a metal chromium film to enhance the adhesion between the metal electrode Cu film 4 and the electric heating film 2, achieve high adhesion between the Cu film with a thickness of micrometers and the electric heating film, and improve the firmness of the metal electrode film layer; the Cu film 4 realizes the convergence transmission of current. The metal electrode structure consists of a transition connection layer 3 and a Cu film 4. The metal electrode structure described above not only realizes the low resistance convergence current function of the electrode, but also realizes that the film layer does not perforate and fall off when the electrode lead is welded, and the electrode film layer is stable and reliable after multiple power-ons.

[0036] Specifically, the transition connection layer is made of a metal chromium film with a thickness of 12nm to 15nm.

[0037] Specifically, the optical substrate is made of K9 tempered glass, sapphire or silicon.

[0038] Specifically, the electric heating film is made of a suitable material according to the working band required by the optical window, and specifically uses an ITO conductive film or a metal grid electrode.

[0039] Specifically, the Cu film has a thickness of 1100nm to 1300nm and is deposited at 180°C in three stages;

[0040] The first stage is low-rate deposition with ion source assistance, with a deposition rate of 0.4±0.1nm / s and a deposition thickness of (75±5)nm;

[0041] The second stage is a higher rate deposition with ion source assistance, the deposition rate is 1.5±0.1nm / s, and the deposition thickness is (225±10)nm;

[0042] In the third stage, no auxiliary ion source was added and high-rate deposition was performed. The deposition rate was 3.5±0.1nm / s and the deposition thickness was (900±50)nm.

[0043] The specific embodiment also provides a method for preparing the above-mentioned high-adhesion Cu thin film electrode, comprising the following steps:

[0044] 1) According to the heating requirements of the optical element, an ITO electric heating film with a suitable resistance range (such as 150Ω±20Ω) is plated on the substrate surface by vacuum coating, or a sub-millimeter line width metal film (Al or Au) grid is prepared on the substrate surface by mask lithography and vacuum coating; after the electric heating film is prepared, its surface resistance is tested, and a dielectric protective film is prepared on the surface of the appropriate area of ​​the heating film; after the resistance and film firmness of the heating film are tested and qualified, it is transferred to the next process;

[0045] 2) After cleaning, the substrate with the heating film that has passed the test is placed in a vacuum evaporation coating machine;

[0046] 3) Baking treatment: Turn on the upper and lower baking systems of the coating machine to perform high-temperature baking treatment on the optical parts. The baking temperature is set to 180°C and the insulation time is 2 hours;

[0047] 4) Ion beam cleaning: Oxygen and argon with a purity of not less than 99.99% are introduced into the Mark II ion source at the same time. The ion source parameters are: anode voltage of (180±5)V, anode current of (3±0.2)A, neutralization current of (16.5±0.2)A, argon flow rate of (5±0.2)sccm, oxygen flow rate of (7.5±0.2)sccm, and ion beam cleaning treatment time of not less than 10 minutes;

[0048] 5) Plating of transition connection layer: the ion-assisted anode voltage of Cr film is (175±5)V, the anode current is (3±0.2)A, the electron gun beam current is (42±2)mA, the working gas Ar flow rate is (10.0±0.5)sccm; the deposition rate is (0.20±0.02)nm / s, and the thickness is 12nm~15nm;

[0049] 6) Three-stage plating of Cu film:

[0050] For the plating of the Cu connecting layer, the ion-assisted source was turned on, the ion-assisted anode voltage was (180±5) V, the anode current was (3±0.2) A, the deposition rate was (0.4±0.1) nm / s, and the deposition physical thickness was (75±5) nm;

[0051] For the plating of the Cu connecting layer, the ion-assisted source was turned on, the ion-assisted anode voltage was (180±5) V, the anode current was (3±0.2) A, the deposition rate was (1.5±0.1) nm / s, and the deposition physical thickness was (225±10) nm;

[0052] For the deposition of Cu film, the ion-assisted source was turned off, the deposition rate was (3.5±0.1)nm / s, and the deposition physical thickness was (900±50)nm;

[0053] 7) Keep warm for 1 hour and then remove.

[0054] The equipment used is Leybold ARES1110 vacuum coating machine, which is equipped with Mark Ⅱ ion source, two sets of 6-hole electron gun evaporation systems, two sets of substrate heating bakers, crystal oscillator film thickness monitoring system, vacuum exhaust system (oil-free dry pump, Polycold cold trap and cold pump), etc.

[0055] Example 1

[0056] A double-sided polished K9 tempered glass of 150mm×80mm×15mm is used as the substrate, an ITO film is selected as the electric heating film, chromium (Cr) is used as the coating material of the transition connection layer, and copper (Cu) is used as the metal material of the thin film electrode.

[0057] The plating process is specifically implemented as follows:

[0058] 1) Take K9 tempered glass, sapphire or silicon with good thermal shock performance as the substrate, and use ion-assisted vacuum evaporation to coat a layer of ITO electric heating film on its surface, and coat the dielectric protective film on the surface of the substrate ITO film except the position of the heating electrode. After the coating is completed, test its surface resistance within the range of 150Ω±20Ω to be qualified, and inspect the firmness of the film layer. After passing the inspection, transfer to the next process;

[0059] 2) Substrate cleaning: First, use a non-woven cloth dipped in a small amount of alcohol and ether mixture to clean the K9 glass with ITO film on the surface. The wiping track is circular. During the wiping process, the breath method is used to check the cleanliness of the substrate. Wipe and check while wiping until the substrate surface is free of pollution. CeO2 and other polishing liquids are prohibited during the wiping process. After the glass component is installed in the coating fixture, it is dried with dry high-purity nitrogen and finally placed in the vacuum coating machine.

[0060] 3) Heating and baking treatment of optical components: Place the optical component in the upper part of the vacuum chamber with the coated surface facing downward, and then turn on the substrate rotation system. When the background vacuum degree of the coating machine is ≤2.0E-6mbar, turn on the upper and lower baking systems of the coating machine at the same time to perform high-temperature baking treatment on the optical parts and keep them warm for a long time. The baking temperature is set to 180℃ and the insulation time is 2 hours.

[0061] 4) Ion beam cleaning of optical components: After the baking holding time is reached, oxygen and argon with a purity of not less than 99.99% are simultaneously introduced into the Mark II ion source. The ion source parameters are: anode voltage of (180±5)V, anode current of (3±0.2)A, neutralization current of (16.5±0.2)A, argon flow rate of (5±0.2)sccm, oxygen flow rate of (7.5±0.2)sccm, and the ion beam cleaning treatment time is not less than 10 minutes.

[0062] 5) A layer of Cr film was deposited on the optical element by ion beam assisted thermal evaporation: the ion assisted anode voltage of the Cr film was (175±5) V, the anode current was (3±0.2) A, the electron gun beam current was (42±2) mA, the working gas Ar flow rate was (10.0±0.5) sccm; the deposition rate was (0.20±0.02) nm / s, and the physical thickness of the Cr film was 12 nm to 15 nm.

[0063] 6) The deposition process of micron-scale Cu thin film is divided into four steps: ① Pre-melting treatment of Cu film material, the emission current is gradually loaded to 150mA, and the time is not less than 5 minutes until its blue molten pool opens; ② Plating of Cu connecting layer, turn on the ion-assisted source, the ion-assisted anode voltage is (180±5)V, the anode current is (3±0.2)A, the deposition rate is (0.4±0.1)nm / s, and the deposition physical thickness is (75±5)nm; ③ Plating of Cu connecting layer, turn on the ion-assisted source, the ion-assisted anode voltage is (180±5)V, the anode current is (3±0.2)A, the deposition rate is (1.5±0.1)nm / s, and the deposition physical thickness is (225±10)nm; ④ Plating of Cu film, turn off the ion-assisted source, the deposition rate is (3.5±0.1)nm / s, and the deposition physical thickness is (900±50)nm.

[0064] 7) After the Cu film is plated, continue to keep warm for 1 hour. After the last layer of moisture-proof, mildew-proof and hydrophobic film is plated, turn off the electron gun, keep the vacuum state, and leave it for 2 hours before opening the door to take out the parts.

[0065] Performance Testing:

[0066] The adhesion and firmness of the Cu thin film electrode obtained in this embodiment were tested using a plating sample of the same size. The surface of the film layer was scratched in a tic-tac-toe pattern using a blade, and a 25.4 mm wide Scotch 610 tape was adhered to the surface of the Cu film and then quickly pulled up vertically. The film layer did not fall off or peel off.

[0067] The resistance of the Cu thin film electrode obtained in this embodiment is tested by using a multimeter, and the probes of the multimeter are placed at both ends of the electrode film. The tested resistance of the electrode film is less than 1Ω.

[0068] The Cu thin film electrode of this embodiment is applied to the dielectric anti-reflection film and then the wire is welded. Under the condition of 60℃±10℃, the obtained optical element is connected to a 100V DC power supply for heating and power supply, and is also connected to a temperature control and temperature measuring device. The power is continuously supplied for more than 100 hours, and there is no abnormality in the electrode film.

Claims

1. A high adhesion Cu thin film electrode, characterized in that From bottom to top, they are optical substrate, electric heating film, transition connection layer, and Cu film; The transition connection layer is made of a metal chromium film with a thickness of 12nm to 15nm, which is prepared by ion beam assisted thermal evaporation; The electric heating film selects a suitable technical path according to the working band required by the optical window, and specifically adopts ITO conductive film or metal grid electrode; The Cu film is plated in three stages: The first stage is low-rate deposition with ion source assistance, with a deposition rate of 0.4±0.1nm / s and a deposition thickness of 75±5nm; The second stage is a higher rate deposition with ion source assistance, the deposition rate is 1.5±0.1nm / s, and the deposition thickness is 225±10nm; In the third stage, no auxiliary ion source was added and high-rate deposition was performed, the deposition rate was 3.5±0.1nm / s, and the deposition thickness was 900±50nm.

2. The high adhesion Cu thin film electrode as claimed in claim 1, characterized in that The optical substrate is made of K9 tempered glass, sapphire or silicon.

3. The method for preparing the high-adhesion Cu thin film electrode according to claim 1, characterized in that The following steps are involved: 1) According to the heating requirements of the optical element, an electric heating film is prepared on the surface of the substrate; 2) After passing the inspection, it is cleaned and then put into the vacuum coating machine; 3) Baking treatment: Turn on the upper and lower baking systems of the vacuum coating machine to perform high-temperature baking treatment on the optical parts. The baking temperature is set to 180°C and the insulation time is 2 hours; 4) Ion beam cleaning: Oxygen and argon with a purity of not less than 99.99% are introduced into the Mark II ion source at the same time. The ion source parameters are: anode voltage of 180±5V, anode current of 3±0.2A, neutralization current of 16.5±0.2A, argon flow rate of 5±0.2sccm, oxygen flow rate of 7.5±0.2sccm, and ion beam cleaning time of not less than 10 minutes; 5) Plating of transition connection layer: The ion-assisted anode voltage of the Cr film is 175±5V, the anode current is 3±0.2A, the electron gun beam current is 42±2mA, the working gas Ar flow rate is 10.0±0.5sccm; the deposition rate is 0.20±0.02nm / s, and the thickness is 12nm~15nm; 6) Three-stage plating of micron-scale Cu film: For the plating of the Cu connection layer, the ion-assisted source was turned on, the ion-assisted anode voltage was 180±5V, the anode current was 3±0.2A, the deposition rate was 0.4±0.1nm / s, and the deposition physical thickness was 75±5nm; For the plating of the Cu connection layer, the ion-assisted source was turned on, the ion-assisted anode voltage was 180±5V, the anode current was 3±0.2A, the deposition rate was 1.5±0.1nm / s, and the deposition physical thickness was 225±10nm; For the deposition of Cu film, the ion-assisted source was turned off, the deposition rate was 3.5±0.1nm / s, and the deposition physical thickness was 900±50nm; 7) Keep warm for 1 hour and then remove.