A fluorine-containing internal mold release agent and its preparation and application
The problem of insufficient compatibility and mobility of fluoropolymers is solved by using acrylate polymerized monomers and monomers with specific chain lengths in the internal mold release agent, and adding biomodified cellulose. It improves the demolding efficiency and quality of rubber and other products, reduces residue and adhesion properties, and enhances anti-aging properties.
Patent Information
- Application Number
- CN202210653949.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-06-10
AI Technical Summary
When used as internal release agents, due to poor compatibility and insufficient mobility, the release effect is poor and remains inside the product, affecting the quality of the product.
By selecting a solution polymerization reaction of acrylate polymerized monomers and monomers with specific chain lengths and adding biomodified cellulose to improve the compatibility and mobility of fluorine-containing polymers, a fluorine-containing mold release was prepared. agent.
Improve the mold release efficiency of the product, reduce mold stain generation, improve the fluidity and dispersion of the product, reduce the residue on the product, and effectively detach it during the second stage of vulcanization, improve the anti-adhesion property of the product and Anti-aging properties.
Smart Images

Figure CN115746206B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a fluorine-containing internal mold release agent and a preparation and application thereof. Background Art
[0002] Rubber and other polymer materials have become an indispensable part of today's society. They not only provide people with daily necessities and medical products, but also play an irreplaceable role in road traffic, mechanical electronics and other fields. With the rapid development of polymer synthetic materials such as rubber and plastics, the research on release agents has begun to attract attention from various industries at home and abroad.
[0003] Release agents are a type of industrial additives used to reduce the adhesion between polymer products such as rubber and molds and improve their demoulding effects. The addition of release agents can effectively improve demoulding efficiency, improve the integrity of products after demoulding, and ensure that the appearance quality is qualified. Release agents can be divided into external release agents and internal release agents according to different usage methods. External release agents are sprayed on the mold surface before the molded product is injected into the mold, and the operation is cumbersome. Internal release agents are generally added during product mixing. After heating, they will migrate to the contact surface between the product and the mold, helping the product to be removed smoothly. It is easy to operate and can be used for continuous production.
[0004] Commonly used release agents include wax release agents, silicon release agents and fluorine release agents. Relatively speaking, fluorine release agents have better demoulding effects. CN108659160A discloses a fluorine-containing polymer release agent, which is obtained by copolymerizing (1) a perfluoroalkyl group having 1 to 6 carbon atoms and a free radical polymerization reactive monomer without a functional group and (2) a free radical polymerization reactive monomer without a functional group. This polymer has good film-forming properties and demoulding properties when used as an external release agent, but when used as an internal release agent, due to the poor compatibility of the polymer with the molded product and the difficulty in migrating from the inside of the product to the surface, not only is the demoulding effect poor, but it will also remain inside the product, affecting the quality of the product. CN102782075A discloses a release agent composition, which comprises a fluorinated polymer and a medium, wherein the fluorinated copolymer comprises (a) a monomer based on a polyfluoroalkyl group with a specific carbon number of 1 to 6 and (b) an alkyl (meth) acrylate monomer with a specific carbon number of 18 to 30. The invention provides a release agent composition that can impart appropriate adhesion and peelability to the surface of articles such as protective materials, release films, and release papers of the bonding surface of label paper, adhesive sheets or adhesive tapes, and has a low environmental load. The product is an emulsion, mainly used for coating, and is an external release agent.
[0005] Bio-modified cellulose is a natural high molecular polymer formed by cellulose separated and purified from the residue of plant raw materials fermentation to prepare functional polysaccharides or bioethanol and modified by specific microorganisms. Its preparation and extraction process also adopts relatively mild process conditions. Compared with the cellulose obtained by traditional industries, bio-modified cellulose better retains the structural characteristics and chemical activity of natural cellulose. Direct addition can improve the performance of the product. Moreover, due to the amphiphilic properties of bio-modified cellulose, it can well alleviate the mixing of organic and inorganic phases in the product, so that the components can be better mixed and migrated, achieving the effect of uniform composition. Summary of the invention
[0006] The purpose of the present invention is to provide a fluorine-containing internal mold release agent and its preparation and application, by selecting acrylic ester polymer monomers with specific chain lengths and monomer input ratios, the compatibility and mobility of fluorine-containing polymers in products are improved, thereby improving the use effect of fluorine-containing polymers as internal mold release agents. In addition, the addition of cellulose modified by specific microorganisms greatly improves the performance of the product.
[0007] A fluorine-containing internal mold release agent is prepared by solution polymerization of a fluorine-containing monomer and a fluorine-free monomer. The fluorine-containing monomer is perfluorohexylethyl acrylate or perfluorohexylethyl methacrylate, and the fluorine-free monomer is behenyl acrylate.
[0008] A fluorine-containing internal mold release agent, the preparation process of which includes: solution polymerization and solvent removal.
[0009] Solution polymerization: add heptane (50-70%, mass fraction, the same below), ethyl acetate (0-10%), fluorine-containing monomer (10-30%), non-fluorine-containing monomer (5-10%), octadecyl mercaptan (1-0.1%) to the reactor, heat and stir to dissolve under the protection of inert gas, and raise the temperature to 60-90°C. Dissolve azobisisobutyronitrile (0.5-1.5%) and bio-modified cellulose (0.5-1.5%) in ethyl acetate (3-10%), and after the above temperature reaches the set value, add the azobisisobutyronitrile-ethyl acetate solution to the reactor, and react at a constant temperature for 6-8 hours under the protection of inert gas.
[0010] Solvent removal: The reaction product of the above step is subjected to rotary evaporation to remove the solvent, the rotary evaporation temperature is 60-70°C, and the pressure is 100-300 mbar. After the rotary evaporation is continued until no more solvent is evaporated, the product is taken out and placed in an oven for 6-8 hours, and the oven temperature is set to 80-120°C. After drying, a fluorine-containing internal mold release agent is obtained.
[0011] Wherein, the preparation method of bio-modified cellulose is:
[0012] Take industrially produced cellulose scraps (such as paper mill residues, straw, wood, etc.), dry and crush them, then pass through a 2mm sieve to remove impurities, weigh sodium alginate according to a dry material ratio of 1000:1-5, mix them, stir and mix them, spray water to make the water content reach 15-30%, and prepare a solid culture medium of lignocellulose raw material powder. Inoculate the bio-modified composite bacteria into the solid culture medium of lignocellulose raw material powder at an inoculation amount of 5-10%, and culture them at room temperature for 5 to 15 days. Weigh the modified lignocellulose raw material powder solid, put it into a three-necked flask, add a mixed solution of tetrahydrofuran and dioxane (the volume ratio of tetrahydrofuran and dioxane is 2:1), stir to promote the dissolution of bio-modified cellulose into the organic solvent, then heat to 90°C and a pressure of 0.3-0.5MPa for 1.5-3 hours, separate the bio-modified cellulose solution from other impurities insoluble in organic solvents by filtering, and remove the solvent from the solution by distillation to obtain bio-modified cellulose.
[0013] The bio-modified composite bacteria are commercial basidiomycetes (including one or more of Echinodontium sp., Trichaptum sp., Armillariella sp., Polyporellus sp., and Fomitopsis sp.) and Xanthomonas (including one or more of Xanthomonas vulgaris and Xanthomonas campestris), and the ratio of the two bacteria is 2-3:1-5.
[0014] Compared with the prior art, the benefits of the release agent of the present invention are: 1. It can improve the demoulding efficiency of the product; 2. It can reduce the generation of mold contamination; 3. It can improve the fluidity of the product and help the injection molding of the product; 4. It has good dispersibility and mobility in the molded product. The fluorocarbon chain of the above-mentioned fluorine-containing monomer will improve the compatibility of the polymer release agent in the product. After the fluorine-containing monomer is added to the polymer, the internal release agent can be evenly dispersed inside the product. The hydrocarbon chain of the non-fluorine-containing monomer will pull the polymer release agent to migrate to the mold surface during the product temperature vulcanization process to form a demoulding layer; 5. The residue on the product is low. Rubber and other products will be heated to 180-230°C during the second stage vulcanization. At this temperature, the release agent of the present invention will be detached in large quantities. In addition to being used for demoulding of products, the present invention can also be used for the storage of products. When rubber and other products are stacked and stored, the products will stick together due to intermolecular movement. Adding the release agent of the present invention to the product can effectively improve the anti-adhesion property of the product. Bio-modified cellulose is a network polymer. When it is compounded with other ingredients, it forms a cross-linked network structure with other ingredients, thus improving the performance of the product. This is mainly because bio-modified cellulose is a polyphenol-type polymer composed of phenylpropane structural units, which has the functions of absorbing ultraviolet light and anti-aging. Adding bio-modified cellulose can effectively improve the anti-aging properties of the product. Bio-modified cellulose has more active groups than traditional cellulose. Under certain conditions, aldehydes, phenols, epoxides, isocyanates, amines or halogenated derivatives of bio-modified cellulose can be prepared. It can also form grafted products with other monomers or co-precipitate with other polymer emulsions to form complexes, which can be used as an effective modification additive. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the state of the product after demoulding in Application Example 1
[0016] Figure 2 This is a comparison of the difficulty of separating rubber with and without fluorinated internal mold release agents. The left picture shows the rubber separation without spraying fluorinated internal mold release agents, and the right picture shows the rubber separation with spraying fluorinated internal mold release agents.
[0017] Figure 3 This is the state of the product after demoulding in Application Example 2
[0018] Figure 4 This is the state of the product after demoulding in Application Example 3
[0019] Figure 5 This is the state diagram of the product after demoulding in comparative application example 1
[0020] Figure 6 This is the state diagram of the product after demoulding in comparative application example 2
[0021] Figure 7 This is the state diagram of the product after demoulding in comparative application example 3
[0022] Figure 8 This is the state of the product after demoulding in comparative application example 4
[0023] Fig. 9 This is the state of the product after demoulding in comparative application example 5 DETAILED DESCRIPTION
[0024] The solution of the present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0025] Example 1: Add 69g of heptane, 4.5g of ethyl acetate, 20g of perfluorohexylethyl acrylate, 10g of behenyl acrylate, and 0.1g of octadecyl mercaptan to a closed reactor. Heat and stir to dissolve under nitrogen protection, and raise the temperature to 70°C. Dissolve 1.0g of azobisisobutyronitrile in 7.5g of ethyl acetate, and add it to the reactor after the temperature reaches 70°C. React at a constant temperature for 8 hours under nitrogen protection.
[0026] The above reaction product was subjected to rotary evaporation to remove the solvent, the rotary evaporation temperature was set at 60°C and the pressure was set at 250 mbar, and after the rotary evaporation was continued until no more solvent was evaporated, the product was placed in an oven for 8 hours, and the oven temperature was set at 90°C. After drying, a milky white solid was obtained, which was the fluorine-containing internal mold release agent, recorded as sample 1.
[0027] Example 2: Add 69g of heptane, 4.5g of ethyl acetate, 20g of perfluorohexylethyl methacrylate, 10g of behenyl acrylate, and 0.1g of octadecyl mercaptan to a sealed reactor. Heat and stir to dissolve under nitrogen protection, and raise the temperature to 70°C. Dissolve 1.0g of azobisisobutyronitrile in 7.5g of ethyl acetate, and add it to the reactor after the temperature reaches 70°C. React at a constant temperature for 8 hours under nitrogen protection.
[0028] The above reaction product was subjected to rotary evaporation to remove the solvent, the rotary evaporation temperature was set at 60°C and the pressure was set at 250 mbar, and after the rotary evaporation until no more solvent was evaporated, the product was placed in an oven for 8 hours, and the oven temperature was set at 90°C. After drying, a milky white solid was obtained, which was recorded as sample 2.
[0029] Example 3: Add 69g of heptane, 4.5g of ethyl acetate, 15g of perfluorohexylethyl acrylate, 8g of behenyl acrylate, and 0.1g of octadecyl mercaptan to a sealed reactor. Heat and stir to dissolve under nitrogen protection, and raise the temperature to 70°C. Dissolve 1.0g of azobisisobutyronitrile in 7.5g of ethyl acetate, and add it to the reactor after the temperature reaches 70°C. React at a constant temperature for 8 hours under nitrogen protection.
[0030] The above reaction product was subjected to rotary evaporation to remove the solvent, the rotary evaporation temperature was set at 60°C and the pressure was set at 250 mbar, and after the rotary evaporation was continued until no more solvent was evaporated, the product was placed in an oven for 8 hours, and the oven temperature was set at 90°C. After drying, a milky white solid was obtained, which was recorded as sample 3.
[0031] Example 4: Prepared according to the method of Example 1, recorded as sample 4, wherein 1.0 g of bio-modified cellulose was added to ethyl acetate at the same time, wherein the preparation method of bio-modified cellulose is:
[0032] Take the common farm waste straw, dry it, crush it, and then pass it through a 2mm sieve to remove the impurities. Weigh the sodium alginate according to the dry material ratio of 1000:1, mix it, stir and mix it, spray water to make the water content reach 15%, and prepare the solid culture medium of lignocellulose raw material powder. The biologically modified composite bacteria (commercial basidiomycete agent, commercial Xanthomonas agent, the ratio of the two bacteria is 1:1) are inoculated into the solid culture medium of lignocellulose raw material powder at an inoculation rate of 5%, and cultured at room temperature for 10 days. Weigh the modified lignocellulose raw material powder solid, put it into a three-necked flask, add a mixed solution of tetrahydrofuran and dioxane (the volume ratio of tetrahydrofuran and dioxane is 2:1), stir to promote the dissolution of biologically modified cellulose in the organic solvent, and then heat it to 90℃ and pressure 0.5MPa for 1.5 hours. The biologically modified cellulose solution is separated from other impurities insoluble in organic solvents by filtration, and the solution is distilled to remove the solvent to obtain biologically modified cellulose.
[0033] Example 5: Prepared according to the method of Example 2, recorded as sample 5, wherein 1.0 g of bio-modified cellulose was simultaneously added to ethyl acetate, wherein the preparation method of the bio-modified cellulose was the same as that of Example 4.
[0034] Comparative Example 1: In a closed reactor, add 69g of heptane, 4.5g of ethyl acetate, 20g of perfluorohexylethyl acrylate, 10g of tetradecyl acrylate, and 0.1g of octadecyl mercaptan. Under nitrogen protection, heat and stir to dissolve, and raise the temperature to 70°C. Dissolve 1.0g of azobisisobutyronitrile in 7.5g of ethyl acetate, and add it to the reactor after the temperature reaches 70°C. React at a constant temperature for 8 hours under nitrogen protection.
[0035] The above reaction product was subjected to a rotary evaporation to remove the solvent, the rotary evaporation temperature was set at 60°C and the pressure was set at 250 mbar, and after the rotary evaporation was continued until no more solvent was evaporated, the product was placed in an oven for 8 hours, and the oven temperature was set at 90°C. After drying, a milky white solid was obtained, which was recorded as comparative sample 1.
[0036] Comparative Example 2: After fully dissolving 45 g of perfluorohexylethyl methacrylate and 5 g of behenyl acrylate, add 4 g of polyoxyethylene (n=20) lauryl ether, 0.2 g of lauryl mercaptan, 7 g of dipropylene glycol monomethyl ether and 95 g of ion exchange water, and emulsify using a high-pressure homogenizer. The obtained emulsion is connected to a 300 ml four-necked bottle with a reflux cooling tube, a nitrogen inlet tube, a thermometer and a stirring device, and maintained at 60°C for about 1 hour under a nitrogen flow. A solution obtained by dissolving 0.3 g of ammonium persulfate in 5 g of water is added to initiate polymerization. Heat and stir at 60°C for 3 hours to prepare an aqueous copolymer latex.
[0037] The above product was placed in an oven for 8 hours, and the oven temperature was set at 90° C. After drying, a milky white solid was obtained, which was recorded as comparative sample 2.
[0038] Comparative Example 3: 69 g of heptane, 4.5 g of ethyl acetate, 20 g of perfluorobutylethyl methacrylate, 10 g of behenyl acrylate, and 0.1 g of octadecyl mercaptan were added to a sealed reactor. Under nitrogen protection, the mixture was heated and stirred to dissolve, and the temperature was raised to 70°C. 1.0 g of azobisisobutyronitrile was dissolved in 7.5 g of ethyl acetate, and after the temperature reached 70°C, it was added to the reactor. The reaction was carried out at a constant temperature for 8 hours under nitrogen protection.
[0039] The above reaction product was subjected to a rotary evaporation to remove the solvent, the rotary evaporation temperature was set at 60°C and the pressure was set at 250 mbar, and after the rotary evaporation was continued until no more solvent was evaporated, the product was placed in an oven for 8 hours, and the oven temperature was set at 90°C. After drying, a milky white solid was obtained, which was recorded as comparative sample 3.
[0040] Comparative Example 4: 69 g of heptane, 4.5 g of ethyl acetate, 20 g of perfluorobutyl ethyl acrylate, 10 g of hexadecyl acrylate, and 0.1 g of octadecyl mercaptan were added to a closed reactor. Under nitrogen protection, the mixture was heated and stirred to dissolve, and the temperature was raised to 70°C. 1.0 g of azobisisobutyronitrile was dissolved in 7.5 g of ethyl acetate, and after the temperature reached 70°C, it was added to the reactor. The reaction was carried out at a constant temperature for 8 hours under nitrogen protection.
[0041] The above reaction product was subjected to a rotary evaporation to remove the solvent, the rotary evaporation temperature was set at 60° C., the pressure was set at 250 mbar, and after the rotary evaporation was continued until no more solvent was evaporated, the product was placed in an oven for 8 hours, and the oven temperature was set at 90° C. After drying, a milky white solid was obtained, which was recorded as comparative sample 4.
[0042] Comparative Example 5: 69 g of heptane, 4.5 g of ethyl acetate, 20 g of perfluorooctylethyl acrylate, 10 g of behenyl acrylate, and 0.1 g of octadecyl mercaptan were added to a sealed reactor. Under nitrogen protection, the mixture was heated and stirred to dissolve, and the temperature was raised to 70°C. 1.0 g of azobisisobutyronitrile was dissolved in 7.5 g of ethyl acetate, and after the temperature reached 70°C, it was added to the reactor. The reaction was carried out at a constant temperature for 8 hours under nitrogen protection.
[0043] The above reaction product was subjected to a rotary evaporation to remove the solvent, the rotary evaporation temperature was set at 60° C., the pressure was set at 250 mbar, and after the rotary evaporation was continued until no more solvent was evaporated, the product was placed in an oven for 8 hours, and the oven temperature was set at 90° C. After drying, a milky white solid was obtained, which was recorded as comparative sample 4.
[0044] Application of fluorinated internal release agents in rubber products:
[0045] Application Example 1: Add the fluorinated mold release agent of Sample 1 prepared in Example 1 to the rubber during mixing, with the addition amount being mold release agent: rubber = 1:100. After the rubber is vulcanized and formed, the rubber product is taken out of the mold and the demoulding tensile force is measured. Sample 1 is dissolved in heptane to prepare a 0.1% (mass fraction, the same below) solution, which is applied to the rubber surface. Multiple layers of rubber coated with the solution are stacked together and stored at room temperature for one month, and the tensile force required to separate the rubber product is measured.
[0046] Demolding effect: The demoulding force is 17N. The state of the rubber product after demoulding is as follows: Figure 1 shown.
[0047] Separation force: 20N. Figure 2 This is a comparison chart of the difficulty of separating rubber with and without fluorinated internal mold release agents.
[0048] At the same time, the same experiment was carried out on sample 4, and the measured pressures were: demoulding tension: 13N, separation tension: 19N.
[0049] Application Example 2: Add the fluorinated mold release agent of Sample 2 prepared in Example 2 to the rubber during mixing, with the addition amount being mold release agent: rubber = 1:100. After the rubber is vulcanized and formed, the mold is opened to take out the rubber product, and the demoulding tensile force is measured. Sample 2 is dissolved in heptane to prepare a 0.1% solution, which is applied to the rubber surface. Multiple layers of rubber coated with the solution are stacked together and stored at room temperature for one month, and the tensile force required to separate the rubber product is measured.
[0050] Demolding effect: The demoulding force is 15N. The state of the rubber product after demoulding is as follows: Figure 3 shown.
[0051] Separation force: 20N.
[0052] At the same time, the same experiment was carried out on sample 5, and the measured pressures were: demoulding tension: 13N, separation tension: 18N.
[0053] Application Example 3: Add the fluorinated release agent of Sample 3 prepared in Example 3 to the rubber during mixing, with the addition amount being release agent: rubber = 1:100. After the rubber is vulcanized and formed, the mold is opened to take out the rubber product, and the demoulding tensile force is measured. Sample 3 is dissolved in heptane to prepare a 0.1% solution, which is applied to the rubber surface. Multiple layers of rubber coated with the solution are stacked together and stored at room temperature for one month, and the tensile force required to separate the rubber product is measured.
[0054] Demolding effect: The demoulding force is 16N. The state of the rubber product after demoulding is as follows: Figure 4 shown.
[0055] Separation force: 22N.
[0056] Comparative Application Example 1: The fluorine-containing mold release agent of Comparative Sample 1 prepared in Comparative Example 1 was added to the rubber during mixing, and the addition amount was mold release agent: rubber = 1:100. After the rubber was vulcanized and formed, the mold was opened to take out the rubber product, and the demoulding tensile force was measured.
[0057] Demolding effect: The demoulding force is 41N. The state of the rubber product after demoulding is as follows: Figure 5 shown.
[0058] Comparative Application Example 2: The fluorine-containing mold release agent of Comparative Sample 2 prepared in Comparative Example 2 was added to the rubber during mixing, and the addition amount was mold release agent: rubber = 1:100. After the rubber was vulcanized and formed, the mold was opened to take out the rubber product, and the demoulding tensile force was measured.
[0059] Demolding effect: The demoulding force is 32N. The state of the rubber product after demoulding is as follows: Figure 6 shown.
[0060] Comparative Application Example 3: The fluorine-containing mold release agent of Comparative Sample 3 prepared in Comparative Example 3 was added to the rubber during mixing, and the addition amount was mold release agent: rubber = 1:100. After the rubber was vulcanized and formed, the mold was opened to take out the rubber product, and the demoulding tensile force was measured.
[0061] Demolding effect: The demoulding force is 29N. The state of the rubber product after demoulding is as follows: Figure 7 shown.
[0062] Comparative Application Example 4: The fluorine-containing mold release agent of Comparative Sample 4 prepared in Comparative Example 4 was added to the rubber during mixing, and the addition amount was mold release agent: rubber = 1:100. After the rubber was vulcanized and formed, the mold was opened to take out the rubber product, and the demoulding tensile force was measured.
[0063] Demolding effect: The demoulding force is 31N. The state of the rubber product after demoulding is as follows: Figure 8 shown.
[0064] Comparative Application Example 5: The fluorine-containing mold release agent of Comparative Sample 5 prepared in Comparative Example 5 was added to the rubber during mixing, and the addition amount was mold release agent: rubber = 1:100. After the rubber was vulcanized and formed, the mold was opened to take out the rubber product, and the demoulding tensile force was measured.
[0065] Demolding effect: The demoulding force is 29N. The state of the rubber product after demoulding is as follows: Fig. 9 shown.
[0066] The comparison of rubber demoulding tensile force between each application example and the comparative application example is shown in Table 1:
[0067] Table 1 Comparison of demoulding tensile force between application examples and comparative application examples
[0068]
[0069]
[0070] The above is only a specific description of several embodiments and application examples of the present invention, and the contents are only for clearly explaining the technical solution of the present invention. It should be understood that these examples are not intended to limit the implementation and application scope of the present invention. Any modification or improvement made by those skilled in the art according to the present invention shall fall within the scope of protection of the claims of the present invention.
Claims
1. A fluorine-containing internal mold release agent, characterized in that: It is prepared by polymerization reaction of fluorine-containing monomers and fluorine-free monomers, and bio-modified cellulose is additionally added, wherein the fluorine-containing monomer is perfluorohexyl ethyl acrylate or perfluorohexyl ethyl methacrylate; the fluorine-free monomer is docosyl acrylate, and the molar ratio of the above fluorine-containing monomer to the fluorine-free monomer is 1-3:
1.
2. The method for preparing a fluorine-containing internal mold release agent according to claim 1, characterized in that: Step 1: Add fluorinated monomer, non-fluorinated monomer, heptane, ethyl acetate and octadecyl mercaptan into the reaction kettle in sequence, dissolve them under the protection of inert gas, and heat to 60-90°C; Step 2: dissolving azobisisobutyronitrile and bio-modified cellulose in ethyl acetate; Step 3: After the temperature of the reactor reaches the set temperature, add the solution of the second step into the reactor and react for 6-8 hours under inert gas protection and stirring conditions; Step 4: The product obtained in the third step is subjected to rotary evaporation at 150-400 mbar and 60-80° C., and after removing the solvent, it is placed in an oven for drying to obtain a fluorine-containing internal mold release agent; wherein the molar ratio of the fluorine-containing monomer to the fluorine-free monomer is 1-3:
1.
3. A method for preparing a fluorine-containing internal mold release agent as claimed in claim 2, characterized in that: The dissolution in the first step and the reaction in the third step are both carried out under the protection of inert gas.
4. The method according to claim 2, wherein the preparation process is as follows: Solution polymerization: add 50-70% by mass of heptane, 0-10% by mass of ethyl acetate, 10-30% by mass of fluorine-containing monomer, 5-10% by mass of non-fluorine-containing monomer, and 0.1-1% by mass of octadecyl mercaptan to a reactor, and heat and stir to dissolve under the protection of inert gas, and raise the temperature to 60-90°C; dissolve 0.5-1.5% by mass of azobisisobutyronitrile and 0.5-1.5% by mass of bio-modified cellulose in 3-10% by mass of ethyl acetate, and after the above temperature reaches the set value, add the azobisisobutyronitrile-ethyl acetate solution to the reactor, and react at a constant temperature for 6-8 hours under the protection of inert gas; Solvent removal: The reaction product of the above step is subjected to rotary evaporation to remove the solvent, the rotary evaporation temperature is 60-70°C, and the pressure is 100-300mbar; after rotary evaporation until no more solvent is evaporated, the product is taken out and placed in an oven for 6-8 hours, and the oven temperature is set to 80-120°C; after baking, a fluorine-containing internal release agent is obtained.
5. The method as claimed in claim 4, wherein the preparation method of bio-modified cellulose is as follows: take industrially produced cellulose scraps, dry them, crush them, and then pass them through a 2 mm sieve to remove impurities, weigh sodium alginate according to a dry-to-dry ratio of 1000:1-5, mix them, stir and mix them, spray water to make the water content reach 15-30%, and prepare a solid culture medium of lignocellulose raw material powder; inoculate the bio-modified composite bacteria into the solid culture medium of lignocellulose raw material powder at an inoculation rate of 5-10%, and culture them at room temperature for 5 to 15 days; weigh the modified lignocellulose raw material powder The solid powder is put into a three-necked flask, and a mixed solution of tetrahydrofuran and dioxane is added, wherein the volume ratio of tetrahydrofuran to dioxane is 2:1, and stirring is carried out to promote the dissolution of the bio-modified cellulose in the organic solvent, and then the mixture is heated to 90°C and the pressure is 0.3-0.5MPa for 1.5-3 hours, and the bio-modified cellulose solution is separated from impurities in other organic solvents by filtration, and the solution is distilled to remove the solvent to obtain the bio-modified cellulose; the bio-modified composite bacteria are commercial basidiomycetes and xanthomonas, and the ratio of the two bacteria is 2-3:1-5.
6. Use of the fluorine-containing internal mold release agent as claimed in claim 1 in the production of rubber and plastic products in a pultrusion process.
7. Use of the fluorine-containing internal mold release agent as claimed in claim 1 in preventing rubber products from sticking during storage.