A high-reliability polyimide resin absorbing adhesive film with controllable fluidity and a preparation method thereof
By adding inorganic fillers and perforating the absorbing film, the problems of uncontrollable fluidity and poor air permeability of the absorbing film are solved, the fluidity control and internal quality improvement of the absorbing laminate are realized, and the wave absorption efficiency is improved. The reliability of the laminate.
Patent Information
- Application Number
- CN202211414479.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-11
AI Technical Summary
The fluidity of the absorbing film is uncontrollable during the molding process, resulting in absorbent migration and poor air permeability, which reduces the reliability of the absorbing laminate.
Inorganic fillers are added to the absorbing adhesive film to adjust the viscosity and fluidity, and a hole punch is used to drill breathable holes, combined with vacuum bag exhaust to improve the curing quality of the laminate.
It achieves controllable fluidity of the absorbing film, avoids inter-layer migration of the absorber, ensures excellent absorbing performance and internal quality of the laminate, and improves the reliability of the absorbing laminate.
Smart Images

Figure CN115746719B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparing absorbing materials, and in particular relates to a highly reliable polyimide resin absorbing adhesive film with controllable fluidity and a preparation method thereof. Background Art
[0002] Absorbing materials refer to a type of material that can absorb and attenuate incident electromagnetic waves, and convert their electromagnetic energy into heat energy to dissipate or make the electromagnetic waves disappear due to interference. With the development of science and technology, absorbing materials have been widely used in various fields. For example, they are of great significance in electromagnetic protection, microwave darkroom, mobile communications, and military stealth. Due to the advantages of resin-based absorbing composite materials such as strong designability and large-area integral molding, they have become one of the most important application materials in the field of aerospace stealth.
[0003] Absorbent film is an intermediate material for preparing resin-based absorbing composite materials. It is mainly composed of electromagnetic wave absorbers and resin matrices. The absorbent film is formed by mixing the absorbent and the matrix resin and then calendering it into a film. It is then laminated with composite prepreg and cured to prepare a laminate material with both load-bearing and absorbing functions. Since absorbing laminates generally require a wider absorption frequency band, absorbing films with different electromagnetic parameters are required for matching laminations, so the fluidity of the absorbing film needs to be precisely controlled. Too high fluidity will lead to absorbent migration between different types of absorbing films, resulting in changes in electromagnetic parameters. Too low fluidity will cause the resin to be unable to fill the defects inside the laminate, resulting in reduced reliability of the absorbing laminate. At the same time, although the high-density absorbing film prepared by the calendering method has excellent electrical and mechanical properties, its air permeability is poor. It is difficult to effectively discharge the internal air during the molding process, and defects will form after curing, which will reduce the reliability of the laminate. Summary of the invention
[0004] In order to solve the problem of uncontrollable fluidity of absorbing film during the molding process and the problem of reduced reliability of absorbing layer due to exhaust difficulties, the present invention provides a highly reliable polyimide resin absorbing film with controllable fluidity and a preparation method thereof. Although related patents such as CN202010950674.3 and CN201910201141.2 mention the preparation method of absorbing film, the fluidity of the absorbing film prepared therefrom is uncontrollable. Too high fluidity of the absorbing film will lead to absorbent migration between different types of absorbing films, resulting in changes in electromagnetic parameters. Too low fluidity will result in the inability of the resin to fill the defects inside the ply, resulting in reduced reliability of the absorbing layer. At the same time, due to the dense internal structure of the absorbing film, its air permeability is poor, and it is difficult to effectively discharge the internal air during the molding process. Defects will be formed after curing, which will reduce the reliability of the layer.
[0005] In order to solve the above problems of the absorbing film, this patent will add inorganic fillers to the absorbing film. The concentration of inorganic fillers can effectively adjust the viscosity of the absorbing film, so that the thickness and fluidity of the film can be controlled during the curing process. At the same time, the inorganic fillers are low dielectric constant materials, which can adjust the fluidity of the film without affecting its absorbing performance. At the same time, a puncher is used to prepare air holes in the absorbing film, and a vacuum bag can be used to vent it after laying, effectively improving the reliability of the absorbing layer after curing.
[0006] In order to achieve the above object, the present invention provides, in a first aspect, a highly reliable polyimide resin absorbing adhesive film with controllable fluidity and a preparation method thereof, the method comprising the following steps:
[0007] (1) concentrating the polyimide resin solution to prepare a polyimide resin system;
[0008] (2) placing the polyimide resin system obtained in step (1), the absorbent, and the inorganic filler into a resin internal mixer for rough mixing, and then using an open mixer for fine mixing to obtain an absorbing resin blank;
[0009] (3) placing the absorbing resin blank obtained in step (2) into a precision calender to calender an absorbing film, and obtaining an absorbing resin film after calendering;
[0010] (4) The absorbing resin film obtained in step (3) is punched with air holes by a puncher to complete the preparation of the absorbing resin film.
[0011] Preferably, in the step (1), the polyimide prepolymer solution is concentrated using a rotary evaporator to a solid content of 50%-90% at a concentration temperature of 60-120°C.
[0012] Preferably, the internal mixing temperature of the internal mixing in step (2) is 20-300° C., the mixing time is 10 min-120 min, and the internal mixing rotor speed is 10-250 r / min.
[0013] Preferably, in step (2), an open mill is used for fine mixing, the open mill temperature is 20-300° C., the mixing time is 10-80 min, and the mixing roller speed is 2-17 m / min.
[0014] Preferably, in step (3), the calendering temperature is 20-300° C., the calendering thickness is 0.1-5 mm, the calendering pressure is 1-200 tons, and the calendering speed is 0.5-8 m / s.
[0015] Preferably, in step (4), the diameter of the air holes is 0.1 mm-2 mm, and the distance between the holes is between 0.5 mm and 15 mm.
[0016] Preferably, the mass fraction of each constituent substance in the wave-absorbing adhesive film is:
[0017] Absorbent: 15-85wt%; polyimide resin matrix: 10-45wt%; inorganic filler: 1-40wt%.
[0018] Preferably, the polyimide resin matrix is at least one selected from the group consisting of norbornene-terminated polyimide resin, cyano-terminated polyimide resin, and phenylethynyl-terminated polyimide resin.
[0019] Preferably, the absorbent is at least one selected from the group consisting of carbonyl iron, sendust, ferrite, conductive carbon black, carbon fiber, graphene, carbon nanotubes, and silicon carbide.
[0020] Preferably, the inorganic filler is at least one selected from the group consisting of hollow glass microspheres, nano-silicon dioxide, montmorillonite, and nano-alumina.
[0021] In a second aspect, the present invention provides a highly reliable polyimide wave-absorbing adhesive film with controllable fluidity, which is prepared by the method described in the first aspect of the present invention.
[0022] Compared with the existing wave-absorbing adhesive film with uncontrollable fluidity and low reliability, the present invention has at least the following beneficial effects:
[0023] (1) The absorbing film prepared by the present invention has no interlayer migration of absorbent during the curing process, the electromagnetic parameters of the absorbing film layer can be well maintained before and after curing, and the absorbing layer plate has good absorbing performance after curing.
[0024] (2) In the process of mixing the absorbing film, the vent holes can be used to fully exhaust the air. Meanwhile, during the curing process, the vent holes can be well filled with the absorbing resin. The internal quality of the absorbing layer is excellent and the reliability is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 .Microscopic photograph of the interlayer of the absorbing layer after curing in Example 1.
[0026] Figure 2 .Example 1 Ultrasonic scanning internal quality photos of the absorbing layer after curing.
[0027] Figure 3 Comparative Example 1: Ultrasonic scanning internal quality photo of the absorbing layer after curing. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:
[0031] (1) The polyimide prepolymer solution is concentrated using a rotary evaporator to a solid content of 80% at a concentration temperature of 100° C. The polyimide resin matrix is a norbornene-terminated polyimide resin.
[0032] (2) The polyimide resin system, absorbent and inorganic solid filler obtained in step (1) are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, fine mixing is performed using an open mixer to obtain an absorbing resin blank. In this step, the internal mixing temperature is 200°C, the mixing time is 80 minutes, and the internal mixing rotor speed is 200r / min; in this step, the open mixing temperature is 200°C, the mixing time is 60 minutes, and the mixing roller speed is 15m / min. The mass fractions of each substance are: polyimide resin system: 45wt%; absorbent dosage: 35wt%, inorganic filler: 20wt%. The absorbent is free carbonyl iron; and the inorganic filler is hollow glass microspheres.
[0033] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender for calendering an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 200° C., the calendering thickness is 2 mm, the calendering pressure is 100 tons, and the calendering speed is 6 m / s.
[0034] (4) The absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the absorbing film. In this step, the diameter of the air holes is 1 mm, and the hole spacing is 10 mm.
[0035] Example 2
[0036] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:
[0037] (1) The polyimide prepolymer solution is concentrated using a rotary evaporator to a solid content of 50% at a concentration temperature of 60° C. The polyimide resin matrix is a cyano-terminated polyimide resin.
[0038] (2) The polyimide resin system, absorbent and inorganic solid filler obtained in step (1) are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, fine mixing is performed using an open mixer to obtain an absorbing resin blank. In this step, the internal mixing temperature is 20°C, the mixing time is 10 min, and the internal mixing rotor speed is 10 r / min; in this step, the open mixing temperature is 20°C, the mixing time is 10 min, and the mixing roller speed is 2 m / min. The mass fractions of each substance are: polyimide resin system: 10 wt%; absorbent dosage: 80 wt%, inorganic filler: 10 wt%. The absorbent is sendust; the inorganic filler is nano-silicon dioxide.
[0039] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender to calender an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 20° C., the calendering thickness is 0.1 mm, the calendering pressure is 1 ton, and the calendering speed is 0.5 m / s.
[0040] (4) The absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the absorbing film. In this step, the diameter of the air holes is 0.1 mm, and the hole spacing is 0.5 mm.
[0041] Example 3
[0042] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:
[0043] (1) The polyimide prepolymer solution is concentrated using a rotary evaporator to a solid content of 90% at a concentration temperature of 120° C. The polyimide resin matrix is a polyimide resin terminated with phenylethynyl groups.
[0044] (2) The polyimide resin system, absorbent and inorganic solid filler obtained in step (1) are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, fine mixing is performed using an open mixer to obtain an absorbing resin blank. In this step, the internal mixing temperature is 300°C, the mixing time is 120min, and the internal mixing rotor speed is 250r / min; in this step, the open mixing temperature is 300°C, the mixing time is 80min, and the mixing roller speed is 17m / min. The mass fractions of each substance are: polyimide resin system: 45wt%; absorbent dosage: 45wt%, inorganic filler: 10wt%. The absorbent is ferrite; and the inorganic filler is montmorillonite.
[0045] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender for calendering an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 300° C., the calendering thickness is 5 mm, the calendering pressure is 200 tons, and the calendering speed is 8 m / s.
[0046] (4) The absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the absorbing film. In this step, the diameter of the air holes is 2 mm, and the hole spacing is 15 mm.
[0047] Example 4
[0048] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:
[0049] (1) The polyimide prepolymer solution is concentrated using a rotary evaporator to a solid content of 70% at a concentration temperature of 80° C. The polyimide resin matrix is a norbornene-terminated polyimide resin or a cyano-terminated polyimide resin.
[0050] (2) The polyimide resin system, absorbent and inorganic solid filler obtained in step (1) are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, fine mixing is performed using an open mixer to obtain an absorbing resin blank. In this step, the internal mixing temperature is 50°C, the mixing time is 50 minutes, and the internal mixing rotor speed is 100 r / min; in this step, the open mixing temperature is 60°C, the mixing time is 40 minutes, and the mixing roller speed is 8 m / min. The mass fractions of each substance are: polyimide resin system: 40wt%; absorbent dosage: 59wt%, inorganic filler: 1wt%. The absorbent is conductive carbon black; and the inorganic filler is nano-alumina.
[0051] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender to calender an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 100° C., the calendering thickness is 1 mm, the calendering pressure is 50 tons, and the calendering speed is 3 m / s.
[0052] (4) The absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the absorbing film. In this step, the diameter of the air holes is 1 mm, and the hole spacing is 3 mm.
[0053] Example 5
[0054] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:
[0055] (1) The polyimide prepolymer solution is concentrated using a rotary evaporator to a solid content of 80% at a concentration temperature of 90° C. The polyimide resin matrix is selected from the group consisting of norbornene-terminated polyimide resin, cyano-terminated polyimide resin, and phenylethynyl-terminated polyimide resin.
[0056] (2) The polyimide resin system, absorbent and inorganic solid filler obtained in step (1) are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, an open mixer is used for fine mixing to obtain an absorbing resin blank. In this step, the internal mixing temperature is 150°C, the mixing time is 60 minutes, and the internal mixing rotor speed is 120r / min; in this step, the open mixing temperature is 150°C, the mixing time is 50 minutes, and the mixing roller speed is 12m / min. The mass fractions of each substance are: polyimide resin system: 30wt%; absorbent dosage: 45wt%, inorganic filler: 25wt%. The absorbent is sendust and ferrite; the inorganic filler is hollow glass microspheres and nano-silica.
[0057] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender for calendering an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 150° C., the calendering thickness is 3 mm, the calendering pressure is 150 tons, and the calendering speed is 5 m / s.
[0058] (4) The absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the absorbing film. In this step, the diameter of the air holes is 1.5 mm, and the hole spacing is 10 mm.
[0059] Example 6
[0060] In this embodiment, the method for preparing a high-reliability wave-absorbing adhesive film with controllable fluidity comprises the following steps:
[0061] (1) The polyimide prepolymer solution is concentrated using a rotary evaporator to a solid content of 90% at a concentration temperature of 60° C. The polyimide resin matrix is a cyano-terminated polyimide resin or a phenylethynyl-terminated polyimide resin.
[0062] (2) The polyimide resin system, absorbent and inorganic solid filler obtained in step (1) are placed in a resin internal mixer for internal mixing and rough mixing. After rough mixing, fine mixing is performed using an open mixer to obtain an absorbing resin blank. In this step, the internal mixing temperature is 200°C, the mixing time is 100 min, and the internal mixing rotor speed is 200 r / min; in this step, the open mixing temperature is 250°C, the mixing time is 70 min, and the mixing roller speed is 16 m / min. The mass fractions of each substance are: polyimide resin system: 45wt%; absorbent dosage: 45wt%, inorganic filler: 10wt%. The absorbent is conductive carbon black; and the inorganic filler is nano-alumina.
[0063] (3) The absorbing resin blank obtained in step (2) is placed in a precision calender to calender an absorbing film to obtain an absorbing resin film. In this step, the calendering temperature is 250° C., the calendering thickness is 3 mm, the calendering pressure is 200 tons, and the calendering speed is 8 m / s.
[0064] (4) The absorbing film obtained in step (3) is punched with a puncher to form air holes, thereby completing the preparation of the absorbing film. In this step, the diameter of the air holes is 2 mm, and the hole spacing is 15 mm.
[0065] Comparative Example 1
[0066] This embodiment is consistent with the first three steps of embodiment 1, but does not include the fourth step, that is, no air holes are prepared.
[0067] The present invention provides a highly reliable polyimide resin wave-absorbing adhesive film with controllable fluidity and a preparation method thereof. Figure 1 This is a microscope photograph of the interlayers of the absorbing layer after curing of Example 1. As shown in the figure, the interface between the absorbing adhesive film layers of the absorbing layer material prepared by the present invention is clear, and there is no absorbent migration between the layers, which means that the fluidity of the absorbing adhesive film is controllable during the curing process and the layer structure is well maintained. Figure 2 This is a nondestructive ultrasonic test diagram of Example 1 after preparing air holes and then curing. It can be seen from the figure that there are no obvious defects in the layer board and the material has high reliability. Figure 3 This is the non-destructive test result of the laminate after curing of the wave-absorbing film without air-permeable holes prepared in comparative example 1. It can be seen that the laminate has large-area internal defects. Due to poor exhaust performance, there is air holding inside the laminate, which reduces the reliability of the laminate.
[0068] The specific embodiments of the present invention disclosed above are intended to help understand the content of the present invention and implement it accordingly. It can be understood by those skilled in the art that various replacements, changes and modifications are possible without departing from the spirit and scope of the present invention. The present invention should not be limited to the contents disclosed in the embodiments of this specification, and the scope of protection of the present invention shall be subject to the scope defined in the claims.
Claims
1. A method for preparing a highly reliable polyimide resin absorbing film with controllable fluidity, characterized in that: The method comprises the following steps: The polyimide resin solution is concentrated to prepare a polyimide resin system; wherein the polyimide resin solution is concentrated by using a rotary evaporator to concentrate the polyimide prepolymer solution to a solid content of 50% to 90% at a concentration temperature of 60 to 120° C. The polyimide resin system, the absorbent, and the inorganic filler are placed in a resin internal mixer for rough mixing, and then finely mixed using an open mixer to obtain an absorbing resin blank; the inorganic filler is at least one selected from the group consisting of hollow glass microspheres, nano-silica, montmorillonite, and nano-alumina; The absorbing resin blank is placed in a precision calender to calender the absorbing film, and a polyimide absorbing resin film is obtained after calendering; The absorbing resin film is punched with a punch to form air holes, thereby completing the preparation of the absorbing film. The air holes are used to fully exhaust the air during the mixing process of the absorbing film. At the same time, the air holes are filled with resin during the curing process, thereby improving the reliability of the absorbing layer after curing. The mass fraction of each constituent substance in the absorbing film is: Absorbent: 15-85wt%; polyimide resin matrix: 10-45wt%; inorganic filler: 1-40wt%.
2. The preparation method according to claim 1, characterized in that The banburying temperature of the rough mixing is 20-300° C., the mixing time is 10-120 minutes, and the rotating speed of the banburying rotor is 10-250 r / min.
3. The preparation method according to claim 1, characterized in that The open mill is used for fine mixing, and the adopted opening temperature is 20-300° C., the mixing time is 10-80 min, and the mixing roller speed is 2-17 m / min.
4. The preparation method according to claim 1, characterized in that The calendering temperature is 20-300° C., the calendering thickness is 0.1-5 mm, the calendering pressure is 1-200 tons, and the calendering speed is 0.5-8 m / s.
5. The preparation method according to claim 1, characterized in that The diameter of the air holes is 0.1mm-2mm, and the hole spacing is between 0.5mm-15mm.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The polyimide resin matrix is at least one selected from the group consisting of norbornene-terminated polyimide resin, cyano-terminated polyimide resin, and phenylethynyl-terminated polyimide resin; the absorbent is at least one selected from the group consisting of carbonyl iron, sendust, ferrite, conductive carbon black, carbon fiber, graphene, carbon nanotubes, and silicon carbide.
7. A high-reliability polyimide resin absorbing film with controllable fluidity prepared according to the method of any one of claims 1 to 6.
Citation Information
Patent Citations
Wave-absorbing adhesive film and preparation method thereof
CN111704868A
Wave-absorbing adhesive film material and preparation method thereof
CN112029421A
Broadband wave-absorbing force-bearing composite material and preparation method thereof
CN112644103A
Copper-based shielding wave-absorbing material
CN216752646U