A polyolefin release film with high dimensional stability and a method for manufacturing the same

By optimizing the material components and processes of the polyolefin base film layer in the release film, the problems of insufficient temperature resistance and complex process of the base film are solved, high dimensional stability and efficient production are achieved, and product quality and processing efficiency are improved. .

CN115746725BActive Publication Date: 2024-12-03ZHEJIANG DAOMING NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211492983.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-12-03
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

The base film of the existing release film has insufficient temperature resistance and complex process, which leads to the film being easily contracted and poor appearance under high temperature conditions, and has low processing efficiency and high cost.

Method used

A high-dimensional stability polyolefin release film was designed, by using rubber-containing block copolymerized polypropylene, maleic anhydride modified polypropylene, nucleating agent and other materials in the release agent adhesive layer and support layer. Optimize the layer thickness ratio and component ratio, balance mechanical properties and high-temperature dimensional stability, and use single-screw extruder and hot air circulation drying to improve adhesion and temperature resistance.

Benefits of technology

It improves the temperature resistance and quality of the film, simplifies the process flow, improves production efficiency and reduces costs, and ensures the high-temperature stability and appearance performance of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115746725B_ABST
    Figure CN115746725B_ABST
Patent Text Reader

Abstract

The present invention discloses a polyolefin release film with high dimensional stability and a manufacturing method thereof, comprising a release agent layer and a polyolefin base film layer, wherein the polyolefin base film layer comprises a release agent adhesive layer and a support layer, wherein the release agent layer, the release agent adhesive layer and the support layer are connected in sequence, wherein the layer thickness ratio of the release agent adhesive layer to the support layer is 80-90:10-20, the release agent adhesive layer is composed of a rubber phase-containing block copolymer polypropylene, maleic anhydride-modified polypropylene, a nucleating agent and an adhesion agent in a mass ratio of 85-95:5-15:0.1-1:0.05-0.5, and the support layer is composed of a homopolymer polypropylene, a toughening agent and a nucleating agent in a mass ratio of 80-95:1-15:0.1-1. The present invention solves the problem of insufficient temperature resistance through the above-mentioned design, and the product quality is higher and the structure is simpler, thereby making the manufacturing method simpler, the production efficiency higher and the cost lower.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of release films, and in particular to a polyolefin release film with high dimensional stability and a manufacturing method thereof. Background Art

[0002] The release material is coated with a release agent on the substrate. After being attached to the sticky material, it has a low and controllable peeling force and can be easily separated from the sticky material. Common release materials use BOPP, PET, paper, and paper-plastic composite substrates as the substrate. We call this type of release material a rigid release material. The rigid release material itself has high rigidity, modulus, stiffness, and low elongation. When the rigid release material is compounded with a film material that also has rigidity and a material that is more sensitive to temperature changes, when the material is bent, curved, or wound, or when the coil is wound too loosely and the tightness difference between the two ends is large, the stress will cause separation between the two, commonly known as "tunnel" and "wrinkle" phenomenon, which will damage the appearance and performance of the product. In this type of application, in order to avoid these problems, relatively flexible materials can be used as substitutes. Polyolefin films, especially polyethylene and polypropylene films, are relatively suitable for this type of application because of their good temperature resistance and relatively moderate modulus. However, many problems need to be solved in the actual preparation and application of release films. For example, after the release agent of the release film is applied, the free radicals of the silicone resin need to fully react to form a cross-linked structure to stabilize the release force and have a certain adhesion to the substrate. It usually needs to be thermally cured at 100℃~150℃, and light radiation curing and other means can also be used. It is also inevitable to withstand high temperatures. When the temperature resistance of the base film of the release film is insufficient, it is easy to cause the film to shrink, resulting in wide-width shrinkage, and may also cause poor appearance such as ripples. In addition, the use of generally commercially available flexible release materials is often only able to adopt the transfer bonding method due to their insufficient high temperature resistance, that is, first apply an adhesive (such as a solvent-based pressure-sensitive adhesive) on the substrate of the rigid release material and dry it, and then bond it to the rigid protected material, and then peel off the rigid release material on the rigid protected material and bond it to the flexible release material, commonly known as the "cold bonding" process. Its process is complicated, which will also affect processing efficiency, increase processing costs and quality risks.

[0003] Therefore, it is necessary to improve the above problems. Summary of the invention

[0004] The present invention aims at the defects of the prior art such as insufficient temperature resistance of the base film and complex process, and provides a novel polyolefin release film with high dimensional stability and a manufacturing method thereof.

[0005] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:

[0006] A polyolefin release film with high dimensional stability comprises a release agent layer and a polyolefin base film layer, wherein the polyolefin base film layer comprises a release agent adhesive layer and a support layer, wherein the release agent layer, the release agent adhesive layer and the support layer are connected in sequence, wherein the layer thickness ratio of the release agent adhesive layer to the support layer is 80-90:10-20, wherein the release agent adhesive layer is composed of a rubber phase-containing block copolymer polypropylene, maleic anhydride-modified polypropylene, a nucleating agent and an adhesion agent in a mass ratio of 85-95:5-15:0.1-1:0.05-0.5, and wherein the support layer is composed of a homopolymer polypropylene, a toughening agent and a nucleating agent in a mass ratio of 80-95:1-15:0.1-1.

[0007] The release agent adhesive layer and the support layer balance the mechanical properties and dimensional stability and adhesion at high temperature through the design of the above materials, layer thickness ratio and mass ratio. The main material of the release agent adhesive layer is a rubber-containing block copolymer polypropylene, whose heat deformation temperature is slightly lower than that of homopolymer polypropylene. Its flexibility and adhesion to the release agent are better than homopolymer polypropylene, and when a rubber-containing block copolymer polypropylene such as EPDM and EPDM is used, the flexibility and temperature resistance can be further enhanced. The auxiliary material in the release agent adhesive layer is maleic anhydride-modified polypropylene, whose polar functional group can improve the adhesion of the release agent and improve the compatibility between the compositions. The adhesion agent focuses on improving the adhesion between the release agent adhesive layer and the silicon-containing release agent. The nucleating agent further improves the mechanical properties and temperature resistance. The main material of the support layer is homopolymer polypropylene, which has strong rigidity and high heat deformation temperature. The design of the above components and proportions prevents the reduction of the overall flexibility of the release film. The toughening agent and nucleating agent of the auxiliary materials of the support layer are based on the supplement of the physical properties of the membrane material, further improving the mechanical properties and temperature resistance, so that the support layer has excellent dimensional stability and release agent adhesion after high-temperature baking.

[0008] The present invention solves the problem of insufficient temperature resistance through the above design, and the product quality is higher and the structure is simpler, thereby making the manufacturing method simpler, the production efficiency higher and the cost lower.

[0009] Preferably, in the above-mentioned polyolefin release film with high dimensional stability, the toughening agent is one or two of ethylene propylene diene monomer rubber and styrene-butadiene-styrene block copolymer.

[0010] The toughening of homopolypropylene can generally be achieved by blending random polypropylene copolymers, block copolymer polypropylene, POE elastomers, rubber elastomers, etc. The present invention not only takes advantage of the flexibility of polypropylene, but also needs to maintain a low thermal shrinkage rate, so EPDM rubber and styrene-butadiene-styrene block copolymers are preferred, and these two toughening agents have good compatibility with homopolypropylene, and have nucleation properties and good high temperature resistance, and can also reduce the stress whitening problem of homopolypropylene when the film is stretched.

[0011] Preferably, in the above-mentioned high dimensional stability polyolefin release film, the nucleating agent is a polypropylene masterbatch containing one or more of 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, 2,2'-methylene-bis(4,6-di-tert-butylphenyl) sodium phosphate, talc, and calcium carbonate.

[0012] The addition of nucleating agents can change the crystallinity of polypropylene and form an island structure, thereby improving the heat resistance and dimensional stability of the film material. The two nucleating agents, 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum and 2,2'-methylene bis(4,6-di-tert-butylphenyl) phosphate sodium, have a high heat-resistant decomposition temperature, good dispersibility in the polypropylene resin system, and better precipitation resistance than other types of small molecule nucleating agents. Inorganic nucleating agents such as talcum powder and calcium carbonate can synergistically enhance the toughening effect of the system. In order to improve processability, the nucleating agent is mixed with the polypropylene resin and then granulated by melt extrusion to form a masterbatch, which can improve the dispersion uniformity when used in film making.

[0013] Preferably, in the above-mentioned polyolefin release film with high dimensional stability, the adhesive is a mixed prefabricated masterbatch containing block copolymer polypropylene and siloxane-coated nano-silicon dioxide or macromolecular silicone.

[0014] Generally, the surface energy of release agents is low, so the adhesion to the substrate is high. After the release agent adhesive layer is attached to the release surface of the release film and then peeled off, the release agent is transferred to a lower degree and has less impact on the adhesion performance of the sticky material. The adhesion performance of siloxane-coated nano-fumed silica or macromolecular silicone and silicone release agents is better than other materials. After mixing siloxane-coated nano-fumed silica or macromolecular silicone with block copolymer polypropylene, it is melt-extruded and granulated to form a masterbatch, which improves the dispersibility and processing performance.

[0015] Preferably, in the above-mentioned polyolefin release film with high dimensional stability, the dynamic friction coefficient of the support layer side is 0.5-0.8.

[0016] The friction coefficient is controlled at the above level because the release film is bonded to the release agent adhesive layer to improve operability when used by back-end users. For example, it can avoid problems such as difficulty in fixing or resulting dimensional deviations during film cutting, spraying, and engraving due to an excessively low friction coefficient.

[0017] Preferably, in the above-mentioned polyolefin release film with high dimensional stability, a film venting groove is arranged in the release agent adhesive layer, and the film venting groove is one of a triangular structure, a square structure, a diamond structure, and a trapezoidal structure. The film venting grooves are regularly arranged, and the line width of the film venting groove is 5μm to 25μm, the line height is not more than 10μm, and the area of ​​a single structural unit is not more than 1mm 2 .

[0018] The purpose of setting the film venting groove in the release agent adhesive layer is that after the release agent adhesive layer is compounded with the release agent layer, an exhaust channel is formed on the surface of the release agent adhesive layer due to the "rubbing" effect. During the laminating operation, it can effectively prevent the formation of bubbles caused by encapsulating air and ensure the flatness of re-laminating, especially when performing manual operations or laminating irregular surfaces. Excellent laminating flatness can also be obtained. The design of the line width, line height and structural unit area of ​​the film venting groove ensures the effectiveness of the film venting groove. When the line width and line height are too small or the structural unit area is too large, a good exhaust effect cannot be obtained. When the line width and line height are too large, the release agent adhesive layer may not be leveled or the overall appearance may be affected. The above design can be adapted to more applications.

[0019] Preferably, in the above-mentioned polyolefin release film with high dimensional stability, the strength of the polyolefin-based film layer at a tensile elongation of 10% in an environment of 120° C. is 10N / 25mm to 20N / 25mm.

[0020] The tensile strength test in a high temperature environment can effectively characterize the temperature resistance of the release film. As a carrier of a viscous composite material, the release material may be a release film as a base film in actual application, and an adhesive such as a pressure-sensitive adhesive is coated on one side of the release agent. Whether it is water-based, solvent-based or light-curing pressure-sensitive adhesive, it needs to withstand high temperatures more or less during the manufacturing process. If the tolerance to high temperatures is poor, it will cause significant deformation of the release film in a high temperature environment, especially in roll-to-roll production, which will lead to problems such as narrowing of the width.

[0021] The reason for choosing to stretch at 120℃ and taking the value when the tensile deformation is 10% is that the drying temperature of the general solvent-based pressure-sensitive adhesive after coating is between 70℃ and 120℃, and 10% is basically close to the tensile yield point of the release film. When the strength at this point is too low, the film is more likely to be stretched or the width is significantly narrowed due to the tension and temperature of the equipment during roll-to-roll processing. When the strength is too high, it means that the rigidity of the polyolefin release film is too large and the flexibility is insufficient, and the products made from it are prone to "tunnel" and "wrinkle" problems.

[0022] Preferably, in the above-mentioned high dimensional stability polyolefin release film, after the polyolefin base film layer is baked at 150°C for 30 minutes, the thermal shrinkage rate along the directions of 0°, 45°, 90°, and 135° is less than or equal to 1%, and the difference in thermal shrinkage rate along 0° and 90° is within plus or minus 0.5%.

[0023] There are large differences in the temperature resistance of polyolefin release films obtained under different preparation conditions. Even if the same material and thickness are used, the heat shrinkage of the products obtained under different process conditions will be significantly different. For example, due to anisotropy, the difference in heat shrinkage in TD and MD directions is particularly large, which limits the application of release films in the back end, and the possibility of "tunnels" and "wrinkles" due to poor dimensional stability is also greater. Testing the heat shrinkage at 0°, 45°, 90°, and 135° respectively can also more strictly design the preparation conditions of release films. If the heat shrinkage is too large and exceeds the limit value, it means that its thermal deformation is large, and its applicability to specific applications is weakened. Limiting the difference in heat shrinkage between the 0° and 90° test points to within plus or minus 0.5% can better prevent problems caused by excessive dimensional changes during use.

[0024] Preferably, in the above-mentioned polyolefin release film with high dimensional stability, the release agent layer contains water-based or photosensitive free radical reactive silicone resin, fluorine-containing modified silicone resin, and fluorine-based release agent.

[0025] The release agent has a low surface tension and a low and controllable peeling force with the sticky material, so it can be used for sticky materials such as adhesive tapes. The above design improves the applicability of the present invention.

[0026] Preferably, the above-mentioned method for manufacturing a polyolefin release film with high dimensional stability comprises the following steps:

[0027] S1: using more than two groups of single screw extruders with a length-to-diameter ratio of 30:1, the prepared materials are respectively sent to the corresponding single screw extruders according to the functional layers, and then filtered through a melt filter, and enter a distributor, a confluence die head, a cooling roller group, a heat setting and recooling device, a transfer and traction device, and a winding device to obtain a polyolefin base film layer;

[0028] S2: coating a release agent on the upper side of the polyolefin base film layer by direct transfer or multi-roller transfer, then using hot air circulation drying or light radiation excitation to allow the release agent to react completely, and finally winding up to obtain a polyolefin release film with high dimensional stability.

[0029] Step S1, generally, the materials of different layers are batched and mixed according to the corresponding components, and then sent to the corresponding single-screw extruder. The main function of the melt filter is to filter impurities. The distributor re-meters the melt and distributes it in multiple layers. The converging die head refers to the melt co-extruded by multiple groups of screws or distributed into multiple layers by the distributor. It can be merged at the die head to achieve multi-layer co-extrusion. The main function of the cooling roller group is to cool the melt to achieve the purpose of shaping and film formation. The heat setting and re-cooling device is to better control the heat resistance of the CPP film. The transmission and traction device and the winding device are necessary units for the continuous production of coils.

[0030] Step S2, selecting the corresponding coating and drying method according to the type and characteristics of the release agent and the basic performance requirements of the release film. The direct transfer method or the multi-roller transfer method can be used to coat the release agent to obtain a high coverage and uniform coating. Hot air circulation drying and light radiation excitation are both aimed at the release agent, and make it react to make the release force and adhesion performance more stable.

[0031] Preferably, in the above-mentioned method for manufacturing a polyolefin release film with high dimensional stability, the processing temperature of the single-screw extruder, the melt filter, the distributor, and the confluence die is 200°C to 250°C.

[0032] The above design ensures that each layer of materials is melted, mixed evenly and maintains certain melt properties to form a stable film layer. If the temperature is too low, the material may not be fully melted or the melt viscosity may be too high. If the temperature is too high, excessive polymer may be produced, affecting the film-forming properties and appearance.

[0033] Preferably, in the above-described method for manufacturing a polyolefin release film with high dimensional stability, more than two groups of cooling rollers are arranged in the cooling roller group, the cooling rollers are located below the confluence die and the distance between the cooling rollers and the die lips of the confluence die is within 5 mm, the cooling rollers and the front of the confluence die are provided with a negative pressure adsorption device, the cooling rollers and the rear of the confluence die are provided with a positive pressure air knife device, and the cooling rollers are provided with roller exhaust grooves.

[0034] A negative pressure adsorption device is used to absorb the air between the film layer and the cooling roller after the material is discharged, ensuring that the melt flowing out of the confluence die head and the cooling roller are effectively attached to each other and quickly cooled to form a film. A positive pressure air knife device is used to allow high-speed airflow to sweep the surface of the film during film formation, accelerating the cooling of the film surface and forming a supplement to the negative pressure adsorption to prevent the formation of wrinkles. More than two sets of cooling rollers further enhance the cooling effect.

[0035] Preferably, in the above-described method for manufacturing a polyolefin release film with high dimensional stability, a setting roller group is provided in the heat setting and recooling device, and the setting roller group is composed of metal rollers with polished surfaces and a diameter greater than or equal to 500 mm, the number of the metal rollers is more than 5, and the metal rollers include more than 3 heating setting rollers and more than 2 cooling setting rollers.

[0036] The shaping roller group can reduce the stress and shape of the polyolefin film during the heating-cooling process, significantly reduce the thermal shrinkage of the polyolefin film, and improve the processing performance in the subsequent coating of release agent and pressure-sensitive adhesive.

[0037] Preferably, in the above-mentioned method for manufacturing a polyolefin release film with high dimensional stability, the heat setting temperature of the heat setting and recooling device is 100°C to 160°C, and the recooling temperature is 20°C to 40°C.

[0038] The above design is adapted to the characteristics of the material and the requirements after film formation. On the one hand, it eliminates the internal stress of polyolefin. At the same time, through the adaptation of heat setting and recooling devices, it can control the crystallinity of polyolefin and effectively regulate the mechanical properties of the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a structural schematic diagram of the present invention;

[0040] Figure 2 A reference diagram of the use state of the present invention;

[0041] Figure 3 It is a schematic diagram of the heat shrinkage test of the present invention. DETAILED DESCRIPTION

[0042] The following is combined with Figure 1-3 The present invention is further described in detail with specific embodiments, but they are not intended to limit the present invention:

[0043] Example 1

[0044] A polyolefin release film with high dimensional stability comprises a release agent layer 1 and a polyolefin base film layer 2, wherein the polyolefin base film layer 2 comprises a release agent adhesive layer 21 and a support layer 22, wherein the release agent layer 1, the release agent adhesive layer 21 and the support layer 22 are connected in sequence, wherein the layer thickness ratio of the release agent adhesive layer 21 to the support layer 22 is 80:20, wherein the release agent adhesive layer 21 comprises a rubber phase-containing block copolymer polypropylene, maleic anhydride-modified polypropylene, a nucleating agent and an adhesion agent in a mass ratio of 95:5:1:0.5, and wherein the support layer 22 comprises a homopolymer polypropylene, a toughening agent and a nucleating agent in a mass ratio of 95:1:1.

[0045] Preferably, the toughening agent is one or two of EPDM rubber and styrene-butadiene-styrene block copolymer.

[0046] Preferably, the nucleating agent is a polypropylene masterbatch containing one or more of 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, 2,2'-methylene-bis(4,6-di-tert-butylphenyl) sodium phosphate, talc, and calcium carbonate.

[0047] Preferably, the adhesive is a mixed prefabricated masterbatch containing block copolymer polypropylene and siloxane-coated nano-silicon dioxide or macromolecular silicone.

[0048] Preferably, the dynamic friction coefficient of the support layer 22 side is 0.5.

[0049] Preferably, the release agent adhesive layer 21 is provided with a film venting groove, which is a triangular structure, a square structure, a diamond structure, and a trapezoidal structure. The film venting grooves are regularly arranged, and the line width of the film venting grooves is 5 μm, the line height is not more than 10 μm, and the area of ​​a single structural unit is not more than 1 mm 2 .

[0050] Preferably, the strength of the polyolefin-based film layer 2 at a tensile elongation of 10% in an environment of 120° C. is 10 N / 25 mm.

[0051] Preferably, after the polyolefin-based film layer 2 is baked at 150°C for 30 minutes, the thermal shrinkage rate along the directions of 0°, 45°, 90° and 135° is less than or equal to 1%, and the difference in thermal shrinkage rate along 0° and 90° is within plus or minus 0.5%.

[0052] Preferably, the release agent layer 1 contains water-based or photosensitive free radical reactive silicone resin, fluorine-containing modified silicone resin, or fluorine-based release agent.

[0053] As a preference, the method comprises the following steps:

[0054] S1: using more than two groups of single screw extruders with a length-to-diameter ratio of 30:1, the prepared materials are respectively sent to the corresponding single screw extruders according to the functional layers, and then filtered through a melt filter, and enter a distributor, a confluence die head, a cooling roller group, a heat setting and recooling device, a transfer and traction device, and a winding device to obtain a polyolefin base film layer 2;

[0055] S2: coating the release agent on the upper side of the polyolefin base film layer 2 by direct transfer or multi-roller transfer, then using hot air circulation drying or light radiation excitation to allow the release agent to react completely, and finally winding up to obtain a polyolefin release film with high dimensional stability.

[0056] Preferably, the processing temperature of the single-screw extruder, the melt filter, the distributor and the confluence die is 200°C.

[0057] Preferably, more than two groups of cooling rollers are arranged in the cooling roller group, the cooling rollers are located below the confluence die and the distance between the cooling rollers and the die lip of the confluence die is within 5 mm, the cooling rollers and the front of the confluence die are provided with a negative pressure adsorption device, the cooling rollers and the rear of the confluence die are provided with a positive pressure air knife device, and the cooling rollers are provided with roller exhaust grooves.

[0058] Preferably, a setting roller group is provided in the heat setting and recooling device, and the setting roller group consists of metal rollers with polished surfaces and a diameter greater than or equal to 500 mm. The number of the metal rollers is more than 5, and the metal rollers include more than 3 heating setting rollers and more than 2 cooling setting rollers.

[0059] Preferably, the heat setting temperature of the heat setting and recooling device is 100°C, and the recooling temperature is 20°C.

[0060] Example 2

[0061] A polyolefin release film with high dimensional stability comprises a release agent layer 1 and a polyolefin base film layer 2, wherein the polyolefin base film layer 2 comprises a release agent adhesive layer 21 and a support layer 22, wherein the release agent layer 1, the release agent adhesive layer 21 and the support layer 22 are connected in sequence, wherein the layer thickness ratio of the release agent adhesive layer 21 to the support layer 22 is 85:15, wherein the release agent adhesive layer 21 comprises a rubber phase-containing block copolymer polypropylene, maleic anhydride-modified polypropylene, a nucleating agent and an adhesion agent in a mass ratio of 90:10:0.5:0.25, and wherein the support layer 22 comprises a homopolymer polypropylene, a toughening agent and a nucleating agent in a mass ratio of 87.5:12.5:0.5.

[0062] Preferably, the toughening agent is one or two of EPDM rubber and styrene-butadiene-styrene block copolymer.

[0063] Preferably, the nucleating agent is a polypropylene masterbatch containing one or more of 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, 2,2'-methylene-bis(4,6-di-tert-butylphenyl) sodium phosphate, talc, and calcium carbonate.

[0064] Preferably, the adhesive is a mixed prefabricated masterbatch containing block copolymer polypropylene and siloxane-coated nano-silicon dioxide or macromolecular silicone.

[0065] Preferably, the dynamic friction coefficient of the support layer 22 side is 0.65.

[0066] Preferably, the release agent adhesive layer 21 is provided with a film venting groove, which is a triangular structure, a square structure, a diamond structure, and a trapezoidal structure. The film venting grooves are regularly arranged, and the line width of the film venting grooves is 15 μm, the line height is not more than 10 μm, and the area of ​​a single structural unit is not more than 1 mm 2 .

[0067] Preferably, the strength of the polyolefin-based film layer 2 at a tensile elongation of 10% in an environment of 120° C. is 15 N / 25 mm.

[0068] Preferably, after the polyolefin-based film layer 2 is baked at 150°C for 30 minutes, the thermal shrinkage rate along the directions of 0°, 45°, 90° and 135° is less than or equal to 1%, and the difference in thermal shrinkage rate along 0° and 90° is within plus or minus 0.5%.

[0069] Preferably, the release agent layer 1 contains water-based or photosensitive free radical reactive silicone resin, fluorine-containing modified silicone resin, or fluorine-based release agent.

[0070] As a preference, the method comprises the following steps:

[0071] S1: using more than two groups of single screw extruders with a length-to-diameter ratio of 30:1, the prepared materials are respectively sent to the corresponding single screw extruders according to the functional layers, and then filtered through a melt filter, and enter a distributor, a confluence die head, a cooling roller group, a heat setting and recooling device, a transfer and traction device, and a winding device to obtain a polyolefin base film layer 2;

[0072] S2: coating the release agent on the upper side of the polyolefin base film layer 2 by direct transfer or multi-roller transfer, then using hot air circulation drying or light radiation excitation to allow the release agent to react completely, and finally winding up to obtain a polyolefin release film with high dimensional stability.

[0073] Preferably, the processing temperature of the single-screw extruder, the melt filter, the distributor and the confluence die is 225°C.

[0074] Preferably, more than two groups of cooling rollers are arranged in the cooling roller group, the cooling rollers are located below the confluence die and the distance between the cooling rollers and the die lip of the confluence die is within 5 mm, the cooling rollers and the front of the confluence die are provided with a negative pressure adsorption device, the cooling rollers and the rear of the confluence die are provided with a positive pressure air knife device, and the cooling rollers are provided with roller exhaust grooves.

[0075] Preferably, a setting roller group is provided in the heat setting and recooling device, and the setting roller group consists of metal rollers with polished surfaces and a diameter greater than or equal to 500 mm. The number of the metal rollers is more than 5, and the metal rollers include more than 3 heating setting rollers and more than 2 cooling setting rollers.

[0076] Preferably, the heat setting temperature of the heat setting and recooling device is 130°C, and the recooling temperature is 30°C.

[0077] Example 3

[0078] A polyolefin release film with high dimensional stability comprises a release agent layer 1 and a polyolefin base film layer 2, wherein the polyolefin base film layer 2 comprises a release agent adhesive layer 21 and a support layer 22, wherein the release agent layer 1, the release agent adhesive layer 21 and the support layer 22 are connected in sequence, wherein the layer thickness ratio of the release agent adhesive layer 21 to the support layer 22 is 90:10, wherein the release agent adhesive layer 21 comprises a rubber phase-containing block copolymer polypropylene, maleic anhydride-modified polypropylene, a nucleating agent and an adhesion agent in a mass ratio of 85:15:0.1:0.05, and wherein the support layer 22 comprises a homopolymer polypropylene, a toughening agent and a nucleating agent in a mass ratio of 80:15:0.1.

[0079] Preferably, the toughening agent is one or two of EPDM rubber and styrene-butadiene-styrene block copolymer.

[0080] Preferably, the nucleating agent is a polypropylene masterbatch containing one or more of 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, 2,2'-methylene-bis(4,6-di-tert-butylphenyl) sodium phosphate, talc, and calcium carbonate.

[0081] Preferably, the adhesive is a mixed prefabricated masterbatch containing block copolymer polypropylene and siloxane-coated nano-silicon dioxide or macromolecular silicone.

[0082] Preferably, the dynamic friction coefficient of the support layer 22 side is 0.8.

[0083] Preferably, the release agent adhesive layer 21 is provided with a film venting groove, which is a triangular structure, a square structure, a diamond structure, and a trapezoidal structure. The film venting grooves are regularly arranged, and the line width of the film venting grooves is 25 μm, the line height is not more than 10 μm, and the area of ​​a single structural unit is not more than 1 mm 2 .

[0084] Preferably, the strength of the polyolefin-based film layer 2 at a tensile elongation of 10% in an environment of 120° C. is 20 N / 25 mm.

[0085] Preferably, after the polyolefin-based film layer 2 is baked at 150°C for 30 minutes, the thermal shrinkage rate along the directions of 0°, 45°, 90° and 135° is less than or equal to 1%, and the difference in thermal shrinkage rate along 0° and 90° is within plus or minus 0.5%.

[0086] Preferably, the release agent layer 1 contains water-based or photosensitive free radical reactive silicone resin, fluorine-containing modified silicone resin, or fluorine-based release agent.

[0087] As a preference, the method comprises the following steps:

[0088] S1: using more than two groups of single screw extruders with a length-to-diameter ratio of 30:1, the prepared materials are respectively sent to the corresponding single screw extruders according to the functional layers, and then filtered through a melt filter, and enter a distributor, a confluence die head, a cooling roller group, a heat setting and recooling device, a transfer and traction device, and a winding device to obtain a polyolefin base film layer 2;

[0089] S2: coating the release agent on the upper side of the polyolefin base film layer 2 by direct transfer or multi-roller transfer, then using hot air circulation drying or light radiation excitation to allow the release agent to react completely, and finally winding up to obtain a polyolefin release film with high dimensional stability.

[0090] Preferably, the processing temperature of the single-screw extruder, the melt filter, the distributor and the confluence die is 250°C.

[0091] Preferably, more than two groups of cooling rollers are arranged in the cooling roller group, the cooling rollers are located below the confluence die and the distance between the cooling rollers and the die lip of the confluence die is within 5 mm, the cooling rollers and the front of the confluence die are provided with a negative pressure adsorption device, the cooling rollers and the rear of the confluence die are provided with a positive pressure air knife device, and the cooling rollers are provided with roller exhaust grooves.

[0092] Preferably, a setting roller group is provided in the heat setting and recooling device, and the setting roller group consists of metal rollers with polished surfaces and a diameter greater than or equal to 500 mm. The number of the metal rollers is more than 5, and the metal rollers include more than 3 heating setting rollers and more than 2 cooling setting rollers.

[0093] Preferably, the heat setting temperature of the heat setting and recooling device is 160°C, and the recooling temperature is 40°C.

[0094] Example 4

[0095] The polyolefin release films with high dimensional stability and a thickness of 80±2 μm obtained in the above embodiments were taken, and then according to the parameters in Table 1, comparative examples 1 and 2 with a thickness of 80±2 μm were prepared, and then the tensile properties, thermal shrinkage rate and friction coefficient were tested. The test method is as follows:

[0096] 1. Tensile performance test:

[0097] (1) Cut a strip sample with a width of 15 mm and a length of 150 mm.

[0098] (2) Load the sample into the high-temperature tensile testing machine fixture with a gauge length of 100 mm between the upper and lower fixtures. The temperature of the high-temperature box is 120°C and the sample is allowed to stand in the high-temperature box for 5 minutes.

[0099] (3) Test the tensile force and take the tensile strength value when the stretch is 10%.

[0100] 2. Thermal shrinkage test:

[0101] (1) Cut a 100 mm x 100 mm specimen and mark the TD and MD directions.

[0102] (2) Mark the center line and diagonal line along the TD and MD directions, and mark 0° with the center line in the TD direction as the base point, and then mark 45°, 90°, and 135° in a clockwise direction based on this.

[0103] (3) Use a tool with an accuracy of not less than 0.1 mm to measure the length of each line and record the length L1 of each line.

[0104] (4) Place the sample in a 150°C environment for 30 minutes, then take it out and cool it to room temperature.

[0105] (5) Use a measuring tool with an accuracy of not less than 0.1 mm to measure the length of each line after baking and record it as L2.

[0106] (6) Calculate the shrinkage rate according to the formula (L1-L2) / L1*100%.

[0107] 3. Friction coefficient test:

[0108] Refer to the national standard GBT 10006-2021 "Determination of friction coefficient of plastic films and sheets" to test the friction coefficient between the non-release surface and the non-release surface.

[0109] The product information parameters of the polyolefin release films with high dimensional stability obtained in various embodiments of the present invention and comparative example 1 are shown in Table 1, and the performance test parameters are shown in Table 2:

[0110] Table 1

[0111]

[0112] Table 2

[0113]

[0114] In conclusion, the above is only a preferred embodiment of the present invention, and all equivalent changes and modifications made within the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A polyolefin release film with high dimensional stability, comprising a release agent layer (1) and a polyolefin base film layer (2), characterized in that: The polyolefin-based film layer (2) comprises a release agent adhesive layer (21) and a support layer (22); the release agent layer (1), the release agent adhesive layer (21), and the support layer (22) are connected in sequence; the layer thickness ratio of the release agent adhesive layer (21) to the support layer (22) is 80-90:10-20; the release agent adhesive layer (21) is composed of ethylene propylene diene monomer rubber phase block copolymer polypropylene, maleic anhydride modified polypropylene, nucleating agent, and adhesion agent in a mass ratio of 85-95:5-15:0.1-1:0.05-0.5; and the support layer (22) is composed of homopolymer polypropylene, toughening agent, and nucleating agent in a mass ratio of 80-95:1-15:0.1-1; The method for manufacturing the polyolefin release film with high dimensional stability comprises the following steps: S1: using more than two groups of single-screw extruders with a length-to-diameter ratio of 30:1, the prepared materials are respectively sent to the corresponding single-screw extruders according to the functional layers, and then filtered through a melt filter, and enter a distributor, a confluence die head, a cooling roller group, a heat setting and recooling device, a transfer and traction device, and a winding device to obtain a polyolefin base film layer (2); S2: coating a release agent on the upper side of the polyolefin-based film layer (2) by direct transfer or multi-roller transfer, then allowing the release agent to react completely by hot air circulation drying or light radiation excitation, and finally winding up to obtain a polyolefin release film with high dimensional stability.

2. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The toughening agent is one or two of ethylene propylene diene monomer rubber and styrene-butadiene-styrene block copolymer.

3. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The nucleating agent is a polypropylene masterbatch containing one or more of 2,2'-methylene-bis(4,6-di-tert-butylphenyl phosphate) basic aluminum, 2,2'-methylene-bis(4,6-di-tert-butylphenyl) sodium phosphate, talc and calcium carbonate.

4. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The adhesive is a mixed prefabricated masterbatch containing block copolymerized polypropylene, macromolecular silicone or siloxane-coated nano silicon dioxide.

5. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The dynamic friction coefficient of the support layer (22) side is 0.5327-0.6522.

6. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The release agent adhesive layer (21) is provided with a film venting groove, the film venting groove is one of a triangular structure, a square structure, a diamond structure, and a trapezoidal structure, the film venting grooves are regularly arranged, the line width of the film venting grooves is 5 μm to 25 μm, the line height is not greater than 10 μm, and the area of ​​a single structural unit is not greater than 1 mm 2 .

7. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The strength of the polyolefin-based film layer (2) at a tensile elongation of 10% in an environment of 120° C. is 10 N / 25 mm to 20 N / 25 mm.

8. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: After the polyolefin-based film layer (2) is baked at 150°C for 30 minutes, the heat shrinkage rate along the directions of 0°, 45°, 90° and 135° is less than or equal to 1%, and the difference in the heat shrinkage rate along the directions of 0° and 90° is within plus or minus 0.5%.

9. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The release agent layer (1) contains water-based or photosensitive free radical reactive silicone resin, fluorine-containing modified silicone resin, and fluorine release agent.

10. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The processing temperature of the single-screw extruder, the melt filter, the distributor and the confluence die is 200°C to 250°C.

11. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The cooling roller group is provided with more than two groups of cooling rollers, the cooling rollers are located below the confluence die and the distance between the cooling rollers and the die lip of the confluence die is within 5 mm, the front of the cooling rollers and the confluence die is provided with a negative pressure adsorption device, the rear of the cooling rollers and the confluence die is provided with a positive pressure air knife device, and the cooling rollers are provided with roller exhaust grooves.

12. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The heat setting and recooling device is provided with a setting roller group, which is composed of metal rollers with polished surfaces and a diameter greater than or equal to 500 mm. The number of the metal rollers is more than 5, and the metal rollers include more than 3 heating setting rollers and more than 2 cooling setting rollers.

13. The polyolefin release film with high dimensional stability according to claim 1, characterized in that: The heat setting temperature of the heat setting and recooling device is 100°C to 160°C, and the recooling temperature is 20°C to 40°C.