Short-term aging simulation method of SBS modified asphalt considering the characteristics of maintenance engineering

By using a short-term aging simulation method that takes into account the characteristics of maintenance projects, and replacing long-term storage and repeated heating with thin-film oven aging, the characteristics of maintenance projects that were not considered in traditional methods are solved, and reasonable evaluation and quality control of the performance of SBS modified asphalt are achieved.

CN115754257BActive Publication Date: 2024-11-26HOHAI UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211409463.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-11-26
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

Traditional short-term aging methods fail to effectively consider the long-term storage and repeated heating process of SBS modified asphalt in highway maintenance projects, resulting in the degradation of asphalt material performance in maintenance projects and failing to meet the technical requirements for maintenance.

Method used

A short-term aging simulation method that takes into account the characteristics of maintenance projects was adopted. Three asphalt samples were prepared and subjected to routine performance testing, simulated storage aging test and typical working condition test respectively. The matching of the simulation test method was evaluated by combining the aging index formula. Thin film oven aging was used to replace long-term storage and repeated heating process.

Benefits of technology

The aging process of SBS modified asphalt in highway maintenance projects was effectively simulated, its performance was reasonably evaluated, a quality control system for highway maintenance projects was established, and indoor simulation time was saved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115754257B_ABST
    Figure CN115754257B_ABST
Patent Text Reader

Abstract

The present invention discloses a short-term aging simulation method of SBS modified asphalt considering the characteristics of maintenance engineering, including: preparing asphalt samples and dividing them into equal parts to obtain a first sample, a second sample, and a third sample; constructing an aging index index, testing based on the first sample, and obtaining the original performance index of the asphalt binder; performing a storage aging test of SBS modified asphalt for simulating maintenance engineering based on the second sample, and testing to obtain the simulated performance index of the asphalt binder; performing indoor simulation of the typical working conditions after the SBS modified asphalt enters the site based on the third sample, and testing to obtain the actual performance index of the asphalt binder; and evaluating the matching of the short-term aging simulation test method with the actual situation according to the simulated performance index and the actual performance index. The present invention can effectively simulate the asphalt aging process in an all-round way from asphalt raw materials, production process, storage process and construction process, and lays a foundation for establishing a quality control system for highway maintenance engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of traffic engineering, and in particular relates to a short-term aging simulation method of SBS modified asphalt taking into account the characteristics of maintenance engineering. Background Art

[0002] Asphalt pavement has significant advantages such as good flatness, low noise, and easy maintenance. It has become the main pavement structure used in highway construction. At present, the service life of some pavement structures exceeds 10 years, and some have even exceeded 15 years, entering an important stage of maintenance and repair. SBS modified asphalt is commonly used in the upper and middle layers of asphalt materials used in asphalt pavements of highways. During the use of asphalt pavements, with the repeated combined effects of traffic loads and natural environmental factors, its performance gradually declines, the surface anti-skid performance and driving quality decrease, and various diseases such as oil spilling, rutting, congestion, and looseness appear. For this reason, the maintenance of asphalt pavements on highways is becoming increasingly important, and the technical requirements for SBS modified asphalt used for maintenance are higher.

[0003] There are great differences between highway maintenance projects and new construction projects. The characteristics of maintenance projects are mainly as follows: long-term storage and repeated heating of asphalt after entering the site. The heating temperature of modified asphalt during the construction stage is usually between 160 and 165°C; the construction interval is generally not less than 150°C; the longest high-temperature storage time of a single tank of asphalt is 10-15 days; under normal circumstances, the number of repeated heating times of a single tank of asphalt is 3 to 5 times, and the maximum is 8 times. Secondly, the maintenance mixing volume is small, the construction is scattered, and the transportation distance is long. The transportation distance of general maintenance projects is within 50 to 60 km, and the transportation time is within 2 hours. The farthest point can reach 200 km, and the transportation time in the middle is 5 to 6 hours. In order to ensure that the mixture has sufficient temperature during the construction of the maintenance section, the production temperature of the asphalt mixture at the mixing station is usually high. Conventional short-term aging tests do not take into account the aging caused by the long-term storage and repeated heating of asphalt caused by the characteristics of maintenance projects.

[0004] The traditional short-term aging method mainly considers the aging of asphalt during mixing, paving and rolling, and is suitable for asphalt materials used in new construction projects. However, SBS modified asphalt used in maintenance projects needs to be stored for a long time and heated repeatedly after entering the site, and the construction is scattered and the transportation distance is relatively long. In view of the characteristics of highway maintenance projects, the traditional short-term aging method does not take the characteristics of maintenance projects into account, and adding aging time on the basis of the original short-term aging does not take the characteristics of maintenance projects into account. Summary of the invention

[0005] To solve the above problems, the present invention provides the following solution: a short-term aging simulation method of SBS modified asphalt considering the characteristics of maintenance engineering, comprising:

[0006] preparing an asphalt sample and dividing it into equal parts to obtain a first sample, a second sample, and a third sample;

[0007] Constructing an aging index indicator, and testing the first sample to obtain an original performance index of the asphalt binder;

[0008] After performing a storage aging test of SBS modified asphalt for a simulated maintenance project based on the second sample, the simulated performance index of the asphalt binder is obtained by testing;

[0009] Based on the third sample, a typical working condition of SBS modified asphalt after entering the site is simulated indoors to obtain the actual performance index of the asphalt binder;

[0010] The matching of the short-term aging simulation test method with the actual situation is evaluated based on the simulated performance index and the actual performance index.

[0011] Preferably, the aging index indicators include softening point, ductility at 5°C, viscosity at 135°C, irreversible creep compliance Jnr3.2, zero shear viscosity at 60°C, and segregation.

[0012] Preferably, the process of testing the first sample to obtain the original performance index of the asphalt binder includes:

[0013] Based on the first sample, conventional performance testing is carried out according to the method specified in the test procedures for asphalt and asphalt mixtures in highway engineering, and the test index results of the aged sample are obtained in accordance with the provisions of the specifications for asphalt and asphalt mixtures.

[0014] Preferably, after performing a storage aging test of SBS modified asphalt for a simulated maintenance project based on the second sample, the process of testing and obtaining the simulated performance index of the asphalt binder includes:

[0015] The second sample was placed in a film oven preheated to 163°C, and after aging for 5h20min, the sample was poured out and tested to obtain simulated performance indicators of the asphalt binder.

[0016] Preferably, the process of placing the second sample in a film oven preheated to 163° C. and pouring out the sample after aging for 5 hours and 20 minutes comprises:

[0017] Adjust the oven to a level where the turntable rotates at a speed of 5.5r / min±1r / min on the horizontal plane, with the inclination angle of the turntable to the horizontal plane not greater than 3°. Set the thermometer to be equidistant from the center and edge of the turntable. After the oven reaches a constant temperature of 163°C, quickly place the sample dish containing the second sample on the turntable in the oven, close the oven door and start the turntable rack. Start timing when the temperature in the oven returns to 162°C, and maintain it at 163°C±1°C for 5h20min.

[0018] Preferably, the process of conducting indoor simulation of typical working conditions of SBS modified asphalt after entering the site based on the third sample and testing to obtain actual performance indicators of the asphalt binder includes:

[0019] Based on the third sample, indoor simulation of typical working conditions of constant temperature storage and cyclic heating of SBS modified asphalt after entering the site was carried out. After simulating the typical working conditions, the third sample was aged in a thin film oven for 5 hours, and the sample was poured out for testing to obtain the actual performance indicators of the asphalt binder.

[0020] Preferably, the simulation conditions of the typical working condition of constant temperature storage are: storage at 60°C for 3 days, storage at 180°C for 1 day, and cyclic heating at 160°C for 5 hours + 150°C for 19 hours for 2 times;

[0021] The simulation conditions of the typical cyclic heating working condition are: cyclic heating at 160°C for 5h + 130°C for 19h + 5d, cyclic heating once.

[0022] Preferably, the process of evaluating the matching of the short-term aging simulation test method with the actual situation according to the simulation performance index and the actual performance index includes:

[0023] By substituting the test values ​​of the performance indicators into the aging index formula, the aging index of the second sample and the aging index of the third sample are calculated; based on the aging index of the second sample and the aging index of the third sample, the test method of short-term aging simulation is evaluated.

[0024] Preferably, the aging index formula is expressed as:

[0025]

[0026] Among them, Y(J nr3.2 ) is the irrecoverable creep compliance of the original asphalt; T(J nr3.2 ) is the irrecoverable creep compliance after aging.

[0027] The present invention discloses the following technical effects:

[0028] The present invention provides a short-term aging simulation method for SBS modified asphalt that takes into account the characteristics of maintenance projects. Starting from the characteristics of maintenance projects, the present invention combines scientific research and the convenience of engineering application to determine a short-term aging simulation test method based on the characteristics of maintenance projects. It effectively simulates the asphalt aging process from all aspects of asphalt raw materials, production process, storage process and construction process, laying the foundation for establishing a quality control system for highway maintenance projects. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 The figure is a flow chart of a method according to an embodiment of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0033] like Figure 1 As shown, the present invention provides a short-term aging simulation method for SBS modified asphalt taking into account the characteristics of maintenance engineering, comprising the following steps:

[0034] Firstly, three identical asphalt samples A, B and C were prepared. Sample A was used to test the performance indicators of the original asphalt binder. Sample B was placed in a thin film oven preheated to 163°C, aged for 5h20min and then the sample was poured out to test the performance indicators of the asphalt binder. Sample C was stored at a constant temperature and repeatedly heated to simulate typical working conditions. After simulating the typical working conditions, the sample was aged in a thin film oven for 5h, and the performance indicators of the asphalt binder were poured out to test. Finally, an aging index (AI) was proposed, based on which the matching of the short-term aging simulation test method with the actual situation was evaluated.

[0035] Further optimization plan, the first step: Sample A is tested for routine performance according to the method specified in the test procedures for asphalt and asphalt mixtures of highway engineering, and the aging sample test indicators are taken out according to the specifications for asphalt and asphalt mixtures, including softening point, 5℃ elongation, 135℃ viscosity, irreversible creep compliance Jnr3.2, 60℃ zero shear viscosity, and segregation;

[0036] Step 2: Sample B is subjected to a storage aging test of SBS modified asphalt used in a simulated maintenance project, specifically: adjust the oven to a level so that the turntable rotates at a speed of 5.5r / min±1r / min on the horizontal plane, the turntable is tilted at an angle of no more than 3° to the horizontal plane, and the thermometer is at an equal distance from the center and edge of the turntable. After the oven reaches a constant temperature of 163°C, quickly place the sample dish containing the sample on the turntable in the oven, close the oven door and start the turntable rack; start timing when the oven temperature returns to 162°C, and maintain it at 163°C±1°C for 5h20min.

[0037] Step 3: Take out the aged samples and test the indicators according to the specifications of asphalt and asphalt mixture, including softening point, ductility at 5℃, viscosity at 135℃, irreversible creep compliance Jnr3.2, zero shear viscosity at 60℃, and segregation. The test results are shown in Table 1.

[0038] Step 4: Sample C was subjected to indoor simulation of typical storage conditions of SBS modified asphalt after it was delivered to the site: storage at a constant temperature of 160°C for 3 days, storage at a constant temperature of 180°C for 1 day, cyclic heating at 160°C for 5h + 150°C for 19h for 2 times, and cyclic heating at 160°C for 5h + 130°C for 19h + 5d for 1 time. Through a large number of experiments, the typical storage conditions and extreme storage times of the maintenance project were obtained as shown in Table 1 below.

[0039] Table 1

[0040]

[0041] Step 5: Perform a film oven aging test on the SBS modified asphalt samples after long-term storage, with an aging time of 5 hours;

[0042] Step 6: Take out the samples after aging in the fifth step and test the performance indicators, including softening point, ductility at 5°C, viscosity at 135°C, irreversible creep compliance Jnr3.2, zero shear viscosity at 60°C, and segregation. The test results are shown in Table 2.

[0043] Table 2

[0044]

[0045] As can be seen from Table 2, the changes in the various indicators of SBS modified asphalt after entering the site under the typical working conditions of constant temperature storage and cyclic heating first pass through the storage for the maximum time, and then undergo aging in the film oven for 5 hours, and the attenuation degree of various indicators after aging in the film oven for 5 hours and 20 minutes is the same. Therefore, the film oven aging for 5 hours and 20 minutes can be used to replace the short-term aging of SBS modified asphalt after long-term storage and cyclic heating, followed by mixing, paving, and rolling.

[0046] Step 7: Substitute the test value into the aging index formula;

[0047] The aging index is defined as: Where: Y(J nr3.2 ) is the irrecoverable creep compliance of the original asphalt; T(J nr3.2 ) is the irrecoverable creep compliance after aging;

[0048] The aging index of sample B in the short-term aging simulation test method based on the characteristics of the maintenance project is 0.123, which is basically consistent with the aging index results of 0.129, 0.135, 0.124, and 0.121 under different working conditions. Therefore, the proposed SBS modified asphalt short-term aging simulation test method considering the characteristics of the maintenance project is consistent with the aging degree of the construction site.

[0049] The present application discloses a short-term aging simulation test method for SBS modified asphalt which takes into account the characteristics of maintenance projects. The thin film oven aging (TFOT5h20min) is used to replace the traditional thin film oven aging. The characteristics of long-term storage and repeated heating of SBS modified asphalt used in maintenance projects are taken into account, thus saving the time for indoor simulation of long-term storage.

[0050] The present application discloses a short-term aging simulation test method for SBS modified asphalt that takes into account the characteristics of maintenance projects, which overcomes the shortcomings of traditional short-term aging methods. Traditional short-term aging methods mainly take into account the aging of asphalt during mixing, paving, and rolling, and are suitable for asphalt materials used in new construction projects. However, SBS modified asphalt used in maintenance projects needs to be stored for a long time and heated repeatedly after entering the site, and the construction is scattered and the transportation distance is relatively long. In view of the characteristics of highway maintenance projects, the characteristics of maintenance projects are not taken into account in traditional short-term aging methods, and the characteristics of maintenance projects are not taken into account when the aging time is increased on the basis of the original short-term aging. Starting from the characteristics of maintenance projects, this embodiment determines a short-term aging simulation test method based on the characteristics of maintenance projects in combination with the convenience of scientific research and engineering application. It can more reasonably judge the performance of SBS modified asphalt used in maintenance projects, and effectively simulates the asphalt aging process from the perspectives of asphalt raw materials, production process, storage process, and construction process, laying the foundation for establishing a quality control system for highway maintenance projects.

[0051] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for simulating short-term aging of SBS modified asphalt taking into account the characteristics of maintenance engineering, characterized in that: include: preparing an asphalt sample and dividing it into equal parts to obtain a first sample, a second sample, and a third sample; Constructing an aging index indicator, and testing the first sample to obtain an original performance index of the asphalt binder; After performing a storage aging test of SBS modified asphalt for a simulated maintenance project based on the second sample, the simulated performance index of the asphalt binder is obtained by testing; Based on the third sample, a typical working condition of SBS modified asphalt after entering the site is simulated indoors to obtain the actual performance index of the asphalt binder; Evaluate the compatibility of the short-term aging simulation test method with the actual situation according to the simulated performance index and the actual performance index; The process of obtaining the original performance index of the asphalt binder by testing the first sample includes: Based on the first sample, conventional performance testing is performed according to the method specified in the test procedures for asphalt and asphalt mixtures in highway engineering, and the test index results of the aged sample are obtained according to the provisions of the specification procedures for asphalt and asphalt mixtures; After the SBS modified asphalt storage aging test for the simulated maintenance project is carried out based on the second sample, the process of testing and obtaining the simulated performance index of the asphalt binder includes: The second sample was placed in a film oven preheated to 163°C, aged for 5h20min, and then poured out to obtain the simulated performance index of the asphalt binder; Based on the third sample, the typical working condition of SBS modified asphalt after entering the site is simulated indoors, and the process of testing and obtaining the actual performance index of the asphalt binder includes: Based on the third sample, an indoor simulation of a typical working condition of constant temperature storage and a typical working condition of cyclic heating after the SBS modified asphalt is brought into the site is performed, and the third sample after the typical working condition is simulated is aged in a thin film oven for 5 hours, and the sample is poured out for testing to obtain the actual performance index of the asphalt binder; The process of evaluating the matching of the short-term aging simulation test method with the actual situation according to the simulation performance index and the actual performance index includes: By substituting the test value of the performance index into the aging index formula, the aging index of the second sample and the aging index of the third sample are calculated; evaluating a test method for short-term aging simulation based on the aging index of the second sample and the aging index of the third sample; The expression of the aging index formula is: in, is the irrecoverable creep compliance of the original asphalt; It is the irrecoverable creep compliance after aging.

2. The SBS modified asphalt short-term aging simulation method considering the characteristics of the maintenance project according to claim 1 is characterized in that: The aging index indicators include softening point, 5°C elongation, 135°C viscosity, irreversible creep compliance Jnr3.2, 60°C zero shear viscosity, and segregation.

3. The SBS modified asphalt short-term aging simulation method considering the characteristics of the maintenance project according to claim 1 is characterized in that: The process of placing the second sample in a film oven preheated to 163°C and pouring out the sample after aging for 5h20min includes: Adjust the oven to a level where the turntable rotates at a speed of 5.5r / min±1r / min on the horizontal plane, with the inclination angle of the turntable to the horizontal plane not greater than 3°. Set the thermometer to be equidistant from the center and edge of the turntable. After the oven reaches a constant temperature of 163°C, quickly place the sample dish containing the second sample on the turntable in the oven, close the oven door and start the turntable rack. Start timing when the temperature in the oven returns to 162°C, and maintain it at 163°C±1°C for 5h20min.

4. The SBS modified asphalt short-term aging simulation method considering the characteristics of the maintenance project according to claim 1 is characterized in that: The simulation conditions of the typical constant temperature storage condition are: storage at 60°C for 3 days, storage at 180°C for 1 day, and cycle heating at 160°C for 5 hours + 150°C for 19 hours for 2 times; The simulation conditions of the typical cyclic heating working condition are: cyclic heating at 160°C for 5h + 130°C for 19h + 5d, cyclic heating once.