A method for beneficiating copper-molybdenum ores containing different ore grades
By adopting dual-system grinding and flotation technology in copper-molybdenum ore beneficiation to process high- and low-grade ores respectively, the problem of fluctuating ore supply grade and unstable beneficiation indicators has been solved, and the recovery rate and beneficiation efficiency of copper and molybdenum have been improved.
Patent Information
- Application Number
- CN202211557348.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Due to the limited mining ore blending conditions, the ore supply grade fluctuates greatly in copper-molybdenum ore beneficiation production, and the copper-molybdenum ore beneficiation index cannot be stabilized, resulting in low recovery rates and high loss rates of copper and molybdenum.
Two ore supply and storage systems are used to store high-grade and low-grade ores respectively. Dual-system grinding and flotation technology are used. High-grade ores are ground once and low-grade ores are ground twice. Through the high-grade flotation system and the low-grade flotation system, Carry out multiple roughing, sweeping and concentrating operations respectively, and finally mix the concentrates obtained by the dual system flotation for copper and molybdenum separation flotation.
It effectively reduces the impact of supply grade fluctuations and ore property differences, improves the recovery rate of copper and molybdenum, reduces the loss rate, and achieves more stable mineral processing indicators.
Smart Images

Figure CN115780068B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper-molybdenum ore dressing, and in particular to a method for dressing copper-molybdenum ores containing different ore grades. Background Art
[0002] Copper-molybdenum ore is one of the main sources of molybdenum concentrate. The copper-molybdenum deposits currently used for molybdenum mining have a minimum copper grade of 0.2-0.3% and a minimum molybdenum grade of 0.01-0.011%. Due to the limitations of mineral processing technology, the removal of intercalated stones or stripping of surrounding rocks in mining sites with lower copper grades can only be discarded as waste slag. In order to increase the ore mining rate, the recovery and utilization of low-grade copper-molybdenum ores can be improved by mixed flotation and separation.
[0003] In actual ore mining, there are many and diverse ore supply points, and the properties of ore are complex and changeable. In mining, the copper grade is about 0.2-0.3%, and the molybdenum grade is about 0.01% in the removal of interlayer stones, stripping of surrounding rocks near the mine and by-product ore; while in the main ore, the copper grade is about 0.4%-0.8%, and the molybdenum grade is about 0.02%. Due to the limited mining and ore matching conditions, it is difficult to achieve ore supply balance, resulting in large fluctuations in the ore supply grade in actual ore dressing production; affected by the fluctuation of ore supply grade and the different properties of ores at different mining points, the flotation foam concentration, concentrate yield and other factors change rapidly, and the controllability of the ore dressing process is reduced, resulting in the inability to stabilize the ore dressing indicators as a whole, increasing the difficulty of ore dressing.
[0004] Therefore, how to reduce the fluctuation of ore grade and stabilize the beneficiation index of copper-molybdenum ore so as to be suitable for beneficiation of copper-molybdenum ores with different ore grades at the same time is an urgent problem to be solved. Summary of the invention
[0005] The technical problems to be solved by the present invention are:
[0006] At present, due to the limited mining and ore matching conditions, it is difficult to achieve balanced ore supply, resulting in large fluctuations in the ore grade in actual mineral processing production, and the inability to stabilize the copper-molybdenum ore processing indicators, which ultimately leads to low copper and molybdenum recovery rates and high loss rates during copper-molybdenum ore processing.
[0007] The technical solution adopted by the present invention is:
[0008] The present invention provides a method for beneficiating copper-molybdenum ores containing different ore grades, comprising the following steps:
[0009] S1 stores the ore in high-grade storage system and low-grade storage system according to the grade of the ore;
[0010] The high-grade ore in the S2 high-grade storage system is sent to the high-grade flotation system after one grinding; the low-grade ore in the low-grade storage system is sent to the low-grade flotation system after multiple grindings;
[0011] S3.1 High-grade ore is subjected to multiple roughing and scavenging operations in the high-grade flotation system to obtain high-grade rough concentrate and scavenging tailings; the high-grade rough concentrate is taken and passed into the hydrocyclone for classification and re-grinding, and the overflow of the hydrocyclone is subjected to multiple centralized concentrating operations to obtain high-grade copper-molybdenum concentrate; the scavenging tailings are taken and subjected to multiple centralized intensive scavenging operations;
[0012] S3.2 Low-grade ore is subjected to multiple roughing and scavenging in the low-grade flotation system to obtain low-grade rough concentrate and flotation tailings. The low-grade rough concentrate is taken and passed through the hydrocyclone for classification and re-grinding. The low-grade rough concentrate overflowing from the hydrocyclone is subjected to multiple centralized selection to obtain low-grade copper-molybdenum concentrate and tailings. The tailings are returned to the multiple roughing for re-operation.
[0013] S4 mixes the high-grade copper-molybdenum concentrate in S3.1 and the low-grade copper-molybdenum concentrate in S3.2 to separate copper and molybdenum by flotation, including the following steps:
[0014] The mixed copper-molybdenum concentrate is subjected to roughing selection and multiple scavenging selections in sequence, and the obtained mixed rough concentrate is classified by a cyclone and then ground again. The mixed rough concentrate overflowing from the cyclone is subjected to multiple molybdenum selections to obtain a molybdenum concentrate.
[0015] Preferably, in the high-grade flotation system, high-grade flotation reagents are added in the roughing and / or scavenging processes, and the high-grade flotation reagents include one or more of butyl xanthate and diesel, and a frother.
[0016] Preferably, in the low-grade flotation system, low-grade flotation reagents are added during the roughing and / or scavenging process, and the low-grade flotation reagents include butyl xanthate, copper-molybdenum collector, frother and / or diesel.
[0017] Preferably, in the copper-molybdenum separation flotation, a separation flotation reagent is added in the roughing and / or scavenging and / or concentrating process, and the separation flotation reagent includes sodium sulfide or a sodium sulfide-depressant mixture.
[0018] Preferably, in the high-grade flotation system, the fineness of the high-grade ore entering the flotation system is controlled to be 45-55%, and the fineness of the high-grade copper-molybdenum concentrate obtained is 80-90% of -0.074mm; in the low-grade flotation system, the fineness of the low-grade ore entering the flotation system is controlled to be greater than 60-70%, and the fineness of the low-grade copper-molybdenum concentrate obtained is 92-98% of -0.074mm.
[0019] The beneficial effects of the present invention are as follows:
[0020] The present invention adopts two ore supply and storage systems to store two ores of different grades, respectively; dual-system grinding is used, wherein the high-grade ore is ground once and the low-grade ore is ground twice; the grinding products enter the subsequent flotation operation, and the dual-system flotation operation is used, wherein the high-grade flotation system is used to select high-grade ores with a grade of about 0.5%-0.8%, and the low-grade flotation system is used to select low-grade ores with a grade of about 0.2%-0.4%; finally, the copper-molybdenum concentrates obtained by the dual-system flotation operation are mixed, and then copper-molybdenum separation flotation is carried out, which is suitable for mining operations in mining areas where mining conditions are limited and balanced ore supply cannot be achieved, reduces the influence of fluctuations in ore supply grade and different ore properties at different mining points, and finally can obtain molybdenum concentrate and copper concentrate with higher recovery rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the flow chart of the high-grade flotation system and the low-grade flotation system in Example 1;
[0022] Figure 2 Schematic diagram of the process of the copper-molybdenum flotation system in Example 1. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0024] The present invention provides a method for beneficiating copper-molybdenum ores containing different ore grades, comprising the following steps:
[0025] S1 stores the ore in high-grade storage system and low-grade storage system according to the grade of the ore;
[0026] The high-grade ore in the S2 high-grade storage system is sent to the high-grade flotation system after one grinding; the low-grade ore in the low-grade storage system is sent to the low-grade flotation system after multiple grindings;
[0027] S3.1 High-grade ore is subjected to multiple roughing and scavenging operations in the high-grade flotation system to obtain high-grade rough concentrate and scavenging tailings; the high-grade rough concentrate is taken and passed into the hydrocyclone for classification and re-grinding, and the overflow of the hydrocyclone is subjected to multiple centralized concentrating operations to obtain high-grade copper-molybdenum concentrate; the scavenging tailings are taken and subjected to multiple centralized intensive scavenging operations;
[0028] S3.2 Low-grade ore is subjected to multiple roughing and scavenging in the low-grade flotation system to obtain low-grade rough concentrate and flotation tailings. The low-grade rough concentrate is taken and passed through the hydrocyclone for classification and re-grinding. The low-grade rough concentrate overflowing from the hydrocyclone is subjected to multiple centralized selection to obtain low-grade copper-molybdenum concentrate and tailings. The tailings are returned to the multiple roughing for re-operation.
[0029] S4 mixes the high-grade copper-molybdenum concentrate in S3.1 and the low-grade copper-molybdenum concentrate in S3.2 to separate copper and molybdenum by flotation, including the following steps:
[0030] The mixed copper-molybdenum concentrate is subjected to roughing selection and multiple scavenging selections in sequence, and the obtained mixed rough concentrate is classified by a cyclone and then ground again. The mixed rough concentrate overflowing from the cyclone is subjected to multiple molybdenum selections to obtain a molybdenum concentrate.
[0031] In the high-grade flotation system, high-grade flotation reagents are added in the roughing and / or scavenging process, and the high-grade flotation reagents include one or more of butyl xanthate and diesel, and a frother. In the low-grade flotation system, low-grade flotation reagents are added in the roughing and / or scavenging process, and the low-grade flotation reagents include butyl xanthate, copper-molybdenum collectors, frothers and / or diesel. In the copper-molybdenum separation flotation, separation flotation reagents are added in the roughing and / or scavenging and / or concentrating process, and the separation flotation reagents include sodium sulfide or a sodium sulfide-depressant mixture.
[0032] In the present invention, according to the ore supply ratio and grade change, two ore supply storage systems are used to store two ores of different high and low grades respectively, and dual-system grinding is used, wherein the high-grade ore is ground once and the low-grade ore is ground twice, and the grinding product enters the subsequent flotation operation, and the dual-system flotation technology is used, wherein the high-grade flotation system is used to select high-grade ores with a grade of about 0.5%-0.8%, and the low-grade flotation system is used to select low-grade ores with a grade of about 0.2%-0.4%. In the high-grade flotation system, the fineness of the high-grade ore supply is controlled to be 45-55%, and the fineness of the high-grade copper-molybdenum concentrate obtained is 80-90% of -0.074mm; in the low-grade flotation system, the fineness of the low-grade ore supply is controlled to be greater than 60-70%, and the fineness of the low-grade copper-molybdenum concentrate obtained is 92-98%.
[0033] Example 1
[0034] In this embodiment, the high-grade ore is stored in the high-grade storage system and the low-grade ore is stored in the low-grade storage system; the high-grade ore is sent to the high-grade flotation system after only one grinding, and the low-grade ore is sent to the low-grade flotation system after two grindings; the high-grade copper-molybdenum concentrate after flotation operation is then mixed with the low-grade copper-molybdenum concentrate, and copper-molybdenum separation flotation is carried out to obtain molybdenum concentrate and copper concentrate respectively.
[0035] High-grade flotation system: The incoming ore pulp undergoes two roughing operations and one scavenging operation to obtain coarse concentrate and scavenging tailings. The scavenging tailings enter the centralized enhanced scavenging operation, including three scavenging operations of scavenging I, scavenging II and scavenging III. The coarse concentrate is graded by the hydrocyclone and then ground again. The overflow of the cyclone enters the centralized concentrating operation, including three concentrating operations of concentrating I, concentrating II and concentrating III and one fine scavenging operation to concentrate the coarse concentrate.
[0036] Low-grade flotation system: The incoming ore pulp undergoes three roughing and three scavenging processes to obtain coarse concentrate and flotation tailings. The coarse concentrate is graded by a hydrocyclone and then ground again. The overflow from the hydrocyclone enters the centralized concentration process, which includes three concentrations of concentration I, II and III and one scavenging process to obtain low-grade copper-molybdenum concentrate and tailings. The tailings are returned to the roughing process for further selection.
[0037] Copper-molybdenum mixed concentrate is obtained through three centralized concentrations, and the copper-molybdenum mixed concentrate is then subjected to centralized copper-molybdenum separation flotation: one roughing selection and two scavenging selections are adopted, and the rough concentrate is graded by a hydrocyclone and then ground again, and the overflow of the cyclone enters the molybdenum concentration operation, including seven concentrations of concentration I, II, III, IV, V, VI, and VII, to obtain molybdenum concentrate and copper concentrate respectively.
[0038] The specific grinding fineness and selected concentration control are as follows:
[0039]
[0040]
[0041] Since the overall embedded particle size of high-grade ore is coarse, better dissociation can be obtained under the condition that the content of selected fineness -0.074mm accounts for 50%. At the same time, the rough concentrate obtained after flotation of high-grade ore can effectively reduce fine-grained mudding under the condition that the content of rough concentrate fineness -0.074mm accounts for 85%; the overall embedded particle size of low-grade ore is fine, and better dissociation can be obtained under the conditions that the content of selected fineness -0.074mm accounts for 65% and the content of rough concentrate fineness -0.074mm accounts for 95%. Copper and molybdenum are closely connected in the copper-molybdenum mixed concentrate, and better dissociation can be obtained under the conditions that the content of selected fineness -0.074mm accounts for 90% and the content of rough concentrate fineness -0.038mm accounts for 90%. It has been proved through repeated experiments that the process adopts three selective grinding to obtain better mineral processing indicators.
[0042] Due to the special characteristics of large fluctuations in the grade of the raw ore, the distribution particle size characteristics and mineral composition of high-grade and low-grade ores are quite different. In order to strengthen the recovery of copper-molybdenum metal minerals, flotation agents are used in the flotation system. The details are as follows:
[0043] In the high-grade flotation system, the high-grade flotation reagent uses a combination of butyl xanthate and 0# diesel as a collector. The butyl xanthate is added by adding a 5% solution prepared by production return water. The production return water is weakly alkaline (PH value is 8). The production return water contains some residual reagents, which can react with some copper-molybdenum minerals with good floatability to reduce the unit consumption of reagents; 0# diesel is added by stock solution; FRT-3 is used as a frother, and the high-grade flotation reagent is beneficial to improve the flotation rate of copper-molybdenum minerals, thereby achieving the purpose of rapid flotation, as follows:
[0044] Table 1 High-grade flotation system
[0045]
[0046] In the low-grade flotation system, the low-grade flotation reagents are butyl xanthate, No. 0 diesel and BK916 (copper-molybdenum collector) as collectors. Butyl xanthate is added by adding a 10% solution prepared by production return water. The production return water is weakly alkaline (PH value is 8). The production return water contains some residual reagents, which can react with some copper-molybdenum minerals with good floatability to reduce the unit consumption of reagents; BK916 is added by stock solution, has strong collection, and has strong collection ability for fine-grained minerals and conjoined minerals; No. 0 diesel is added by stock solution, and the frother is FRT-3 frother. Low-grade flotation reagents are beneficial to improve the recovery of fine-grained low-grade copper-molybdenum ores, as follows:
[0047] Table 2 Low-grade flotation system
[0048]
[0049]
[0050] In the flotation of copper and molybdenum, sodium sulfide and a depressant are used as a depressant. Sodium sulfide is added to a concentration of about 3% with living water, and D106 is added to a concentration of about 10% with living water to suppress copper and float molybdenum. Sodium sulfide and D106 are adsorbed on the surface of copper minerals to further improve the hydrophilicity of copper minerals, thereby achieving better copper and molybdenum separation effects, as follows:
[0051] Table 3 Mixed copper-molybdenum flotation system
[0052]
[0053]
[0054] Comparative Example 1
[0055] The ore obtained from mining is stored in a centralized manner, and then subjected to one grinding, two roughing, two scavenging and concentrating operations in sequence, and then subjected to copper-molybdenum separation and flotation to obtain molybdenum concentrate and copper concentrate. Among them, the reagent used in the copper-molybdenum separation and flotation process only contains sodium sulfide, and the foaming agent in the added reagent is pine oil; technicians in this field can appropriately increase or decrease the number of grinding and the like according to the ore supply ratio and grade.
[0056] Test example
[0057] The ore dressing test was carried out using Example 1 and Comparative Example 1 respectively, and the recovery rate and loss rate of copper and molybdenum elements were measured. The results are as follows:
[0058]
[0059]
[0060] By analyzing the test results in the test example, it can be concluded that:
[0061] In Example 1, two ore supply and storage systems are provided to store ores of different grades, respectively, so as to create conditions for separate flotation.
[0062] Specifically, for high-grade ores, since the particle size of metal minerals is relatively coarse and there are many powder ores after crushing, the materials stored in the ore supply bin are relatively fine, and the conditions of -0.074mm content accounting for 50% can meet the selection requirements by using one grinding. For low-grade ores, since the particle size of metal minerals is relatively fine and there are many coarse particles after crushing, it is necessary to use two grindings to reach -0.074mm content accounting for 65% to obtain a better selection effect. Combined with the properties of the ore, a double grinding system is set up to truly meet the requirements of selective grinding and effectively avoid over-grinding or under-grinding of the ore.
[0063] The dual flotation system of separate flotation of high-grade and low-grade ores, centralized intensive scavenging and selection, and centralized copper-molybdenum separation flotation effectively solved the problems of large fluctuations in ore grade, unbalanced actual production operations, unsatisfactory recovery of intergrowth minerals, and low copper-molybdenum recovery rates. The copper recovery rate increased from 91.84% to 92.71%. The loss rate of molybdenum in tailings was also reduced from 14.82% to 12.25%.
[0064] The dual flotation system of separate flotation of high-grade and low-grade ores, centralized intensified scavenging and selection, centralized concentration, and centralized copper-molybdenum separation flotation solves the problem of low molybdenum grade in mixed concentrate and poor subsequent separation flotation effect after single selection of low-grade ore. The mixed concentrate obtained by the low-grade flotation system and the high-grade flotation system is used for centralized copper-molybdenum separation flotation, which further improves the molybdenum grade of the mixed concentrate and creates favorable conditions for subsequent copper-molybdenum separation flotation. After application, the copper-molybdenum separation effect is significantly improved, and the loss rate of molybdenum in copper concentrate is reduced from 12.55% to 9.37%.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for beneficiating copper-molybdenum ores containing different ore grades, characterized in that: The steps include: S1 stores the ore in high-grade storage system and low-grade storage system according to the grade of the ore; S2 The high-grade ore in the high-grade storage system is ground once, and the fineness of the high-grade ore is controlled to -0.074mm and the content is 45-55%, and then it is sent to the high-grade flotation system; the low-grade ore in the low-grade storage system is ground multiple times, and the fineness of the low-grade ore is controlled to -0.074mm and the content is 65%, and then it is sent to the low-grade flotation system; S3.1 High-grade ore is subjected to multiple roughing and scavenging operations in the high-grade flotation system to obtain high-grade rough concentrate and scavenging tailings; the high-grade rough concentrate is taken and passed through a hydrocyclone for classification and re-grinding, and the overflow of the hydrocyclone is subjected to multiple centralized concentration operations to obtain high-grade copper-molybdenum concentrate; the scavenging tailings are taken and subjected to multiple centralized intensified scavenging operations; S3.2 Low-grade ore is subjected to multiple roughing and scavenging in the low-grade flotation system to obtain low-grade rough concentrate and flotation tailings. The low-grade rough concentrate is taken and passed through the hydrocyclone for classification and re-grinding. The low-grade rough concentrate overflowing from the hydrocyclone is subjected to multiple centralized selection to obtain low-grade copper-molybdenum concentrate and tailings. The tailings are returned to the multiple roughing for re-operation. S4: Mix the high-grade copper-molybdenum concentrate in S3.1 and the low-grade copper-molybdenum concentrate in S3.2, and perform copper-molybdenum separation and flotation to obtain molybdenum concentrate.
2. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 1, characterized in that: In step S4, the copper-molybdenum separation flotation comprises the following steps: The mixed copper-molybdenum concentrate is subjected to roughing selection and multiple scavenging selections in sequence, and the obtained mixed rough concentrate is classified by a cyclone and then ground again. The mixed rough concentrate overflowing from the cyclone is subjected to multiple molybdenum selections to obtain a molybdenum concentrate.
3. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 1, characterized in that: In the high-grade flotation system, high-grade flotation reagents are added during the roughing and / or scavenging process.
4. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 3 is characterized in that: The high-grade flotation reagent comprises one or more of butyl xanthate and diesel, and a frother.
5. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 1, characterized in that: In the low-grade flotation system, low-grade flotation reagents are added during the roughing and / or scavenging process.
6. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 5, characterized in that: Low-grade flotation reagents include butyl xanthate, copper-molybdenum collectors, frothers and / or diesel.
7. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 2, characterized in that: In the copper-molybdenum separation flotation, separation flotation reagents are added in the roughing and / or scavenging and / or cleaning processes.
8. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 7, characterized in that: Separation flotation reagents include sodium sulfide.
9. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 7, characterized in that: The separation flotation reagent includes a sodium sulfide-depressant mixture.
10. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 1, characterized in that: In the high-grade flotation system, the high-grade copper-molybdenum concentrate obtained has a fineness of -0.074mm and a content of 80-90%.
11. The method for beneficiating copper-molybdenum ores containing different ore grades according to claim 1, characterized in that: In the low-grade flotation system, the low-grade copper-molybdenum concentrate obtained has a fineness of -0.074mm and a content of 92-98%.