A hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer and its preparation method and application
By using hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer in optical fiber and optical cable grease, the existing technology problem of hydrogenated styrene/isoprene block copolymer in optical fiber is solved. Or the performance deficiencies in optical cable grease, achieving high transparency, good thixotropy and excellent viscosity-temperature properties.
Patent Information
- Application Number
- CN202211553835.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Existing hydrogenated styrene/isoprene block copolymers have poor viscosity and temperature properties, poor transparency, poor thixotropic properties, high cone penetration, high dropping point and steel when used in optical fiber or optical cable grease. Defects such as easy separation of net oil affect its practical application performance.
A hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer is used to perform one-stage isoprene homopolymerization and two-stage isoprene and butadiene copolymerization in an anionic polymerization system. , the third stage of styrene copolymerization, and the S-b-(P/E/B)-EP copolymer obtained through hydrogenation reaction. Control the molecular weight and use of structural regulators to reduce the production of small molecule polymers and improve molecular chain entanglement. knot density.
It achieves high transparency, good thixotropy, excellent viscosity-temperature properties, suitable cone penetration and dropping point, and significantly improves the comprehensive performance of optical fiber and optical cable grease.
Smart Images

Figure BDA0003982100820000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of styrene-based thermoplastic elastomer synthesis, and specifically relates to a hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer and a preparation method and application thereof. Background Art
[0002] Since the thermoplastic elastomer SEPS (including SEP) was industrialized worldwide in the late 1980s, it has been widely used in lubricant thickening and lubricating grease, optical cable sealing ointment, cosmetic-grade vaseline, coated leather (artificial leather), and transparent elastomers and film products. Optical fiber and optical cable ointment is a filler in optical fiber and optical cable sheaths. The ointment plays the role of insulation, sealing, waterproofing, moisture-proofing, buffering, and protection. SEP developed by Kraton in the United States is the core material of optical cable ointment. It exhibits excellent thixotropy, suitable viscosity and high and low temperature performance in ointment applications, and has good comprehensive performance. The industrialization of domestic hydrogenated styrene / isoprene polymer products was not achieved until 2017 by Baling Petrochemical, becoming the world's third producer of hydrogenated styrene / isoprene copolymers.
[0003] In the existing technology, in Chinese patent CN107793542A, in order to reduce or eliminate the content of small molecule polystyrene in hydrogenated styrene / isoprene block copolymer, the solvent system of the anionic polymerization system is studied, and toluene mixed in the conventional cyclohexane solvent can effectively increase the reaction probability of the active PS-Li end group with isoprene, reduce the content of small molecule polystyrene, and thus improve the dropping point of hydrogenated styrene / isoprene block copolymer when used in optical fiber or cable grease. However, from the feeding method, the polymer is reacted into a homopolymer of styrene in one stage, and the molecular weight is large, which may cause part of the unreacted styrene to form a partial random copolymer with isoprene, affecting the dropping point of the copolymer when used in optical fiber or cable grease.
[0004] Chinese patent CN112708085 mentions a hydrogenated isoprene / styrene block coupled polymer used in filling grease for optical cables. A new form of coupled polymer is provided, wherein the hydrogenated polymer arm is a two-block polymer arm of hydrogenated polyisoprene block-polystyrene block, which is connected to the coupling center through the polystyrene block to form a multi-arm star polymer, which can improve the performance of the optical cable grease gelling agent. However, the molecular weight of the coupled star polymer is 200,000-350,000, 60,000-75,000 per arm, and the coupling efficiency is 85%-95%. Some uncoupled low molecular weight hydrogenated isoprene-polystyrene block copolymers are prone to exist during the polymerization, and cross-linking and gel formation are also prone to occur during the production process. This affects the cone penetration and dropping point of the copolymer used in the optical cable grease, and the transparency and thixotropic properties are poor.
[0005] Chinese patent CN113563549A discloses an asymmetric branched polystyrene-b-polyethylene-butylene-propylene-isopropylene multi-microblock copolymer, which is obtained by hydrogenating an asymmetric branched polystyrene-b-isoprene-butadiene random copolymer block copolymer (SbI / B / D). The SbE / B / P / D polymer has the characteristics of asymmetric long-chain branching, high side chain groups and high intermolecular entanglement. The polymer is used in combination with cyclohexane white oil to have excellent comprehensive performance and good thixotropic properties, and is very suitable for making optical fiber filling paste. However, the first stage of the polymer polymerization process is styrene polymerization, and the second stage is to increase the branching degree of the polymer molecular chain and avoid excessive DVB from forming homopolymers, and the polymerization is carried out by continuously dropping butadiene, isoprene and DVB. On the one hand, a small amount of low-molecular PS will inevitably be produced. On the other hand, it is difficult to control the degree of branching of the polymer, which can easily broaden the molecular weight distribution of the polymer, affecting the cone penetration, dropping point, transparency and low-temperature viscosity of the copolymer used in optical cable ointment.
[0006] At present, the polymers for optical cable grease in the domestic market include SEPG1701 and G1702 produced by Kraton, USA, which have excellent performance, YH-4010 launched by Baling Petrochemical, and SEP products launched by Zhejiang Zhongcheng Chemical Company in the past two years. From the perspective of polymer structure, the SEPs launched by the three companies are all two-block linear copolymers of styrene and isoprene, with a two-block content of 100%. However, when used as optical cable grease, there are still some shortcomings compared with imported products in terms of actual application performance. Specifically, they are manifested in poor viscosity-temperature performance, poor transparency, poor thixotropic performance, high cone penetration, high dropping point, and easy separation of steel mesh oil. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems existing in the prior art and provide a hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer and a preparation method thereof. The triblock copolymer is applied to optical fiber and optical cable ointment and has the characteristics of high transparency, good thixotropy, good viscosity-temperature performance, suitable cone penetration and dropping point, etc.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] A hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer, wherein the copolymer has a general formula of Sb-(P / E / B)-EP and is obtained by hydrogenating a polymer of the structural formula Sb-(I / B)-I;
[0010] Wherein, Sb is a homopolymer block of styrene;
[0011] P / E / B is a block of I / B (isoprene and butadiene) random copolymer;
[0012] EP is a homopolymer block of isoprene.
[0013] The mass ratio of styrene units in the copolymer Sb-(I / B)-I before hydrogenation is S / (I+B)=(30-40):(70-60).
[0014] The unit mass ratio of butadiene B to isoprene I in the copolymer Sb-(I / B)-I before hydrogenation is (5-10):(95-90).
[0015] In the copolymer Sb-(I / B)-I before hydrogenation, the random copolymerization units of isoprene account for 5%-10% of the total mass of the isoprene units.
[0016] The degree of hydrogenation of the isoprene and butadiene units of the copolymer Sb-(I / B)-I is greater than 98%.
[0017] The block copolymer has a number average molecular weight of 120,000-150,000 and a molecular weight distribution index of 1.01-1.05, wherein the number average molecular weight of the styrene homopolymer segment PS is 25,000-50,000.
[0018] In the block copolymer Sb-(P / E / B)-EP, the 3,4 structure and 1,2 structure of isoprene account for 50-60% of the total mass of isoprene, and the 1,2 structure of butadiene accounts for 50%-70% of the total mass of butadiene.
[0019] A method for preparing a hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer Sb-(P / E / B)-EP comprises the following steps:
[0020] Step (1): in an anionic polymerization system, adding a solvent, isoprene, an activator, a structure regulator, and an initiator into a polymerization reaction kettle to carry out a homopolymerization reaction of isoprene to obtain an active isoprene block polymer PI-Li, wherein the solvent is cyclohexane, the activator is tetrahydrofuran, and the initiator is n-butyl lithium;
[0021] Step (2): After the first stage polymerization is completed, a mixed monomer of isoprene and butadiene is slowly added to the polymerization reactor to carry out a second stage polymerization to obtain active PI-P(I / B)-Li;
[0022] Step (3): After the second stage polymerization is completed, styrene monomer is added to the polymerization reactor to carry out three-stage polymerization to obtain the target copolymer PI-P(I / B)-PSLi;
[0023] Step (4): After the target copolymer PI-P(I / B)-PSLi is terminated, it is transferred to a hydrogenation reactor for hydrogenation reaction, purification, water vapor condensation, and drying to obtain a hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer Sb-(P / E / B)-EP.
[0024] The structure regulator is one or more of ditetrahydroconpropane, TMEDA, 2G, sodium tert-amyl alcohol or potassium tert-butoxide; the molar ratio of the structure regulator to the active lithium is 0.05-1:1.
[0025] The polymerization reaction temperature is 50-100°C.
[0026] The hydrogenation reaction catalyst system is a nickel / aluminum catalyst, the Al / Ni molar ratio is 3-5, and the added amount of the catalyst is 0.5-0.85 mmol nickel / 100 g polymer.
[0027] The temperature of the hydrogenation reaction is 60-110° C., and the hydrogen pressure is 1.5-2.0 MPa.
[0028] The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer Sb-(P / E / B)-EP is used for preparing optical fiber and optical cable filling ointment.
[0029] The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer Sb-(P / E / B)-EP is mixed with alkyl white oil and used as optical fiber and optical cable filling ointment, which helps to improve the performance of the optical cable ointment.
[0030] The advantages and positive effects of the present invention are:
[0031] The present invention innovatively provides a tri-block hydrogenated styrene-b-conjugated diene-isoprene copolymer Sb-(P / E / B)-EP. Compared with the traditional two-block hydrogenated styrene-b-isoprene SEP, without changing the main structure of the copolymer, the isoprene is first polymerized in one stage, the micro-block polypropylene-ethylene-butylene structure is innovatively introduced in the second stage, and the third stage is copolymerized with styrene, which can greatly reduce or even eliminate the production of small molecule polymer PS and random copolymerization of isoprene and styrene PIS. At the same time, the content of side groups of the molecular chain is increased by regulating and controlling the structure regulator, and the entanglement density between the molecular chains is greatly increased. Studies have found that when the modified copolymer is used for optical fiber and cable ointment, it has the characteristics of high transparency, good thixotropy, good viscosity-temperature performance, suitable cone penetration and dropping point, etc. DETAILED DESCRIPTION
[0032] In order to describe the present invention in more detail, the following embodiments are further described, but the present invention is not limited to the scope of the embodiments.
[0033] The molecular weight and molecular weight distribution index of the polymers in the examples were determined by gel permeation chromatography (GPC), and the GPC test standard was Q / SH019.05.P.003(05)-1998. The microstructure of the polymers was determined by H-NMR spectrum using a BRUKER AV-600M nuclear magnetic resonance analyzer. The degree of hydrogenation of the polymers was determined by iodine titration.
[0034] Example 1
[0035] In a 5-liter polymerization kettle under nitrogen protection, 3000 ml of cyclohexane was added, and then 175 g of isoprene, 10 ml of tetrahydrofuran, 0.64 mmol of structure regulator sodium tert-amyl alcohol and ditetrahydrofurfuryl propane (the molar ratio of the two was 1:1) were added to the polymerization kettle, and the solvent system was heated to 60°C. According to the designed molecular weight, 2.0 ml of 1.6 mol / l n-butyl lithium solution was immediately added to the polymerization kettle to carry out a homopolymerization reaction of isoprene. The reaction polymerization temperature was controlled at 60°C and stirred for 30 minutes. Then, 10 g of mixed isoprene monomer and 10 g of butadiene monomer were added to the polymerization kettle, and the reaction was continued for 20 minutes. After the second stage reaction was completed, 105 g of styrene was added to carry out a three-stage polymerization reaction. The temperature was controlled at 60°C, the reaction was stirred for 30 minutes, and about 5 ml of isopropanol was added to terminate the reaction.
[0036] After the polymerization, the polymerized gel was pressed into a 5-liter hydrogenation kettle, the temperature was controlled at 70°C, and an aged Ni / Al catalyst (Al / Ni molar ratio was 4) was added to the hydrogenation kettle, and the catalyst dosage was 0.85mmol nickel / 100g polymer. The hydrogenation reaction was carried out at 70°C and 1.5MPa for 120min. After the reaction was completed, the gel was pressed into an acid washing kettle, and a small amount of citric acid was added for washing to remove the metal ions in the gel. Then 0.5% antioxidant 1076 based on the weight of the polymer was added, and after stirring for 5 minutes, the product was added to steam and hot water for condensation to obtain solid gel particles, which were dried to obtain copolymers. After analysis, the data molecular weight Mn of the copolymer was 120,000, the molecular weight distribution index was 1.02, the content of 3,4-structure in isoprene was 55%, and the content of 1,2-structure (vinyl structure) in butadiene was 65%. The degree of hydrogenation measured by iodine titration was 99.2%. The copolymer was mixed with alkyl white oil to prepare an ointment, and its cone penetration, dropping point and viscosity were measured. The data are shown in Table 1.
[0037] Example 2
[0038] Compared with Example 1, the relevant polymerization conditions remain unchanged, except that the structure regulator system is changed, 0.8mmol of structure regulator sodium tert-amyl alcohol and 2G (the molar ratio of the two is 1:1) are added, and after the polymerization is completed, hydrogenation is carried out according to the hydrogenation process of Example 1. After the reaction is completed, the glue is pressed into the pickling kettle, and a small amount of citric acid solution is added for washing to remove the metal ions in the glue. Then 0.5% antioxidant 1076 based on the weight of the polymer is added, and after stirring for 5 minutes, the product is added to steam and hot water for condensation to obtain solid colloid particles, and the copolymer is obtained after drying. After analysis, the data molecular weight Mn of the copolymer is 123,000, the molecular weight distribution index is 1.03, the content of 3,4-structure in isoprene is 58%, and the content of 1,2-structure (vinyl structure) in butadiene is 61%. The degree of hydrogenation measured by iodine titration is 99.0%. The copolymer is mixed with alkyl white oil to obtain an ointment, and its cone penetration, dropping point and viscosity are measured. The data are shown in Table 1.
[0039] Example 3
[0040] Compared with Example 1, the relevant polymerization conditions remain unchanged, except that 1.5 ml of n-butyl lithium is added. After the polymerization is completed, hydrogenation is carried out according to the hydrogenation process of Example 1. After the reaction is completed, the glue is pressed into the pickling kettle, and a small amount of citric acid solution is added for washing to remove the metal ions in the glue. Then 0.5% antioxidant 1076 based on the weight of the polymer is added, and after stirring for 5 minutes, the product is added to steam and hot water for condensation to obtain solid colloid particles, and the copolymer is obtained after drying. After analysis, the data molecular weight Mn of the copolymer is 140,000, the molecular weight distribution index is 1.05, the content of 3,4-structure in isoprene is 53%, and the content of 1,2-structure (vinyl structure) in butadiene is 56%. The degree of hydrogenation measured by iodine titration is 98.9%. The copolymer is mixed with alkyl white oil to obtain an ointment, and its cone penetration, dropping point and viscosity are measured. The data are shown in Table 1.
[0041] Example 4
[0042] Compared with Example 1, the relevant polymerization conditions remain unchanged, except that the amount of isoprene added in the first stage is 165g, and the amount of isoprene and butadiene mixed monomer added in the second stage is 15g each. After the polymerization is completed, hydrogenation is carried out according to the hydrogenation process of Example 1. After the reaction is completed, the glue is pressed into the pickling kettle, and a small amount of citric acid solution is added for washing to remove the metal ions in the glue solution. Then 0.5% antioxidant 1076 based on the weight of the polymer is added, and after stirring for 5 minutes, the product is added to steam and hot water for condensation to obtain solid colloid particles, and the copolymer is obtained after drying. After analysis, the data molecular weight Mn of the copolymer is 125,000, the molecular weight distribution index is 1.03, the content of 3,4-structure in isoprene is 54%, and the content of 1,2-structure (vinyl structure) in butadiene is 55%. The degree of hydrogenation measured by iodine titration is 99.4%. The copolymer is mixed with alkyl white oil to obtain an ointment, and its cone penetration, dropping point and viscosity are measured. The data are shown in Table 1.
[0043] Example 5
[0044] Compared with Example 1, the relevant polymerization conditions remain unchanged, except that the amount of isoprene added in the first stage is 180g, and the amount of isoprene and butadiene mixed monomer added in the second stage is 15g each. The amount of styrene added in the third stage is 90g. After the polymerization is completed, hydrogenation is carried out according to the hydrogenation process of Example 1. After the reaction is completed, the glue is pressed into the pickling kettle, and a small amount of citric acid solution is added for washing to remove the metal ions in the glue solution. Then, 0.5% antioxidant 1076 based on the weight of the polymer is added, and after stirring for 5 minutes, the product is added to steam and hot water for condensation to obtain solid colloid particles, and the copolymer is obtained after drying. After analysis, the data molecular weight Mn of the copolymer is 125,000, the molecular weight distribution index is 1.03, the content of 3,4-structure in isoprene is 54%, and the content of 1,2-structure (vinyl structure) in butadiene is 53%. The degree of hydrogenation measured by iodine titration is 99.4%. The copolymer is mixed with alkyl white oil to obtain an ointment, and its cone penetration, dropping point and viscosity are measured. See Table 1 for data.
[0045] Comparative Example 1
[0046] In a 5-liter polymerization kettle under nitrogen protection, 3000 ml of cyclohexane was added, and then 195 g of isoprene, 10 ml of tetrahydrofuran, 0.64 mmol of sodium tert-amyl alcohol and ditetrahydrofurfuryl propane (molar ratio of the two was 1:1) were added into the polymerization kettle, and the solvent system was heated to 60°C. According to the designed molecular weight, 2.0 ml of 1.6 mol / l n-butyl lithium solution was immediately added into the polymerization kettle to carry out a homopolymerization reaction of isoprene. The polymerization temperature was controlled at 60°C and the reaction was stirred for 30 minutes. After the first reaction was completed, 105 g of styrene was added to carry out a second-stage polymerization reaction. The temperature was controlled at 60°C and the reaction was stirred for 30 minutes. About 5 ml of isopropanol was added to terminate the reaction.
[0047] After the polymerization, the polymerized gel was pressed into a 5-liter hydrogenation kettle, the temperature was controlled at 70°C, and an aged Ni / Al catalyst (Al / Ni molar ratio was 4) was added to the hydrogenation kettle, and the catalyst dosage was 0.85mmol nickel / 100g polymer. The hydrogenation reaction was carried out at 70°C and 1.5MPa for 120min. After the reaction, the gel was pressed into an acid washing kettle, and a small amount of citric acid solution was added for washing to remove the metal ions in the gel. Then, 0.5% antioxidant 1076 based on the weight of the polymer was added, and after stirring for 5 minutes, the product was added to steam and hot water for condensation to obtain solid gel particles, which were dried to obtain a diblock copolymer SEP. After analysis, the data molecular weight Mn of the copolymer was 125,000, the molecular weight distribution index was 1.07, the content of 3,4-structure in isoprene was 40%, and the degree of hydrogenation measured by iodine titration was 99.0%. The copolymer was mixed with alkyl white oil to obtain an ointment, and its cone penetration, dropping point and viscosity were measured. The data are shown in Table 1.
[0048] Comparative Example 2
[0049] In a 5-liter polymerization kettle under nitrogen protection, 3000 ml of cyclohexane was added, and then 105 g of styrene, 10 ml of tetrahydrofuran, 0.64 mmol of structure regulator sodium tert-amyl alcohol and ditetrahydrofurfuryl propane (the molar ratio of the two was 1:1) were added into the polymerization kettle, and the solvent system was heated to 60°C. According to the designed molecular weight, 2.0 ml of 1.6 mol / l n-butyl lithium solution was immediately added into the polymerization kettle to carry out a first-stage homopolymerization of styrene. The reaction polymerization temperature was controlled at 60°C and the reaction was stirred for 30 minutes. After the first-stage reaction was completed, 195 g of isoprene was added to carry out a second-stage polymerization reaction. The temperature was controlled at 60°C and the reaction was stirred for 30 minutes. About 5 ml of isopropanol was added to terminate the reaction.
[0050] After the polymerization, the polymerized gel was pressed into a 5-liter hydrogenation kettle, the temperature was controlled at 70°C, and an aged Ni / Al catalyst (Al / Ni molar ratio was 4) was added to the hydrogenation kettle, and the catalyst dosage was 0.85mmol nickel / 100g polymer. The hydrogenation reaction was carried out at 70°C and 1.5MPa for 120min. After the reaction, the gel was pressed into an acid washing kettle, and a small amount of citric acid solution was added for washing to remove the metal ions in the gel. Then, 0.5% antioxidant 1076 based on the weight of the polymer was added, and after stirring for 5 minutes, the product was added to steam and hot water for condensation to obtain solid gel particles, which were dried to obtain a diblock copolymer SEP. After analysis, the data molecular weight Mn of the copolymer was 124,000, the molecular weight distribution index was 1.06, the content of 3,4-structure in isoprene was 45%, and the hydrogenation degree was 99.1% measured by iodine titration. The copolymer was mixed with alkyl white oil to obtain an ointment, and its cone penetration, dropping point and viscosity were measured. The data are shown in Table 1.
[0051] Table 1
[0052]
[0053] Note: Preparation method of optical fiber and cable filling ointment: Add 20g block copolymer and 180g alkyl white oil into a 500ml beaker, heat in a heating mantle, stir, and control the temperature at 100-120℃ until it becomes a uniform and viscous ointment.
[0054] The cone penetration test of the optical fiber and cable filling ointment is determined by the depth of the cone inserted into the ointment for 5 seconds after the ointment is placed for 24 hours. The dropping point of the ointment is determined according to GB 4929-85 standard. The viscosity test of the ointment: tested with a Rheolab QC rotational viscometer at 40℃ and 80℃.
[0055] As can be seen from Table 1, the performance of the grease prepared by mixing the hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer of the embodiment of the present invention with the alkyl white oil is significantly better than that of the diblock copolymer SEP of Comparative Examples 1 and 2. The reason for the analysis is that in Comparative Example 1, isoprene is first used and then styrene is used to prepare the diblock SEP, which will produce some small molecule PIS, which has many small molecules, low viscosity, large cone penetration, and low dropping point, affecting the dynamic viscosity, cone penetration, and dropping point. Comparative Example 2 changes the order of feeding, adds styrene first, and prepares the diblock SEP. This process will produce more small molecule PS, which also affects the dynamic viscosity, cone penetration, and dropping point. Therefore, compared with the diblock SEP, the Sb-(P / E / B)-EP triblock copolymer of the present invention has the characteristics of high regular S and EP two-block content and high side chain group content. When the polymer of this structure is used for filling grease for optical fiber and optical cable, the grease has high viscosity, good viscosity-temperature performance, and better low-temperature performance, showing excellent dropping point and cone penetration, and has excellent performance.
Claims
1. A hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer, characterized in that: The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer is prepared by polymerizing isoprene in the first stage, introducing a microblock polypropylene-ethylene-butylene structure in the second stage, and copolymerizing with styrene in the third stage; The general formula of the copolymer is Sb-(P / E / B)-EP, and the copolymer is obtained by hydrogenating a polymer of the structural formula Sb-(I / B)-I; Wherein, Sb is a homopolymer block of styrene; P / E / B is a block obtained by hydrogenating a random copolymer of I / B (isoprene and butadiene); EP is a block obtained by hydrogenating an isoprene homopolymer block.
2. The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to claim 1, characterized in that: The mass ratio of styrene units in the copolymer Sb-(I / B)-I before hydrogenation is S / (I+B)=(30-40):(70-60).
3. The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to claim 1, wherein: The unit mass ratio of butadiene B to isoprene I in the copolymer Sb-(I / B)-I before hydrogenation is (5-10):(95-90).
4. The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to claim 1, wherein: Before hydrogenation, the isoprene random copolymer units in the copolymer Sb-(I / B)-I account for 5%-10% of the total mass of the isoprene units.
5. The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to claim 1, characterized in that: The degree of hydrogenation of the isoprene and butadiene units of the copolymer Sb-(I / B)-I is >98%.
6. The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to claim 1, wherein: The block copolymer Sb-(P / E / B)-EP has a number average molecular weight of 120,000-150,000 and a molecular weight distribution index of 1.01-1.05, wherein the number average molecular weight of the styrene homopolymer segment PS is 25,000-50,000.
7. The hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to claim 1, wherein: In the block copolymer Sb-(P / E / B)-EP, the 3,4 structure and 1,2 structure of isoprene account for 50-60% of the total mass of isoprene, and the 1,2 structure of butadiene accounts for 50%-70% of the total mass of butadiene.
8. A method for preparing the hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step (1): In an anionic polymerization system, a solvent, isoprene, an activator, a structure regulator, and an initiator are added to a polymerization reactor to carry out a first stage of isoprene homopolymerization to obtain an active isoprene block polymer PI-Li, wherein the solvent is cyclohexane, the activator is tetrahydrofuran, and the initiator is n-butyl lithium; Step (2): After the first stage polymerization is completed, a mixed monomer of isoprene and butadiene is slowly added to the polymerization reactor to carry out a second stage polymerization to obtain active PI-P(I / B)-Li; Step (3): After the second stage polymerization is completed, styrene monomer is added to the polymerization reactor to carry out three-stage polymerization to obtain the target copolymer PI-P(I / B)-PSLi; Step (4): After the target copolymer PI-P(I / B)-PSLi is terminated, it is transferred to a hydrogenation reactor for hydrogenation reaction, purification, water vapor condensation, and drying to obtain a hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer Sb-(P / E / B)-EP.
9. The method for preparing a hydrogenated styrene-b-conjugated diene-isoprene triblock copolymer according to claim 8, wherein: The structure regulator is one or more of ditetrahydrofurfuryl propane, TMEDA, 2G, sodium tert-amyl alcohol or potassium tert-butoxide; the molar ratio of the structure regulator to the active lithium is 0.05-1: