A copper alkaline chemical mechanical polishing liquid

By adding diethanolamine as a pH stabilizer to the alkaline copper polishing solution, the problem of unstable pH value of the polishing solution is solved, the stability of the abrasive is maintained, polishing defects are reduced, and storage life is improved.

CN115786918BActive Publication Date: 2024-10-15HEBEI UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211451885.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-21
Publication Date
2024-10-15
Estimated Expiration
2042-11-21

AI Technical Summary

Technical Problem

The pH value of the existing alkaline copper polishing solution is unstable, resulting in uneven abrasive particle size distribution and prone to problems such as delamination of the polishing solution, gel and scratches on the copper wafer surface, which affects the polishing quality.

Method used

Add diethanolamine as a pH stabilizer to the alkaline copper polishing solution to prevent hydrolysis and decomposition of quaternary ammonium alkali, absorb carbon dioxide in the air and H+ ions in the solution, keep the pH value stable, and prevent abrasive agglomeration and stratification.

Benefits of technology

It effectively improves the pH stability of the polishing fluid, prevents abrasive delamination and gel formation, reduces polishing defects such as scratches and roughness, and extends the storage life of the polishing fluid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115786918B_ABST
    Figure CN115786918B_ABST
Patent Text Reader

Abstract

The invention discloses a copper alkaline chemical mechanical polishing liquid. The polishing liquid comprises 0.05-1% of diethanolamine, 3-6% of abrasive, 0.1-2% of quaternary ammonium compound, 8-13% of copper strong etchant, and the balance of deionized water by weight; the pH value of the polishing liquid is 7.5-10; and the polishing liquid further comprises 0.01-0.5% of xanthan gum by weight. The invention can improve the pH stability of the alkaline copper polishing liquid containing quaternary ammonium base, prevent abrasive delamination, gelation, and particle diameter growth, and reduce polishing defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a copper grinding material, in particular to an alkaline copper chemical mechanical polishing liquid containing a quaternary ammonium compound. Background Art

[0002] Metal copper is a common interconnection method for integrated circuits. Through silicon vias can achieve vertical conduction in the Z direction of the chip. It is an emerging chip three-dimensional packaging technology that effectively improves the integration capability of the chip. Through silicon vias are generally filled with metal copper as an interconnection layer. Whether it is used as an interconnection line or a through silicon via conductor, metal copper needs to be chemically mechanically polished. Alkaline polishing liquid mainly uses strong etchants such as organic amines and organic acids to react with copper to polish metal copper. In order to weaken the etching effect of strong etchants and obtain a controllable corrosion rate and good copper surface quality, it is often necessary to add components with weaker etching power to the polishing liquid as polishing defect inhibitors. Sometimes the pH value of the alkaline polishing liquid needs to maintain a stable value in order to maintain the stability of the workpiece removal rate. The pH value in the polishing liquid is an important factor in measuring whether the performance of a polishing liquid is stable. The pH value has a great influence on the abrasive particle size distribution, particle size, and uniformity in the polishing liquid. It is mainly manifested in the decomposition and dissolution of the abrasive, the etching of the polished surface and the formation of the oxide film, and the suspension degree (colloid stability). Therefore, the pH value of the polishing liquid needs to be strictly controlled. When the pH value deviates from the preset value, the material removal rate of the polishing liquid tends to be unstable, the scratches and contamination defects on the copper wafer surface tend to increase, and the roughness of the wafer tends to increase. The pH value of the polishing liquid will change over time. This is because some alkaline polishing liquid components are consumed by hydrolysis during polishing, or are neutralized by dissolved acidic gases such as carbon dioxide during actual polishing. The pH value changes most dramatically after each addition of polishing liquid. In addition, the pH value of some polishing liquids drifts over time during the transportation and storage stages of the polishing liquid, mainly because the components in the polishing liquid may change due to oxidation decomposition reactions.

[0003] The four hydrogen atoms of ammonium hydroxide are replaced by hydrocarbon groups, which is called quaternary ammonium base. Quaternary ammonium base is a class of compounds with the general formula R4NOH, where R is four identical or different aliphatic or aromatic groups. The molecular structure is similar to ammonium hydroxide and can be regarded as the latter NH4 +The derivative obtained by replacing the hydrogen in the quaternary ammonium is strongly alkaline, easy to deliquesce, easily soluble in water and 100% ionized. Choline and betaine, which are commonly present in organisms, are natural quaternary ammonium bases. Tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, trimethylethylammonium hydroxide, etc. are also quaternary ammonium bases. Quaternary ammonium bases have a gentle etching effect on the polished metal materials such as copper materials. They are often used as corrosion defect inhibitors in copper polishing liquids. They are used in combination with strong etchants composed of organic amines such as hydroxylamine, ethylenediamine, EDTA, or carboxylic acids, phosphonic acids, and sulfonic acids with strong chelating effects and added to the polishing liquid. Organic quaternary ammonium salts can be hydrolyzed in water to obtain quaternary ammonium bases, which can replace quaternary ammonium bases, so they are often added to polishing liquids.

[0004]

[0005] Patents CN104250816B and CN111732897A use choline or choline salts to add to the polishing liquid system, and patents 109251673A, CN102337079B, and US2006014390 use organic quaternary ammonium alkalis to add to the polishing liquid system, all of which achieve good metal copper etching effects. However, quaternary ammonium alkalis are unstable in weakly alkaline aqueous solutions with a pH value of 7.5-10, and are easily decomposed into amines, causing the solution pH to drift and fluctuate. The solution pH drift and fluctuation will then cause the abrasive particle size distribution, particle size, and uniformity, and eventually even cause the copper polishing liquid to delaminate and gel; after wafer polishing, there will be a series of problems such as scratches, excessive dishing pits, and excessive roughness. Summary of the invention

[0006] The purpose of the present invention is to provide a copper alkaline chemical mechanical polishing liquid in view of the existing technical problems. The polishing liquid is prepared by adding a small amount of diethanolamine (DEA) as a pH stabilizer for the alkaline copper polishing liquid containing a quaternary ammonium base. The diethanolamine has a strong reducing ability, which can prevent the quaternary ammonium base from hydrolyzing and decomposing to cause pH fluctuations, and can also absorb carbon dioxide dissolved in the polishing liquid from the air, absorb H2O that accidentally appears in the solution, and stabilize the pH of the alkaline copper polishing liquid. + Ions can prevent changes in the equilibrium potential of abrasives caused by pH fluctuations, which can cause abrasive agglomeration and stratification, and changes in abrasive dispersion can cause scratches, contamination, and large roughness on the polished surface. The present invention can improve the pH stability of alkaline copper polishing liquid containing quaternary ammonium bases, prevent abrasive stratification, gelation, and particle diameter growth, and reduce polishing defects.

[0007] To achieve the purpose of the present invention, the technical solution adopted is:

[0008] A copper alkaline chemical mechanical polishing liquid, the mass percentage of which is 0.05-1% of diethanolamine, 3-6% of abrasive, 0.1-2% of quaternary ammonium compound, 8-13% of copper strong etchant, and the balance is deionized water; the pH value of the polishing liquid is 7.5-10;

[0009] The polishing liquid also includes 0.01-0.5% by mass of xanthan gum;

[0010] The abrasive is silicon dioxide or silica sol with a particle size of 60 to 100 nm.

[0011] The quaternary ammonium compound is a quaternary ammonium base or a quaternary ammonium salt; the general formula of the quaternary ammonium base is R4NOH; the general formula of the quaternary ammonium salt is R4NX; wherein the four hydrocarbon groups R may be the same or different; X is F - , Cl - Br - ,I - 、NO3 - 、SO4 2- 、HSO4 - or RCOO - ;

[0012] The quaternary ammonium base is specifically tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, trimethylethylammonium hydroxide, betaine or choline; the quaternary ammonium salt is specifically tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium sulfate, tetramethylammonium nitrate, tetramethylammonium acetate, trimethylglycine hydrochloride, choline carbonate, choline bicarbonate or choline hydrochloride.

[0013] The strong copper etchant is an organic carboxylic acid, an organic phosphonic acid, an organic sulfonic acid, an amino acid and its derivatives. Specifically, the organic amine can be one or a combination of ethylamine, ethylenediamine, hydroxyethylethylenediamine, tetrahydroxyethylethylenediamine, and ethylenediaminetetraacetic acid, preferably ethylenediamine, glycine or a combination of the two.

[0014] The method for preparing the copper alkaline chemical mechanical polishing solution comprises the following steps:

[0015] (1) adding a small amount of deionized water to an abrasive, a quaternary ammonium compound, diethanolamine, and a strong copper etchant respectively, and stirring the mixture to prepare respective diluted solutions;

[0016] (2) adding the diluted quaternary ammonium compound, diethanolamine, and copper strong etchant solution to the abrasive aqueous solution in sequence while stirring;

[0017] (3) Add deionized water to a near-quantitative amount, adjust the pH to the rated value, and make up the remainder with deionized water;

[0018] The pH value regulator is KOH solution or lactic acid.

[0019] The copper alkaline chemical mechanical polishing liquid is used for copper-plated wafers, copper wiring wafers or through-silicon via copper interconnect wafers.

[0020] The essential features of the present invention are:

[0021] In the present invention, a small amount of diethanolamine (DEA) is added to the alkaline polishing liquid as a pH stabilizer. Since diethanolamine has a strong reducing ability, it can remove oxygen free radicals in the solution, which can not only prevent the pH fluctuation caused by the hydrolysis and decomposition of the quaternary ammonium base, but also absorb the carbon dioxide dissolved in the polishing liquid from the air and absorb the H + ions to avoid abrasive agglomeration and stratification caused by changes in abrasive equilibrium potential due to pH fluctuations.

[0022] The beneficial effects of the present invention are:

[0023] The polishing liquid to which diethanolamine is added can prevent the Zeta potential of the abrasive from changing, prevent the abrasive from being delaminated, gelled, and having a larger particle diameter, maintain the stability of the abrasive, reduce polishing defects such as scratches, stains, fog defects, and large roughness, and effectively improve the storage life of the alkaline polishing liquid; it can be kept stable for 50 days, and the pH fluctuation can be basically ignored, with a fluctuation range of 0 to 0.15; while the polishing liquid without diethanolamine has a stable range of less than 5 days, and the fluctuation range gradually increases after 5 days, and on the 50th day, the pH fluctuation reaches 0.65, that is, the effective component of the quaternary ammonium base has begun to decompose. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 SEM image of the abrasive being 80 nanometer silica;

[0025] Figure 2 Fluctuation diagram of copper film removal rate corresponding to Example 1 as a function of polishing liquid storage days;

[0026] Figure 3 Fluctuation graph of pH value of copper polishing solution corresponding to Example 1 with storage days;

[0027] Figure 4 Fluctuation diagram of copper film removal rate corresponding to Example 2 as a function of polishing liquid storage days;

[0028] Figure 5 Fluctuation chart of pH value of copper polishing liquid corresponding to Example 2 with storage days;

[0029] Figure 6 Fluctuation diagram of copper film removal rate corresponding to Example 3 as a function of polishing liquid storage days;

[0030] Figure 7 Fluctuation graph of pH value of copper polishing solution corresponding to Example 3 with storage days;

[0031] Figure 8 Fluctuation diagram of copper film removal rate corresponding to Example 4 versus storage days of polishing liquid;

[0032] Fig. 9 Fluctuation chart of pH value of copper polishing solution corresponding to Example 4 with storage days; DETAILED DESCRIPTION

[0033] In the present invention, diethanolamine (DEA) is a well-known substance with the following chemical formula; as a pH stabilizer for alkali solution, diethanolamine has a strong reducing ability and can remove oxygen free radicals in the solution to prevent quaternary ammonium base from oxidative decomposition. On the other hand, diethanolamine can absorb and neutralize carbon dioxide in the air absorbed by the solution and can absorb H + , stabilize the pH value and prevent it from drifting. In another aspect, diethanolamine is also a good complexing agent, which plays a role in accelerating the complexing and dissolution of copper polishing products.

[0034]

[0035] The copper chemical mechanical polishing (CMP) composition comprises an abrasive, a strong copper etchant (organic amine or organic acid), an organic quaternary ammonium salt (quaternary ammonium base) of a Cu dishing and defect reducing agent, diethanolamine, and deionized water.

[0036] Take the preparation of 1000g polishing liquid as an example:

[0037] Embodiment 1:

[0038] 1. Weigh 150g of 80nm silica sol (mainly composed of silicon dioxide) with a concentration of 40%, 5g of tetramethylammonium hydroxide, 100g of glycine, 10g of ethylenediamine, 5g of diethanolamine, and 0.5g of xanthan gum, add a small amount of deionized water and stir to prepare respective dilution solutions;

[0039] 2. Add the diluted tetramethylammonium hydroxide, glycine, ethylenediamine, diethanolamine and xanthan gum to the aqueous solution of silica sol in sequence, stirring evenly while adding;

[0040] 3. Add deionized water to make the total weight close to 950g, adjust the pH to 9 with 0.5mol / L potassium hydroxide solution, make up the balance to 1000g with deionized water, and stir evenly. (The composition of the obtained polishing liquid is: 6% by mass of silicon dioxide, 0.5% by mass of tetramethylammonium hydroxide, 10% by mass of glycine, 1% by mass of ethylenediamine, 0.5% by mass of diethanolamine, and 0.05% by mass of xanthan gum)

[0041] The polishing machine is a fully automated CMP equipment developed and produced by Huahai Qingke, model U300B, the polishing sheet is a 12-inch copper wafer; the polishing pad is the Dow Chemical Company IC1010 polishing pad; the polishing parameters are: down pressure 1.5psi; polishing head speed 87rpm; polishing disc speed 93rpm; polishing liquid flow 300ml / min. The polishing liquid can be placed for 50 days without precipitation or stratification. After polishing, the copper removal rate is stable at about 12,000 angstroms / minute, with no obvious changes.

[0042] Embodiment 2:

[0043] 1. Weigh 75g of 80nm silica sol (mainly composed of silicon dioxide) with a particle size of 40%, 5g of tetramethylammonium hydroxide, 80g of glycine, 10g of ethylenediamine, 5g of diethanolamine, and 0.5g of xanthan gum, and add a small amount of deionized water to each of them while stirring to prepare their own dilution solutions;

[0044] 2. Add the diluted tetramethylammonium hydroxide, glycine, ethylenediamine, diethanolamine and xanthan gum to the aqueous solution of silica sol in sequence, stirring evenly while adding;

[0045] 3. Add deionized water to make the total weight close to 950g, adjust the pH to 9 with 0.5mol / L potassium hydroxide solution, make up the balance to 1000g with deionized water, and stir evenly; (the composition of the obtained polishing liquid is: 3% by mass of silicon dioxide, 0.5% by mass of tetramethylammonium hydroxide, 8% by mass of glycine, 1% by mass of ethylenediamine, 0.5% by mass of diethanolamine, and 0.05% by mass of xanthan gum)

[0046] The polishing machine is a fully automated CMP equipment developed and produced by Huahai Qingke, model U300B, the polishing sheet is a 12-inch copper wafer; the polishing pad is the Dow Chemical Company IC1010 polishing pad; the polishing parameters are: down pressure 1.5psi; polishing head speed 87rpm; polishing disc speed 93rpm; polishing liquid flow 300ml / min. The polishing liquid can be placed for 50 days without precipitation or stratification. After polishing, the copper removal rate is stable at about 10,000 angstroms / minute, with no obvious changes.

[0047] Embodiment 3:

[0048] 1. Weigh 75g of 80nm silica sol (mainly composed of silicon dioxide) with a concentration of 40%, 5g of tetramethylammonium hydroxide, 130g of glycine, 10g of ethylenediamine, 5g of diethanolamine, and 0.5g of xanthan gum, add a small amount of deionized water and stir to prepare their respective diluted solutions;

[0049] 2. Add the diluted tetramethylammonium hydroxide, glycine, ethylenediamine, diethanolamine and xanthan gum to the aqueous solution of silica sol in sequence, stirring evenly while adding;

[0050] 3. Add deionized water to make the total weight close to 950g, adjust the pH to 9 with 0.5mol / L potassium hydroxide solution, make up the balance to 1000g with deionized water, and stir evenly; (the composition of the obtained polishing liquid is: 3% by mass of silicon dioxide, 0.5% by mass of tetramethylammonium hydroxide, 13% by mass of glycine, 1% by mass of ethylenediamine, 0.5% by mass of diethanolamine, and 0.05% by mass of xanthan gum)

[0051] The polishing machine is a fully automated CMP equipment developed and produced by Huahai Qingke, model U300B, the polishing sheet is a 12-inch copper wafer; the polishing pad is the Dow Chemical Company IC1010 polishing pad; the polishing parameters are: down pressure 1.5psi; polishing head speed 87rpm; polishing disc speed 93rpm; polishing liquid flow 300ml / min. The polishing liquid can be placed for 50 days without precipitation or stratification. After polishing, the copper removal rate is stable at about 16,000 angstroms / minute, with no obvious changes.

[0052] Embodiment 4:

[0053] 1. Weigh 75g of 80nm silica sol (mainly composed of silicon dioxide) with a concentration of 40%, 5g of tetramethylammonium hydroxide, 130g of glycine, 10g of ethylenediamine, and 0.5g of xanthan gum, add a small amount of deionized water and stir to prepare their respective diluted solutions;

[0054] 2. Add the diluted methylammonium hydroxide, glycine, ethylenediamine and xanthan gum to the aqueous solution of silica sol in sequence, stirring evenly while adding;

[0055] 3. Add deionized water to make the total weight close to 950g, adjust the pH to 9 with 0.5mol / L potassium hydroxide solution, make up the balance to 1000g with deionized water, and stir evenly; (the obtained polishing liquid composition content is: 3% by mass of silicon dioxide, 0.5% by mass of tetramethylammonium hydroxide, 13% by mass of glycine, 1% by mass of ethylenediamine, 0.05% by mass of xanthan gum, and the pH value is adjusted to 9.)

[0056] The polishing machine is a fully automated CMP equipment developed and produced by Huahai Qingke, model U300B, the polishing sheet is a 12-inch copper wafer; the polishing pad is the Dow Chemical Company IC1010 polishing pad; the polishing parameters are: down pressure 1.5psi; polishing head speed 87rpm; polishing disc speed 93rpm; polishing liquid flow 300ml / min. The polishing liquid did not produce precipitation or stratification after being placed for 5 days, but then the pH of the polishing liquid gradually deviated from 9 and developed in a smaller direction; the copper removal rate after polishing was stable at about 16,000 angstroms / minute for the first 5 days, and then, due to the lack of the stabilizing effect of diethanolamine, tetramethylammonium hydroxide began to hydrolyze and oxidatively decompose, the abrasive also showed a tendency to grow, the particle size began to agglomerate, the polishing rate began to be unstable, and the surface quality after polishing gradually deteriorated.

[0057] By comparing Examples 1, 2, and 3 (diethanolamine was added) with Example 4 (diethanolamine was not added), it can be seen that diethanolamine can neutralize the carbon dioxide in the air absorbed by the solution, and the H generated by the pH drift + , stabilize the pH value of the solution, prevent the Zeta potential of the abrasive from changing, prevent the abrasive from stratification, gelation, and particle diameter growth, maintain the stability of the abrasive, reduce polishing defects such as scratches, contamination, fog defects, and large roughness, and effectively increase the storage life of the alkaline polishing solution.

[0058] Matters not covered by the present invention are known technologies.

Claims

1. A copper alkaline chemical mechanical polishing liquid, characterized in that the mass percentage of the polishing liquid is 0.05-1% of diethanolamine, 3-6% of abrasive, 0.1-2% of quaternary ammonium compound, 8-13% of copper strong etchant, and the balance is deionized water; the pH value of the polishing liquid is 7.5-10; The polishing liquid also includes 0.01-0.5% by mass of xanthan gum; The quaternary ammonium compound is a quaternary ammonium base or a quaternary ammonium salt; the general formula of the quaternary ammonium base is R4NOH; the general formula of the quaternary ammonium salt is R4NX; X is F - , Cl - Br - ,I - 、NO3 - 、SO4 2- 、HSO4 - or RCOO - ; The quaternary ammonium base is specifically tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, trimethylethylammonium hydroxide, betaine or choline; the quaternary ammonium salt is specifically tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium sulfate, tetramethylammonium nitrate, tetramethylammonium acetate, trimethylglycine hydrochloride, choline carbonate, choline bicarbonate or choline hydrochloride; The copper strong etchant is a combination of ethylenediamine and glycine; The abrasive is silicon dioxide or silica sol.

2. The copper alkaline chemical mechanical polishing solution as claimed in claim 1, characterized in that the particle size of the silicon dioxide particles in the silicon dioxide or silica sol is 60-100 nm.

3. The method for preparing the copper alkaline chemical mechanical polishing solution according to claim 1, characterized in that The following steps are involved: (1) adding abrasive, quaternary ammonium compound, diethanolamine, and copper strong etchant to deionized water respectively and stirring at the same time to prepare respective diluted solutions; (2) adding the diluted quaternary ammonium compound, diethanolamine, and copper strong etchant solution to the abrasive aqueous solution in sequence while stirring; (3) Add deionized water to a near-quantitative amount, adjust the pH to the rated value, and make up the remainder with deionized water.

4. The method for preparing a copper alkaline chemical mechanical polishing solution as claimed in claim 3, wherein the pH regulator is a KOH solution or lactic acid.

5. The use of the copper alkaline chemical mechanical polishing solution as claimed in claim 1, characterized in that it is used for copper-plated wafers, copper wiring wafers or through-silicon via copper interconnect wafers.

Citation Information

Patent Citations

  • Chemically mechanical polishing agent

    CN102337079B

  • Chemical mechanical polishing slurry composition and method for its application in copper and silicon through-hole applications

    CN104250816B

  • Chemico-mechanical polishing solution

    CN109251673A

  • Chemical mechanical polishing for copper and through silicon via applications

    CN111732897A

  • Slurry composition, polishing method using the slurry composition and method of forming a gate pattern using the slurry composition

    US20060014390A1